External fixation medical stent instrument made of continuous fiber reinforced thermoplastic composite material

By using continuous carbon fiber reinforced thermoplastic composite materials and specific structural designs, the problems of corrosion and stress occlusion effects of traditional metal materials in fracture fixation are solved, and external fixed medical stent devices with high biocompatibility and mechanical properties are achieved, simplifying the Structure and improve productivity.

CN119014957AInactive Publication Date: 2024-11-26江苏君华特种高分子材料股份有限公司 +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411127325.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional metal materials have problems such as corrosion, stress occlusion effect, bone inflammation, reduced bone density, osteoporosis and rejection reactions when used for fracture fixation, and the high rigidity of the material leads to poor interlayer shear resistance and poor fatigue resistance.

Method used

Continuous carbon fiber reinforced thermoplastic composite material is used as external fixed medical bracket equipment. By bending and winding core rod structure and specific laying design, combining high-temperature and high-pressure molding and laser winding technology, it improves biocompatibility and mechanical properties and reduces cracking risks. .

Benefits of technology

It achieves higher biocompatibility, mechanical strength and lateral load strength, reduces rejection reactions, simplifies structural design, improves production efficiency and product quality, and reduces cracking risks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119014957A_ABST
    Figure CN119014957A_ABST
Patent Text Reader

Abstract

The invention relates to an external fixation medical stent instrument of a continuous fiber reinforced thermoplastic composite material, which comprises a first bending stent and a second bending stent, the length of the second bending stent is larger than that of the first bending stent, and the bending angle of the second bending stent is larger than that of the first bending stent; the first locking block group is used for fastening the first bending bracket; the second locking block group is used for fastening the second bending bracket; the adjustable locking block group is used for assembling the first bending bracket and the second bending bracket together; the adjustable locking block set fastens the first bending support, and the second bending support can move in the adjustable locking block set to adjust the position and is fixed. Wherein the structures of the first bending bracket and the second bending bracket are bending winding mandrels, the outer layers of the bending winding mandrels are unidirectional prepreg tape winding layers, and the inner layers of the bending winding mandrels are made of continuous carbon fiber reinforced thermoplastic composite materials with layering structures. The fixing support has the advantages of light weight, high strength and low cracking.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of medical devices, and in particular to an external fixation medical bracket device made of continuous fiber reinforced thermoplastic composite material. Background Art

[0002] Continuous carbon fiber reinforced thermoplastic composites not only have the same advantages as thermosetting resin carbon fiber composites in terms of corrosion resistance, high strength, and low density, but also have natural advantages in terms of waste recycling and high production efficiency. They are widely used in aerospace, medical, electrical and electronic fields. Due to technical reasons, the application of continuous carbon fiber reinforced thermoplastic composites in China is relatively limited, and medical treatment is the field where they are widely used.

[0003] The number of patients with traumatic fractures increases year by year, and the types of fixation devices used in orthopedics continue to expand, providing patients with many choices, but a small number of patients still experience slow fracture healing or basically no healing. Although traditional metal materials, such as stainless steel, pure titanium, and titanium alloys, are widely used, there are still some application problems. Metals will corrode and decompose toxic ions, which are harmful to the human body; the large difference in the mechanical modulus between metals and bones will produce a stress shielding effect, resulting in delayed bone healing, bone inflammation, decreased bone density, osteoporosis, fractures, and rejection reactions and other postoperative symptoms; at the same time, metal materials have poor resistance to interlaminar shear and poor fatigue resistance due to their high rigidity. Summary of the invention

[0004] In order to solve the problems caused by the existing use of metal bone plates and metal external fixation brackets, the present invention provides an external fixation medical bracket device made of continuous fiber reinforced thermoplastic composite materials. The present invention uses continuous carbon fiber reinforced thermoplastic composite materials as the main fixing bracket of the external fixation medical bracket device. Compared with metal bone plates, the present invention has higher biocompatibility, can reduce rejection reactions during use, simplifies the structure of the fixing device, and has the advantages of light weight, high mechanical strength, high lateral load strength, and low cracking risk.

[0005] In order to achieve the above objectives, the present invention is implemented by the following technical solutions:

[0006] An external fixation medical stent device of continuous fiber reinforced thermoplastic composite material, comprising: a first bent stent and a second bent stent, wherein the length of the second bent stent is longer than that of the first bent stent, and the bending angle of the second bent stent is greater than that of the first bent stent;

[0007] It also includes a first locking block group for fastening the first bending bracket and a second locking block group for fastening the second bending bracket;

[0008] and an adjustable locking block group for assembling the first bending bracket and the second bending bracket together, wherein the adjustable locking block group can fasten the first bending bracket and enable the second bending bracket to move and adjust its position within the adjustable locking block group and be fastened;

[0009] The structure of the first bending bracket and the second bending bracket is a bending winding mandrel, the outer layer of the bending winding mandrel is a unidirectional prepreg tape winding layer, and the inner layer is a continuous carbon fiber reinforced thermoplastic composite material with a layup structure.

