Manufacturing method of laminated and multi-layer coated elastic plaster
Through the stacked multi-layer coating technology, different levels of the paste are set, the reaction and odor isolation problems between raw materials are solved, the elasticity and functionality of the paste are improved, and the gradient release effect of drug substances is achieved, which is improved. Overall performance of paste patch.
Patent Information
- Application Number
- CN202411159051.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-26
AI Technical Summary
In the single-layer structure of existing paste products, the problems of failure of mutual reaction between raw materials and poor odor isolation have led to poor use.
Using the laminated multi-layer coating elastic paste production method, the parameters of the outermost layer, innermost layer and intermediate layer are set, including hot melt adhesive type, specific materials and mixing methods, to achieve functional divisions at different levels. layer to solve the problems of reaction and odor isolation between raw materials.
It improves the elasticity and functionality of the paste, enhances the comfort of use, and achieves the gradient release and sustained release of drug substances through multi-layer coating technology, improving the overall performance of the paste.
Smart Images

Figure CN119015046A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of plaster making, and in particular to a method for making a laminated and multi-layer coated elastic plaster. Background Art
[0002] At present, the main product structure of the patch industry is composed of three parts: non-woven fabric layer (or woven fabric), hot-melt adhesive layer and release paper layer. The non-woven fabric is tensionless, the additives in the hot-melt adhesive layer are limited by mutual reactions, the hot-melt adhesive layer loses adhesion and cannot be properly adhered to the skin after excessive addition, there is a potential risk of mutual reaction and failure after mixing various effective substances, and the volatile substances in the colloid layer can directly evaporate odor into the air through the non-woven fabric, and there are many other technical limitations and product application shortcomings.
[0003] Chinese patent publication number: CN104887883A discloses a snake oil plaster, comprising a snake oil plaster (01), a snake oil plaster carrier (02) and a double-unit multi-group snake oil plaster machine (03); the snake oil plaster (01) is in a viscous paste state; the snake oil plaster (01) uses snake oil and more than ten kinds of pure Chinese medicine components; the snake oil plaster carrier (02) includes a plaster surface layer (1), a plaster bearing layer (2) and a plaster protective layer (3); the plaster surface layer (1) is made of a breathable elastic non-woven fabric with a thickness of ≥0.15mm; the plaster bearing layer (2) is located in the middle of the snake oil plaster, and the plaster bearing layer (2) is evenly coated with snake oil plaster by the double-unit multi-group snake oil plaster machine (03); the plaster protective layer (3) is covered with a plaster protective layer (3) with the same area as the plaster surface layer (1). However, this solution cannot solve the problems of mutual reaction between raw materials of single-layer plaster and poor odor isolation of the plaster. Summary of the invention
[0004] To this end, the present invention provides a method for producing a laminated and multi-layer coated elastic patch, which is used to overcome the problems of mutual reaction and failure of raw materials in single-layer patches and poor odor isolation of the patches in the prior art.
[0005] To achieve the above object, the present invention provides a method for preparing a laminated multi-layer coated elastic plaster, comprising:
[0006] Step S1, setting the outermost layer parameters according to the type of the elastic patch to be laminated and multi-layered, and preparing the outermost layer according to the outermost layer parameters;
[0007] Step S2, setting the innermost layer parameters according to the type of the elastic patch to be laminated and coated with multiple layers, and preparing the innermost layer according to the innermost layer parameters;
[0008] Step S3, setting the parameters of the intermediate layer ingredients and the intermediate layer mixing method according to the type of the elastic patch to be laminated and multi-layered, and preparing the intermediate unit layer raw materials according to the parameters of the intermediate layer ingredients and the intermediate layer mixing method;
[0009] Step S4: setting the unit layer parameters of the coating method according to the type of laminated multi-layer coated elastic patch, and connecting the outermost layer, the middle unit layer raw materials and the innermost layer according to the coating method to obtain a laminated multi-layer coated elastic patch; the types of laminated multi-layer coated elastic patches include layered coating with organic / inorganic additives, layered coating with odor / fragrance additives and layered coating with multi-layer drugs in sections.
[0010] Further, in the step S3, the intermediate layer is composed of intermediate unit layers of a preset number n, including a first preset intermediate unit layer A, a second preset intermediate unit layer B, ..., an nth preset intermediate unit layer M, and the preset number n≥2 and n is an integer.