[0010] Furthermore, the method for preparing the bending and winding mandrel comprises the following steps:

[0011] S1, stacking and laying sheets of continuous carbon fiber reinforced thermoplastic unidirectional prepreg, and molding them to obtain a blank flat plate;

[0012] S2, machining the blank flat plate into a blank square bar, and then performing external rounding rough processing to obtain a blank round rod;

[0013] S3, spirally winding the outer circumference of the blank round rod with a unidirectional prepreg tape to obtain a blank wound rod;

[0014] S4, performing external rounding finishing on the blank winding rod to obtain a winding mandrel;

[0015] S5. Perform bending and forming according to design requirements to obtain a bending and winding mandrel.

[0016] Furthermore, the continuous carbon fiber reinforced thermoplastic unidirectional prepreg and the unidirectional prepreg tape are both unidirectional prepregs with thermoplastic resin as matrix and continuous carbon fiber as reinforcement material, wherein the thermoplastic resin is selected from one or more of PEEK, PEKK, PEK, PEEKK, PEKEKK, PPSU, and TPI;

[0017] The unidirectional prepreg tape is a narrow tape with a width of 5-15 mm.

[0018] Furthermore, the layers are stacked at the following angles: [0 / 0 / +45 / 0 / 0 / -45 / 0 / 0] Sn, where s is the number of cyclic stacking, n represents mirror symmetry, and s is determined by the diameter of the winding mandrel; wherein the 0° direction ply accounts for 75% of the total weight of the inner layer, and the ±45° direction ply accounts for 25% of the total weight of the inner layer. The blank flat plate stacked according to this ply angle has the best comprehensive mechanical properties. The winding mandrel is a round rod, and its main force direction is the 0° direction. The 0° direction ply accounts for 75wt%, which can ensure that the product can still maintain a high mechanical strength under high load. At the same time, the ±45° direction ply accounts for 25wt%, which can improve the lateral load strength of the round rod and reduce cracking due to excessive lateral load.

[0019] Furthermore, the compression molding process is: under a pre-pressure of 1 MPa, the temperature of the first program heating and heating section is set to 300-350°C, the temperature of the second program heating and heating section is set to 370-400°C, the heating rate is 0.5-5°C / min, the first program heating and heating section is pressurized to 5MPa at 0.5MPa / 5min, and then the second program heating and heating section is pressurized at 1MPa / 5min until it is finally pressurized to 12-18MPa, and after the mold temperature reaches the temperature setting value of the second program heating and heating section, the heating is stopped and kept warm for 90-150min, and then the temperature is reduced to below 140°C at a rate of 3-10°C / min for demolding. Among them, the pre-pressure of 1MPa can make the stacking of thermoplastic prepreg sheets more compact and more efficient in heat transfer, and at the same time, it can also expel the stacking air and reduce the generation of voids inside the composite material; the first program heating and heating section can improve the uniformity of the mold temperature, so that the temperature of each part of the mold can reach 370-400℃ evenly and quickly in the subsequent second program heating and heating section; the first stage is pressurized at 0.5MPa / 5min, which can weaken the impact of high-speed thermoplastic melt on the reinforcing fiber and reduce the probability of slippage and wrinkles in the fiber layer; the second stage is pressurized at 1MPa / 5min to make the melt fully infiltrate the fiber and improve the infiltration. The quality of lubrication can significantly reduce the voids inside the composite material, and significantly increase the interface bonding strength between the thermoplastic engineering material and the reinforcing fiber; after keeping warm for 90-150 minutes, the temperature starts to drop rapidly, which can inhibit the crystallization of the crystalline thermoplastic engineering material, so that the thermoplastic engineering material is in a low crystalline state or amorphous state, thereby improving the toughness of the thermoplastic composite material; the temperature is quickly lowered to below 140℃ for demoulding, and the temperature is quickly lowered to below the glass transition temperature, which can limit the movement of the molecular chain and reduce the occurrence of defects such as deformation and warping. At the same time, it can also reduce the internal stress caused by the inconsistent shrinkage of the reinforcing fiber and the thermoplastic engineering material, and improve the overall mechanical strength of the composite material.