[0011] Furthermore, in step S3, the middle layer ingredients are set to preset types of hot melt adhesive and specific materials, the preset types of hot melt adhesive include low-temperature hot melt adhesive, sweat-resistant hot melt adhesive and high-temperature hot melt adhesive, and the specific materials include pregelatinized starch, ginger extract, bisabolol, menthol, BHT, far-infrared ceramic powder, neodymium iron boron magnetic powder, PVPk30, wintergreen oil, essence, eucalyptus oil and magnesium sulfate.
[0012] Furthermore, in step S3, when setting the ingredients of the middle layer, the ingredients of the middle layer are set according to the type of elastic plaster to be laminated and coated in multiple layers, wherein:
[0013] When the type of the elastic plaster with laminated multilayer coating is layered coating with organic / inorganic additives, the intermediate layer ingredients are set to include intermediate unit layer A ingredients, intermediate unit layer B ingredients and intermediate unit layer C ingredients, wherein:
[0014] The ingredients of the intermediate unit layer A include: sweat-resistant hot melt adhesive accounts for M1, use temperature is T1, PVPk30 accounts for M2, pregelatinized starch accounts for M3, ginger extract accounts for M4, bisabolol accounts for M5, menthol accounts for M6, BHT accounts for M7, wherein 50%<M1<98%, 100℃<T1<140℃, 0.1%<M2<15%, 0.1%<M3<5%, 0.1%<M4<15%, 0.1%<M5<3%, 0.2%<M6<6%, 0.1%<M7<3%;
[0015] The ingredients of the intermediate unit layer B include: low-temperature hot melt adhesive accounts for N1, the use temperature is T2, far-infrared ceramic powder accounts for N2, and BHT accounts for N3, wherein 50%<N1<98%, 90℃<T2<130℃, 2%<N2<50%, and 0.1%<N3<3%;
[0016] The ingredients of the intermediate unit layer C include: a high-temperature hot melt adhesive ratio of P1, a use temperature of T3, and a NdFeB magnetic powder ratio of P2, wherein 50%<P1<98%, 140℃<T3<180℃, and 2%<P2<50%;
[0017] When the type of the laminated multi-layer coated elastic patch is layered coating with odor / fragrance additives, the middle layer ingredients are set to include the middle unit layer A ingredients and the middle unit layer B ingredients:
[0018] The ingredients of the middle unit layer A include: sweat-resistant hot melt adhesive accounts for M1, use temperature is T1, PVPk30 accounts for M2, pregelatinized starch accounts for M3, wintergreen oil accounts for M4, bisabolol accounts for M5, menthol accounts for M6, BHT accounts for M7, wherein 50%<M1<98%, 100℃<T1<140℃, 0.1%<M2<15%, 0.1%<M3<5%, 0.1%<M4<15%, 0.1%<M5<3%, 0.2%<M6<6%, 0.1%<M7<3%;
[0019] The ingredients of the intermediate unit layer B include: low-temperature hot melt adhesive accounts for N1, use temperature is T2, flavor accounts for N2, BHT accounts for N3, among which 92%<N1<98%, 90℃<T2<130℃, 2%<N2<5%, 0.1%<N3<3%;
[0020] When the type of the laminated multi-layer coated elastic patch is multi-layer drug segmented effective layered coating, the intermediate layer ingredients are set to include the intermediate unit layer A ingredients, the intermediate unit layer B ingredients and the intermediate unit layer C ingredients:
[0021] The ingredients of the intermediate unit layer A include: intermediate unit layer A: sweat-resistant hot melt adhesive accounts for M1, use temperature is T1, PVPk30 accounts for M2, pregelatinized starch accounts for M3, eucalyptus oil accounts for M4, bisabolol accounts for M5, menthol accounts for M6, BHT accounts for M7, wherein 50%<M1<98%, 100℃<T1<140℃, 0.1%<M2<15%, 0.1%<M3<5%, 0.1%<M4<15%, 0.1%<M5<3%, 0.2%<M6<6%, 0.1%<M7<3%;
[0022] The ingredients of the intermediate unit layer B include: low-temperature hot melt adhesive accounts for N1, the use temperature is T2, far-infrared ceramic powder accounts for N2, magnesium sulfate accounts for N3, BHT accounts for N4, among which 50%<N1<98%, 90℃<T2<130℃, 2%<N2<50%, 0.5%<N3<10%, 0.1%<N4<3%;
[0023] The ingredients of the middle unit layer C include: high-temperature hot melt adhesive accounting for 100%, and the use temperature is T3, wherein 140°C<T3<180°C.