[0020] Furthermore, the machining adopts a three-axis machining center for segmentation processing, and the tool is a diamond or tungsten steel tool above D4, and the processing parameters are: processing speed 6000-10000mmpm, cutting depth 0.3-0.6mm, feed rate 500-2500rpm;

[0021] A through-type centerless grinder is used to perform the external circular rough machining and the external circular fine machining;

[0022] The outer grinding rough processing is performed by selecting a grinding wheel with a grit of 150-250, and the rough processing is performed on the blank square bar at a rotation speed of 30-80 rpm, with a processing depth of 0.3-0.8 mm. Selecting an outer grinding with a higher surface roughness is beneficial to improving the interface bonding strength with the winding layer and forming a resin interlocking structure;

[0023] The outer grinding finishing process uses a grinding wheel with a particle size of 1200-2000, and the blank winding rod is finished at a rotation speed of 60-120 rpm, with a processing depth of 0.02-0.1 mm, to obtain a winding mandrel with high finish.

[0024] Furthermore, the spiral winding is performed under laser heating, with a laser power of 2000-4000W, a heating temperature of 380-420°C, a winding speed of 50-100mm / s, and a winding tension of 80-200N. The use of single-beam prepreg tape for winding facilitates process adjustment and reduces material waste; laser heating maintained at 380-420℃ can make the resin material in the thermoplastic unidirectional prepreg tape quickly reach a molten state. The high tension formed by the rapid rotation of the winding table and the head pressure roller are used together to perform each circle of winding, so that the winding layer and the core rod have a high interlayer bonding strength. At the same time, the heating efficiency must match the rotation speed. If the rotation speed is too high, the resin on the prepreg tape cannot be fully heated and melted, thereby affecting the interlayer bonding of the wound product. If the speed is too low, the prepreg tape will be overheated, deformed, or even degraded. Appropriate winding tension can provide equivalent pressure to make the interlayer bonding tighter and reduce the interlayer gap. However, when the tension is large, the internal residual internal stress is too high, affecting the winding performance. The use of spiral winding can improve the overall circumferential mechanical strength of the core rod and prevent the core rod from being bent, delaminated, cracked, and other defects in the subsequent forming.

[0025] Furthermore, the bending forming is to place the winding mandrel in an oven at 380-420°C for preheating for 3-5 minutes and then transfer it to a bending mold for bending. The bending mold cools and shapes the material in the mold through circulating water below 30°C. Due to the rapid cooling from a high temperature state, the matrix resin becomes amorphous, which can improve the toughness of the overall material. Preheat at 360-420℃ for 3-5min. Although it exceeds the melting point, it is only softened in a short time and has not formed a melt. It is bent in this state, and the continuous carbon fiber is used as a skeleton support. The round rod is softened as a whole. After passing through the bending mold, the fibers and thermoplastic resin therein are caused to slip. After rapid cooling and shaping, defects such as wrinkles, fiber stretching, pitting, and fracture can be avoided. If the preheating temperature is too low or the time is too short, the thermoplastic resin material will still have a certain rigidity, and the round rod as a whole cannot reach the softened state. After bending, the fibers and thermoplastic resin are difficult to slide, resulting in defects such as inner wrinkles and outer fiber fractures at the arc corners of the round rod. If the preheating temperature is too high or the time is too long, the thermoplastic resin material is in a decomposition state, and the mechanical properties of the material are reduced. Even if the appearance quality of the round rod is normal, the thermoplastic resin material is decomposed, and the overall mechanical properties of the product are reduced and cannot meet the use requirements.

[0026] Furthermore, the first bending bracket and the second bending bracket are set to have unequal arm lengths; the bending radius of the first bending bracket is 40-60mm, the length of its longer arm is 170-220mm, and the length of its shorter arm is 60-100mm; the bending radius of the second bending bracket is 15-30mm, the length of its longer arm is 220-300mm, and the length of its shorter arm is 80-120mm.

[0027] Furthermore, the adjustable locking block group includes a limit adjustment locking block group and a movable adjustment locking block group;

[0028] The shorter arm of the first bending bracket and the longer arm of the second bending bracket are assembled through the limit adjustment locking block group, and the limit adjustment locking block group fixes the shorter arm of the first bending bracket;

[0029] The end of the shorter arm of the first bending bracket and the end of the longer arm of the second bending bracket are assembled through the movable adjustment locking block group, and the movable adjustment locking block group fixes the end of the shorter arm of the first bending bracket;

[0030] The limit adjustment locking block group and the movable adjustment locking block group both have movable adjustment grooves, and the second bending bracket moves in the two movable adjustment grooves at the same time. After adjusting to a suitable position, the longer arm of the second bending bracket is fixed in the limit adjustment locking block group by a limit bolt, and the end of the longer arm of the second bending bracket is fixed in the movable adjustment locking block group; the first bending bracket and the second bending bracket are provided with a plurality of positioning holes corresponding to the insertion of the limit bolts.

[0031] Further, the first locking block group, the second locking block group, the limit adjustment locking block group and the movement adjustment locking block group respectively include a female locking block and a male locking block capable of cooperative locking, and are fastened by a plurality of bolts;

[0032] The first locking block group is located at the bending part of the first bending bracket, and the number is set to be at least 1;

[0033] The second locking block group is located on the shorter arm of the second bending bracket, and the number is set to be at least 2;

[0034] The first locking block group, the second locking block group, and the movable adjustment locking block group are respectively provided with bone screw installation positions for fixing a plurality of the bone screws on the external fixation medical support device, so as to fix fractures at joints such as ankle joints and humeral joints.

[0035] Beneficial technical effects:

[0036] The medical external fixator device of the present invention adopts a continuous carbon fiber reinforced thermoplastic composite material, and compared with a metal bone plate, it has the characteristic of waste material being recyclable, which has significant advantages in terms of environmental protection and resource conservation; in addition, the continuous carbon fiber reinforced thermoplastic composite material used in the external fixator device of the present invention has better biocompatibility, which can reduce rejection reactions during use by patients, and the rod of the device is processed into a rod through a specific layer design (0 / ±45 regular layering) of continuous carbon fiber reinforced thermoplastic unidirectional prepreg, and a continuous carbon fiber reinforced thermoplastic unidirectional prepreg tape is wound around the outside of the rod, so that the product maintains a high mechanical strength under high load, while improving the lateral load strength and reducing the risk of cracking;

[0037] The present invention improves production efficiency and ensures product quality through high temperature and high pressure, rapid bending and forming steps; the manufacturing process includes using a three-axis machining center to perform flat plate segmentation processing, a centerless grinder to perform external round rough processing and fine processing, and laser thermoplastic raw consolidation winding technology, these process steps improve the accuracy and quality of the product; through the combined assembly of arc-wound round rods and locking block groups (the material of the locking block group is the same as that of the rod material), the structural design is simplified, the operation is convenient, and the high strength and light weight characteristics of the product are maintained. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 It is a schematic structural diagram of an external fixation medical stent device made of a continuous fiber reinforced thermoplastic composite material of the present invention;

[0039] Figure 2 It is a schematic structural diagram of an external fixation medical stent device made of a continuous fiber reinforced thermoplastic composite material of the present invention;

[0040] Among them, 1-titanium rod bone screw, 21-first locking block group, 22-second locking block group, 3-first bending bracket, 4-limit adjustment locking block group, 5-second bending bracket, 6-movable adjustment locking block group, 7-movable adjustment slot, 8-limit bolt. DETAILED DESCRIPTION

[0041] The technical solutions in the embodiments of the present invention will be described clearly and completely below in combination with the embodiments of the present invention and the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention are within the scope of protection of the present invention.

[0042] Unless otherwise specifically stated, the numerical value set forth in these embodiments does not limit the scope of the present invention. The technology and method known to those of ordinary skill in the relevant art may not be discussed in detail, but in appropriate cases, the technology and method should be considered as a part of the specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values.

[0043] In addition, it should be noted that the use of words such as "first" and "second" to limit structures such as brackets is only for the convenience of distinguishing the various components. Unless otherwise stated, the above words have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.

[0044] The experimental methods in the following examples without specifying specific conditions are usually measured in accordance with national standards; if there is no corresponding national standard, they are carried out in accordance with general standard requirements or general methods.

[0045] Example 1

[0046] The external fixation medical stent device made of continuous fiber reinforced thermoplastic composite material has a structural schematic diagram as shown in Figure 1 Its three-dimensional structure is shown in Figure 2As shown, it comprises: a first bending bracket 3 and a second bending bracket 5; the first bending bracket 3 and the second bending bracket 5 have unequal arm lengths;

[0047] The bending radius of the first bending bracket 3 is 40-60 mm (typically set to 45 mm), the length of the longer arm is 170-220 mm (typically set to 190 mm), and the length of the shorter arm is 60-100 mm (typically set to 70 mm); the bending radius of the second bending bracket 5 is 15-30 mm (typically set to 20 mm), the length of the longer arm is 220-300 mm (typically set to 220 mm), and the length of the shorter arm is 80-120 mm (typically set to 90 mm);

[0048] It also includes a first locking block group 21 for fastening the first bending bracket 3, and a second locking block group 22 for fastening the second bending bracket 5;

[0049] and an adjustable locking block group for assembling the first bending bracket 3 and the second bending bracket 5 together, wherein the adjustable locking block group fastens the first bending bracket 3, and the second bending bracket 5 can be moved and adjusted in position and fastened within the adjustable locking block group;

[0050] The adjustable locking block group includes a limit adjustment locking block group 4 and a movable adjustment locking block group 6;

[0051] The shorter arm of the first bending bracket 3 and the longer arm of the second bending bracket 5 are assembled through the limit adjustment locking block group 4, and the limit adjustment locking block group 4 fixes the shorter arm of the first bending bracket 3;