[0024] Further, in step S3, the intermediate layer mixing method includes:
[0025] Step S30, adding a preset type of hot melt adhesive into a mixing kettle;
[0026] Step S31, in a mixing kettle, performing a curing treatment on a preset type of hot melt adhesive according to a rated curing temperature and a rated curing time to obtain a cured raw material;
[0027] Step S32, in a mixing kettle, stirring the gelled raw material according to a rated rotation speed and a rated stirring time and adding specific materials to obtain a mixed raw material;
[0028] Step S33, in a mixing kettle, stirring the mixed raw materials at a constant standby temperature to obtain the intermediate unit layer raw materials.
[0029] Furthermore, in the step S3, when preparing the intermediate unit layer raw material, the intermediate unit layer raw material is prepared according to the intermediate layer batching and intermediate layer mixing method parameters, wherein:
[0030] When the type of the elastic patch for laminated multilayer coating is layered coating with organic / inorganic additives, the intermediate layer mixing method parameters are set to include the intermediate unit layer A mixing method parameters, the intermediate unit layer B mixing method parameters and the intermediate unit layer C mixing method parameters, wherein:
[0031] The parameters of the mixing method of the intermediate unit layer A include: a rated curing temperature of 110°C, a rated curing time of 2h, a rated rotation speed of 50rpm, a rated stirring time of 0.5h, and a constant temperature standby temperature of 110°C;
[0032] The parameters of the mixing method of the intermediate unit layer B include: a rated curing temperature of 100°C, a rated curing time of 2h, a rated rotation speed of 50rpm, a rated stirring time of 0.5h, and a constant temperature standby temperature of 100°C;
[0033] The parameters of the mixing method of the intermediate unit layer C include: a rated curing temperature of 150°C, a rated curing time of 2h, a rated rotation speed of 50rpm, a rated stirring time of 0.5h, and a constant temperature standby temperature of 150°C;
[0034] When the type of the elastic patch for laminated multilayer coating is layered coating with odor / fragrance additives, the intermediate layer mixing method parameters are set to include the intermediate unit layer A mixing method parameters and the intermediate unit layer B mixing method parameters.
[0035] The parameters of the mixing method of the intermediate unit layer A include: a rated curing temperature of 110°C, a rated curing time of 2h, a rated rotation speed of 50rpm, a rated stirring time of 0.5h, and a constant temperature standby temperature of 110°C;
[0036] The parameters of the mixing method of the intermediate unit layer B include: a rated curing temperature of 100°C, a rated curing time of 2h, a rated rotation speed of 50rpm, a rated stirring time of 0.5h, and a constant temperature standby temperature of 100°C;
[0037] When the type of the elastic patch with laminated multi-layer coating is multi-layer drug segmented effective layer coating, the intermediate layer mixing method parameters are set to include the intermediate unit layer A mixing method parameters, the intermediate unit layer B mixing method parameters and the intermediate unit layer C mixing method parameters, wherein:
[0038] The parameters of the mixing method of the middle unit layer A are as follows: the rated curing temperature is 110°C, the rated curing time is 2h, the rated speed is 50rpm, the rated stirring time is 0.5h, and the constant temperature standby temperature is 110°C;
[0039] Parameters of the mixing method of the intermediate unit layer B: rated curing temperature is 100°C, rated curing time is 2h, rated speed is 50rpm, rated stirring time is 0.5h, and constant temperature standby temperature is 100°C;
[0040] The parameters of the mixing method of the intermediate unit layer C are as follows: the rated curing temperature is 150°C, the rated curing time is 2h, the rated rotation speed is 50rpm, the rated stirring time is 0.5h, and the constant temperature standby temperature is 150°C.
[0041] Further, in the step S4, the coating method comprises:
[0042] Step S40, starting coating with the innermost layer as the bottom layer;
[0043] Step S41, performing layered coating to obtain a combination of an innermost layer and an intermediate layer;
[0044] Step S42, preparing a roll of plaster according to the combination of the innermost layer and the middle layer and the outermost layer;
[0045] Step S43, aging overnight, packaging the rolled plaster pieces, and obtaining a laminated multi-layer coated plaster.
[0046] Furthermore, in the step S41, when performing layered coating, the intermediate unit layer raw material is coated on the innermost layer according to the intermediate unit layer sequence, the coating rated temperature and the coating rated gram weight, and the coating layer temperature is waited to drop to room temperature, and the above steps are repeated until the intermediate unit layer coating is completed.