[0052] The end of the shorter arm of the first bending bracket 3 and the end of the longer arm of the second bending bracket 5 are assembled through the movable adjustment locking block group 6, and the movable adjustment locking block group 6 fixes the end of the shorter arm of the first bending bracket 3;

[0053] The limit adjustment locking block group 4 and the movable adjustment locking block group 6 are both provided with movable adjustment slots 7, and the second bending bracket 5 moves in the two movable adjustment slots 7 at the same time. After being adjusted to a suitable position, the longer arm of the second bending bracket 5 is fixed in the limit adjustment locking block group 4 by the limit bolt 8, and the end of the longer arm of the second bending bracket 5 is fixed in the movable adjustment locking block group 6; the first bending bracket 3 and the second bending bracket 5 can be provided with a plurality of positioning holes corresponding to the insertion of the limit bolts 8;

[0054] The first locking block group 21, the second locking block group 22, the limit adjustment locking block group 4 and the movement adjustment locking block group 6 respectively include a female locking block and a male locking block that can cooperate for locking, and are fastened by a plurality of bolts;

[0055] The first locking block group 21 is located at the bending position of the first bending bracket 3, and the number is set to 1;

[0056] The second locking block group 22 is located on the shorter arm of the second bending bracket 5, and the number is set to 2;

[0057] The first locking block group 21, the second locking block group 22, and the movable adjustment locking block group 6 are respectively provided with installation positions for titanium rod bone screws 1, which are used to fix multiple titanium rod bone screws 1 on the external fixation medical support device, so as to fix fractures at joints such as ankle joints and humeral joints.

[0058] The material of each locking block group is the same as that of each bending bracket.

[0059] The continuous fiber reinforced thermoplastic composite external fixation medical bracket device of the present invention is mainly used for fixing fractures at joints such as ankle joints and humeral joints. According to the design, the doctor drives titanium rod bone screws 1 into the corresponding positions of the upper and lower parts of the fracture segment, and installs the driven titanium rod bone screws 1 according to the bone screw installation positions on the first locking block group 21, the second locking block group 22, and the movable adjustment locking block group 6. Then, the first bending bracket 3 and the second bending bracket 5 are installed in the first locking block group 21, the second locking block group 22, the limit adjustment locking block group 4, and the movable adjustment locking block group 6. Each locking block group is fixed with screws, and the joint angle of the patient's fracture is adjusted so that the second bending bracket 5 is in the limit adjustment locking block group 4 and the movable adjustment locking block group 6. Move the movable adjustment groove 7 in the movable adjustment locking block group 6 to an appropriate position, and screw the limit bolt 8 into the limit adjustment locking block group 4 and the side of the movable adjustment locking block group 6 until it contacts and fixes the second bending bracket 5 (a corresponding screw-in hole can be set on the second bending bracket 5; or the limit bolt 8 is not required, but a serrated edge is set on one side of one or two movable adjustment grooves 7, and the locking block group is directly locked after being adjusted to an appropriate position, and the serrated edge is engaged and fixed to the second bending bracket 5) and wait for the bone to heal before removing the external fixation medical bracket instrument and taking out the bone screws.

[0060] Example 2

[0061] In order to achieve recyclability and improve biocompatibility while maintaining high mechanical strength, improving lateral load strength and reducing cracking risk, this case improves the material and structure of the first bending bracket 3 and the second bending bracket 5 used in Example 1, and prepares the structure of the first bending bracket 3 and the second bending bracket 5 into a bending and winding mandrel, the outer layer of the bending and winding mandrel is a unidirectional prepreg tape winding layer, and the inner layer is a continuous carbon fiber reinforced thermoplastic composite material with a lay-up structure.

[0062] The specific method for preparing the bending and winding mandrel comprises the following steps:

[0063] S1. Stack and lay sheets of continuous carbon fiber reinforced polyetheretherketone unidirectional prepreg (CCF / PEEK composite prepreg, sheet size 440*290mm, thickness 0.14mm, continuous carbon fiber model T700-12K, resin content 34±3wt%, provided by Jiangsu Junhua Special Polymer Materials Co., Ltd.), and the layers are stacked at the following angles: [0 / 0 / +45 / 0 / 0 / -45 / 0 / 0] Sn , where s is the number of cyclic stacking, s=6, n represents mirror symmetry, and s is determined by the diameter of the winding mandrel; wherein the 0° direction plies account for 75% of the total weight of the inner layer, and the ±45° direction plies account for 25% of the total weight of the inner layer;

[0064] After the ply is laid, it is placed in a mold for compression molding. The compression molding process is: under a pre-pressure of 1 MPa, the temperature of the first program heating and heating section is set to 320°C, the temperature of the second program heating and heating section is set to 400°C, and the mold temperature is stopped when it reaches above 380°C, the heating rate is 2°C / min, and the first section of pressurization is started at 0.5 MPa / 5min to pressurize to 5 MPa, and then the second section of pressurization is performed at 1 MPa / 5min until the final pressurization reaches 16 MPa, and after the mold stops heating, the temperature reaches the temperature and is kept for 150 minutes, and then the temperature is reduced to below 140°C at a rate of 10°C / min for demoulding to obtain a blank flat plate;

[0065] S2, using a three-axis machining center to segment the blank flat machine, the tool used for machining is a D4 diamond tool, the machining speed is 8000mmpm, the cutting depth is 0.5mm, and the feed rate is 1200rpm, to obtain a blank square bar;

[0066] Then, a BC6030 through-type centerless grinder is used to perform external round grinding on the rough square bar to obtain a rough round bar; a 200-mesh grinding wheel is selected for the external round grinding, and the rough square bar is rough-machined at a rotation speed of 60 rpm, with a machining depth of 0.8 mm;

[0067] S3, using continuous carbon fiber reinforced polyetheretherketone unidirectional prepreg (CCF / PEEK composite material prepreg, tape width 12.7mm, thickness 0.14mm, continuous carbon fiber model T700-12K, resin content 34±3wt%, provided by Jiangsu Junhua Special Polymer Materials Co., Ltd.) to spirally wind the outer circumference of the blank round rod, the spiral winding is wound under laser heating, the laser power is 3000W, the heating temperature is 400℃, the winding speed is 80mm / s, the winding tension is 150N, and the blank wound rod is obtained after spiral winding (specifically, for example, a six-axis robot arm can be used) Laser thermoplastic consolidation winding equipment, the two ends of the round rod are tightly pressed with stainless steel cylindrical conical ejector pins, and the use of stainless steel cylindrical conical ejector pins to press and fix can avoid the bad effects such as indentation and low utilization rate caused by direct use of three-claw fixation, and then fixed on the winding table under the action of the three-claw, and the unidirectional prepreg discharge tray placed above the mechanical arm is pulled out of the unidirectional prepreg through the machine head and fixed to one end of the core rod with tape; after the preparation work is completed, the laser heating and winding are turned on, and the single-beam laser locally heats the unidirectional prepreg, and the spiral winding is completed under the rotation of the winding table. After stopping the machine and taking out the product, the blank winding rod is obtained);

[0068] S4, using a BC6030 through-type centerless grinder to perform external rounding finishing on the blank winding rod, selecting a grinding wheel with a grit of 1200 for the external rounding finishing, and performing finishing on the blank winding rod at a rotation speed of 100 rpm, with a processing depth of 0.05 mm, to obtain a winding mandrel with high finish;

[0069] S5. Bending and forming are performed according to the design requirements. The bending and forming is to place the winding mandrel in an oven at 400°C for preheating for 4 minutes and then transfer it to a bending mold for bending. The bending mold cools and shapes the material in the mold through circulating water below 30°C. Due to the rapid cooling from a high temperature state, the PEEK resin becomes amorphous, which can improve the toughness of the overall material, that is, a bending and winding mandrel is obtained.

[0070] Example 3

[0071] The preparation method of the bending and winding mandrel in this case is the same as that in Example 2, except that the process parameters are adjusted, and specifically includes the following steps:

[0072] S1. Stack and lay sheets of continuous carbon fiber reinforced polyetheretherketone unidirectional prepreg (CCF / PEEK composite prepreg, sheet size 490*490mm, thickness 0.14mm, continuous carbon fiber model T700-12K, resin content 34±3wt%, provided by Jiangsu Junhua Special Polymer Materials Co., Ltd.), and the layers are stacked at the following angles: [0 / 0 / +45 / 0 / 0 / -45 / 0 / 0] Sn, where s is the number of cyclic stacking, s=8, n represents mirror symmetry, and s is determined by the diameter of the winding mandrel; wherein the 0° direction plies account for 75% of the total weight of the inner layer, and the ±45° direction plies account for 25% of the total weight of the inner layer;

[0073] After the ply is laid, it is placed in a mold for compression molding. The compression molding process is: under a pre-pressure of 1 MPa, the temperature of the first program heating and heating section is set to 350°C, the temperature of the second program heating and heating section is set to 420°C, and the mold temperature is stopped when it reaches above 390°C, the heating rate is 5°C / min, and the first section of pressurization is started at 0.5 MPa / 5min to pressurize to 5 MPa, and then the second section of pressurization is performed at 1 MPa / 5min until the final pressurization reaches 14 MPa, and the temperature reaches the temperature after the mold stops heating and is kept for 90 minutes, and then the temperature is reduced to below 140°C at a rate of 5°C / min for demolding to obtain a blank flat plate;

[0074] S2, using a three-axis machining center to segment the blank flat machine, the tool used for machining is a D4 diamond tool, the machining speed is 6000mmpm, the cutting depth is 0.3mm, and the feed rate is 800rpm, to obtain a blank square bar;