[0047] Furthermore, in the step S42, when preparing the rolled plaster, the innermost layer and the middle layer combination are compounded with the outermost layer into a roll according to the rated compounding temperature to obtain the rolled plaster.
[0048] Furthermore, in step S4, when setting the unit layer parameters of the coating method, the unit layer parameters of the coating method are set according to the type of elastic patch for laminated multilayer coating, wherein:
[0049] When the type of the elastic patch of the laminated multilayer coating is layered coating with organic / inorganic additives, the coating method unit layer parameters are set to include the coating parameters of the middle unit layer A, the coating parameters of the middle unit layer B and the coating parameters of the middle unit layer C, wherein:
[0050] The coating parameters of the intermediate unit layer A include:
[0051] The rated temperature of the middle unit layer A during coating is 110°C.
[0052] The rated weight of the coating of the middle unit layer A is 50g / m 2 ,
[0053] The coating and compounding temperature of the middle unit layer A is 80±10℃;
[0054] The coating parameters of the intermediate unit layer B include:
[0055] The rated temperature of the middle unit layer B during coating is 100°C.
[0056] The rated weight of the coating of the middle unit layer B is 50g / m 2 ,
[0057] The coating temperature of the middle unit layer B is 80±10℃;
[0058] The coating parameters of the intermediate unit layer C include:
[0059] The rated temperature of the intermediate unit layer C coating is 150°C.
[0060] The rated weight of the middle unit layer C coating is 80g / m 2 ,
[0061] The coating temperature of the middle unit layer C is 80±10℃;
[0062] When the type of the elastic patch for laminated multilayer coating is layered coating of odor / fragrance additives, the coating method unit layer parameters are set to include the coating parameters of the middle unit layer A and the coating parameters of the middle unit layer B, wherein:
[0063] The coating parameters of the intermediate unit layer A include:
[0064] The rated temperature of the middle unit layer A during coating is 110°C.
[0065] The rated weight of the coating of the middle unit layer A is 80g / m2.
[0066] The coating and compounding temperature of the middle unit layer A is 80±10℃;
[0067] The coating parameters of the intermediate unit layer B include:
[0068] The rated temperature of the middle unit layer B during coating is 100°C.
[0069] The rated weight of the middle unit layer B coating is 100g / m 2 ,
[0070] The coating temperature of the middle unit layer B is 80±10℃;
[0071] When the type of the elastic patch with laminated multi-layer coating is multi-layer drug segmented effective layered coating, the coating method unit layer parameters are set to include the coating parameters of the middle unit layer A, the coating parameters of the middle unit layer B and the coating parameters of the middle unit layer C, wherein:
[0072] The coating parameters of the intermediate unit layer A include:
[0073] The rated temperature of the middle unit layer A during coating is 110°C.
[0074] The rated weight of the coating of the middle unit layer A is 50g / m 2 ,
[0075] The coating and compounding temperature of the middle unit layer A is 80±10℃;
[0076] The coating parameters of the intermediate unit layer B include:
[0077] The rated temperature of the middle unit layer B during coating is 100°C.
[0078] The rated weight of the middle unit layer B coating is 100g / m 2 ,
[0079] The coating temperature of the middle unit layer B is 80±10℃;
[0080] The coating parameters of the intermediate unit layer C include:
[0081] The rated temperature of the intermediate unit layer C coating is 150°C.
[0082] The middle unit layer C coating rated weight is 50g / m 2 ,
[0083] The coating temperature of the middle unit layer B is 80±10°C.