[0075] Then, a BC6030 through-type centerless grinder is used to perform external round grinding on the rough square bar to obtain a rough round bar; a grinding wheel with a grit size of 250 is selected for the external round grinding, and the rough square bar is rough-machined at a rotation speed of 80 rpm, with a machining depth of 0.4 mm;

[0076] S3, using continuous carbon fiber reinforced polyetheretherketone unidirectional prepreg (CCF / PEEK composite material prepreg, tape width 6.35mm, thickness 0.14mm, continuous carbon fiber model T700-12K, resin content 34±3wt%, provided by Jiangsu Junhua Special Polymer Materials Co., Ltd.) to spirally wind the outer circumference of the blank round rod, the spiral winding is wound under laser heating, the laser power is 2000W, the heating temperature is 380°C, the winding speed is 100mm / s, the winding tension is 200N, and the blank wound rod is obtained after spiral winding;

[0077] S4, using a BC6030 through-type centerless grinder to perform external rounding finishing on the blank winding rod, selecting a 1500-mesh grinding wheel for the external rounding finishing, and finishing the blank winding rod at a speed of 60 rpm, with a processing depth of 0.05 mm, to obtain a winding mandrel with high finish;

[0078] S5. Bending and forming are performed according to the design requirements. The bending and forming is to place the winding mandrel in an oven at 380°C for preheating for 5 minutes and then transfer it to a bending mold for bending. The bending mold cools and shapes the material in the mold through circulating water below 30°C. Due to the rapid cooling from a high temperature state, the PEEK resin becomes amorphous, which can improve the toughness of the overall material, that is, a bending and winding mandrel is obtained.

[0079] The unwound rod and the wound rod of Example 2-3 were subjected to performance tests. The test results are shown in Table 1.

[0080] Table 1 Rod properties of Examples 2-3

[0081]

[0082] The present invention processes continuous carbon fiber reinforced thermoplastic unidirectional prepreg into a rod through a specific ply design (0 / ±45 regular ply), and winds a continuous carbon fiber reinforced thermoplastic unidirectional prepreg tape outside the rod to form a wound rod, which can ensure that the external fixation medical stent device product maintains a high mechanical strength under high load, while improving the lateral load strength and reducing the risk of cracking.

[0083] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. An external fixation medical stent device made of continuous fiber reinforced thermoplastic composite material, characterized in that: include: A first bending bracket and a second bending bracket, wherein the length of the second bending bracket is longer than that of the first bending bracket, and the bending angle of the second bending bracket is greater than that of the first bending bracket; It also includes a first locking block group for fastening the first bending bracket and a second locking block group for fastening the second bending bracket; and an adjustable locking block group for assembling the first bending bracket and the second bending bracket together, wherein the adjustable locking block group can fasten the first bending bracket and enable the second bending bracket to move and adjust its position within the adjustable locking block group and be fastened; The structure of the first bending bracket and the second bending bracket is a bending winding mandrel, the outer layer of the bending winding mandrel is a unidirectional prepreg tape winding layer, and the inner layer is a continuous carbon fiber reinforced thermoplastic composite material with a layup structure.

2. The external fixation medical stent device of continuous fiber reinforced thermoplastic composite material according to claim 1, characterized in that: The method for preparing the bending and winding mandrel comprises the following steps: S1, stacking and laying sheets of continuous carbon fiber reinforced thermoplastic unidirectional prepreg, and molding them to obtain a blank flat plate; S2, machining the blank flat plate into a blank square bar, and then performing external rounding rough processing to obtain a blank round rod; S3, spirally winding the outer circumference of the blank round rod with a unidirectional prepreg tape to obtain a blank wound rod; S4, performing external rounding finishing on the blank winding rod to obtain a winding mandrel; S5. Perform bending and forming according to design requirements to obtain a bending and winding mandrel.

3. The external fixation medical stent device of continuous fiber reinforced thermoplastic composite material according to claim 2, characterized in that: The continuous carbon fiber reinforced thermoplastic unidirectional prepreg and the unidirectional prepreg tape are both unidirectional prepregs with thermoplastic resin as matrix and continuous carbon fiber as reinforcement material, wherein the thermoplastic resin is selected from one or more of PEEK, PEKK, PEK, PEEKK, PEKEKK, PPSU, and TPI; The unidirectional prepreg tape is a narrow tape with a width of 5-15 mm; The plies are stacked at the following angles: [0 / 0 / +45 / 0 / 0 / -45 / 0 / 0] Sn , where s is the number of cyclic stacking, n represents mirror symmetry, and s is determined by the diameter of the winding mandrel; the 0° direction plies account for 75% of the total weight of the inner layer, and the ±45° direction plies account for 25% of the total weight of the inner layer.

4. The external fixation medical stent device of continuous fiber reinforced thermoplastic composite material according to claim 2, characterized in that: The compression molding process is: under a pre-pressure of 1 MPa, the temperature of the first program heating and heating section is set to 300-350°C, the temperature of the second program heating and heating section is set to 370-400°C, the heating rate is 0.5-5°C / min, the first program heating and heating section is pressurized once to 5MPa at 0.5MPa / 5min, and then the second program heating and heating section is pressurized once at 1MPa / 5min until the final pressurization is 12-18MPa, and after the mold temperature reaches the temperature setting value of the second program heating and heating section, the heating is stopped and kept warm for 90-150min, and then the temperature is reduced to below 140°C at a rate of 3-10°C / min for demolding.

5. The external fixation medical stent device of continuous fiber reinforced thermoplastic composite material according to claim 2, characterized in that: The machining adopts a three-axis machining center for segmentation processing, and the cutting tool is a diamond or tungsten steel cutting tool of D4 or above. The machining process parameters are: machining speed 6000-10000mmpm, cutting depth 0.3-0.6mm, feed rate 500-2500rpm; A through-type centerless grinder is used to perform the external circular rough machining and the external circular fine machining; The outer round roughing process uses a grinding wheel with a grit of 150-250, and the roughing process is performed on the blank square bar at a rotation speed of 30-80 rpm, with a processing depth of 0.3-0.8 mm; The outer grinding finishing process uses a grinding wheel with a particle size of 1200-2000, and the blank winding rod is finished at a rotation speed of 60-120 rpm, with a processing depth of 0.02-0.1 mm.

6. The external fixation medical stent device of continuous fiber reinforced thermoplastic composite material according to claim 2, characterized in that: The spiral winding is performed under laser heating, with a laser power of 2000-4000W, a heating temperature of 380-420°C, a winding speed of 50-100mm / s, and a winding tension of 80-200N; The bending molding is to place the winding mandrel in an oven at 380-420°C for preheating for 3-5 minutes and then transfer it to a bending mold for bending. The bending mold cools and shapes the material in the mold through circulating water below 30°C, and the matrix resin is amorphous.

7. The external fixation medical stent device of continuous fiber reinforced thermoplastic composite material according to claim 2, characterized in that: The first bending bracket and the second bending bracket are set to have unequal arm lengths; the bending radius of the first bending bracket is 40-60mm, the length of its longer arm is 170-220mm, and the length of its shorter arm is 60-100mm; the bending radius of the second bending bracket is 15-30mm, the length of its longer arm is 220-300mm, and the length of its shorter arm is 80-120mm.

8. The external fixation medical stent device of continuous fiber reinforced thermoplastic composite material according to any one of claims 1 to 6, characterized in that: The adjustable locking block group includes a limit adjustment locking block group and a movable adjustment locking block group; The shorter arm of the first bending bracket and the longer arm of the second bending bracket are assembled through the limit adjustment locking block group, and the limit adjustment locking block group fixes the shorter arm of the first bending bracket; The end of the shorter arm of the first bending bracket and the end of the longer arm of the second bending bracket are assembled through the movable adjustment locking block group, and the movable adjustment locking block group fixes the end of the shorter arm of the first bending bracket; The limit adjustment locking block group and the movable adjustment locking block group both have movable adjustment grooves, and the second bending bracket moves in the two movable adjustment grooves at the same time. After adjusting to a suitable position, the longer arm of the second bending bracket is fixed in the limit adjustment locking block group by a limit bolt, and the end of the longer arm of the second bending bracket is fixed in the movable adjustment locking block group; the first bending bracket and the second bending bracket are provided with a plurality of positioning holes corresponding to the insertion of the limit bolts.

9. The external fixation medical stent device made of continuous fiber reinforced thermoplastic composite material according to claim 8, characterized in that: The first locking block group, the second locking block group, the limit adjustment locking block group and the movement adjustment locking block group respectively include a female locking block and a male locking block that can cooperate and lock, and are fastened by a plurality of bolts; The first locking block group is located at the bending part of the first bending bracket, and the number is set to be at least 1; The second locking block group is located on the shorter arm of the second bending bracket, and the number is set to be at least 2; The first locking block group, the second locking block group, and the movable and adjustable locking block group are respectively provided with bone screw installation positions for fixing a plurality of the bone screws on the external fixation medical support device, so as to fix the fracture at the joint position.

Citation Information

Patent Citations

  • Bending device

    CN107468323A

  • Annular winding forming method of thermoplastic composite material

    CN114311742A

  • Continuous carbon fiber CF / PAEK thermoplastic composite material femoral bone fracture plate and preparation method thereof

    CN115581815A

  • Composite forming method of continuous fiber reinforced thermoplastic engineering material profile

    CN117507399A

  • Distal radius fracture reduction fixator

    CN202105008U