[0084] Compared with the prior art, the beneficial effect of the present invention is that the method sets the outermost layer parameters according to the type of the elastic plaster with multi-layer coating through step S1, prepares the outermost layer according to the outermost layer parameters, and makes the elastic plaster with multi-layer coating have better elasticity by changing the performance parameters of the material. The method sets the innermost layer parameters according to the type of the elastic plaster with multi-layer coating through step S2, prepares the innermost layer according to the innermost layer parameters, and uses different innermost layer parameters to improve the functionality of the innermost layer. The method sets the middle layer ingredients and the middle layer mixing method parameters according to the type of the elastic plaster with multi-layer coating through step S3, and mixes the middle layer ingredients and the middle layer mixing method parameters according to the middle layer ingredients and the middle layer mixing method parameters. The unit layer raw materials are prepared, and different intermediate layer ingredients and mixing method parameters are used to solve the problems of mutual reaction failure between the raw materials of the single-layer patch and poor odor isolation of the patch, so as to increase the comfort of use. The method sets the unit layer parameters of the coating method according to the type of the elastic patch with laminated multi-layer coating through step S4, and connects the outermost layer, the intermediate unit layer raw materials and the innermost layer according to the coating method to obtain the elastic patch with laminated multi-layer coating; the types of the elastic patch with laminated multi-layer coating include layered coating of organic / inorganic additives, layered coating of odor / fragrance additives and layered coating of multi-layer drugs with segmented effectiveness. The multi-layer coating technology enables the gradient release and sustained release of multi-layer functional substances, which upgrades the conventional coating technology of the patch. BRIEF DESCRIPTION OF THE DRAWINGS
[0085] Figure 1 It is a schematic diagram of the process of manufacturing the elastic plaster with laminated multi-layer coating in this embodiment;
[0086] Figure 2 Schematic diagram of the process of the interlayer mixing method in this embodiment;
[0087] Figure 3 Schematic diagram of the coating process of this embodiment. DETAILED DESCRIPTION
[0088] In order to make the objects and advantages of the present invention more clearly understood, the present invention is further described below in conjunction with embodiments; it should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0089] The preferred embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.
[0090] See also Figure 1 As shown, it is a schematic diagram of the process of the method for making a laminated multi-layer coated elastic plaster of this embodiment, and the method for making a laminated multi-layer coated elastic plaster comprises:
[0091] Step S1, setting the outermost layer parameters according to the type of the elastic patch to be laminated and multi-layered, and preparing the outermost layer according to the outermost layer parameters;
[0092] Step S2, setting the innermost layer parameters according to the type of the elastic patch to be laminated and coated with multiple layers, and preparing the innermost layer according to the innermost layer parameters;
[0093] Step S3, setting the parameters of the intermediate layer ingredients and the intermediate layer mixing method according to the type of the elastic patch to be laminated and multi-layered, and preparing the intermediate unit layer raw materials according to the parameters of the intermediate layer ingredients and the intermediate layer mixing method;
[0094] Step S4: setting the unit layer parameters of the coating method according to the type of laminated multi-layer coated elastic patch, and connecting the outermost layer, the middle unit layer raw materials and the innermost layer according to the coating method to obtain a laminated multi-layer coated elastic patch; the types of laminated multi-layer coated elastic patches include layered coating with organic / inorganic additives, layered coating with odor / fragrance additives and layered coating with multi-layer drugs in sections.
[0095] Specifically, the method is applied to the production of a patch, and an elastic patch is obtained by laminating and coating multiple layers, thereby improving the production efficiency of the patch and the medicinal function during use. The method sets the outermost layer parameters according to the type of the elastic patch with laminated and multi-layer coating through step S1, prepares the outermost layer according to the outermost layer parameters, and makes the elastic patch with laminated and multi-layer coating have better elasticity by changing the material ratio. The method sets the innermost layer parameters according to the type of the elastic patch with laminated and multi-layer coating through step S2, prepares the innermost layer according to the innermost layer parameters, and uses different innermost layer parameters to improve the functionality of the innermost layer. The method sets the middle layer ingredients and the middle layer mixing method parameters according to the type of the elastic patch with laminated and multi-layer coating through step S3, and The intermediate unit layer raw materials are prepared according to the layer ingredients and the intermediate layer mixing method parameters, and different intermediate layer ingredients and mixing method parameters are used to solve the problems of mutual reaction failure between the raw materials of the single-layer plaster and poor odor isolation of the plaster, so as to increase the comfort of use. The method sets the coating method unit layer parameters according to the type of the laminated multi-layer coated elastic plaster through step S4, and connects the outermost layer, the intermediate unit layer raw materials and the innermost layer according to the coating method to obtain a laminated multi-layer coated elastic plaster; the types of the laminated multi-layer coated elastic plaster include organic / inorganic additive layered coating, odor / fragrance additive layered coating and multi-layer drug segmented onset layered coating. The multi-layer coating technology enables the gradient release and sustained-release of multi-layer functional substances, which upgrades the conventional coating technology of the plaster.
[0096] Specifically, in step S1, when setting the outermost layer parameters, the outermost layer parameters are set according to the type of elastic patch applied in multiple layers, wherein:
[0097] When the type of the elastic patch with multi-layer coating is layered coating with organic / inorganic additives, the outermost layer is set to be a two-way elastic fabric, and the outermost layer parameters are:
[0098] The outermost layer weight is 80±10g / m 2 ;
[0099] The outermost layer has a bidirectional elastic direction;
[0100] The tensile strength of the outermost layer is ≥200N / 5cm in the warp direction and ≥150N / 5cm in the weft direction;
[0101] The elongation at break of the outermost layer is ≥200% in the warp direction and ≥200% in the weft direction
[0102] The tear strength of the outermost layer is ≥25N / 5cm in the warp direction and ≥15N / 5cm in the weft direction;
[0103] The elastic coefficient of the outermost layer is the force used to extend the original length by 50% ≤ 0.5N / cm;
[0104] The resilience of the outermost layer is ≤120%;
[0105] The outermost layer is made of polyester;
[0106] When the type of the laminated multi-layered elastic patch is layered coating with odor / fragrance additives, the outermost layer is set to be a four-way elastic fabric, and the outermost layer parameters are:
[0107] The outermost layer weight is 150±15g / m 2 ;
[0108] The outermost layer has four-way elastic direction;
[0109] The tensile strength of the outermost layer is ≥200N / 5cm in the warp direction and ≥150N / 5cm in the weft direction;
[0110] The elongation at break of the outermost layer is ≥200% in the warp direction and ≥200% in the weft direction;
[0111] The tear strength of the outermost layer is ≥25N / 5cm in the warp direction and ≥15N / 5cm in the weft direction;
[0112] The elastic coefficient of the outermost layer is the force used to extend the original length by 50% ≤ 0.5N / cm;
[0113] The resilience of the outermost layer is ≤120%;
[0114] The outermost layer is made of polyester;
[0115] When the type of the laminated multi-layer coated elastic patch is multi-layer drug segmented effective layer coating, the outermost layer is set to be non-woven fabric, and the parameters of the outermost layer are:
[0116] The outermost layer weight is 80±10g / m 2 ;
[0117] The thickness of the outermost layer is 0.4±0.05mm;
[0118] The tensile strength of the outermost layer is ≥80N / 5cm in the warp direction and ≥80N / 5cm in the weft direction;
[0119] The elongation at break of the outermost layer is ≥80% in the warp direction and ≥80% in the weft direction
[0120] The outermost material is polyester.
[0121] Specifically, the outermost layer parameters are set according to the type of the laminated multi-layer coated elastic patch, and the outermost layer is prepared according to the outermost layer parameters. By changing the parameters of the material, the laminated multi-layer coated elastic patch has better elasticity.
[0122] Specifically, in step S2, when setting the innermost layer parameters, the innermost layer parameters are set according to the type of elastic patch applied in multiple layers, wherein:
[0123] When the type of elastic patch with multi-layer coating is layered coating with organic / inorganic additives, the innermost layer is set to PET, and the parameters of the innermost layer are:
[0124] The weight of the innermost layer is 12±2g / m 2 ;
[0125] The innermost layer thickness is 125±3um;
[0126] The tensile strength of the innermost layer is ≥150N / inch in the longitudinal direction and ≥200N / inch in the transverse direction;
[0127] The elongation at break of the innermost layer is ≥200% in the longitudinal direction and ≥100% in the transverse direction;
[0128] The release force of the innermost layer is 10±2g / inch;
[0129] When the elastic patch with multiple layers of coating is coated with odor / fragrance additives in layers, the innermost layer is set to PET, and the parameters of the innermost layer are:
[0130] The weight of the innermost layer is 10±2g / m 2 ;
[0131] The innermost layer thickness is 100±3um;
[0132] The tensile strength of the innermost layer is ≥150N / inch in the longitudinal direction and ≥200N / inch in the transverse direction;
[0133] The elongation at break of the innermost layer is ≥200% in the longitudinal direction and ≥100% in the transverse direction;
[0134] The release force of the innermost layer is 10±2g / inch;
[0135] When the type of the laminated multi-layered elastic patch is multi-layer drug segmented effect layered coating, the innermost layer is set to PET, and the innermost layer parameters are:
[0136] The weight of the innermost layer is 12±2g / m 2 ;
[0137] The innermost layer thickness is 125±3um;
[0138] The tensile strength of the innermost layer is ≥150N / inch in the longitudinal direction and ≥200N / inch in the transverse direction;
[0139] The elongation at break of the innermost layer is ≥200% in the longitudinal direction and ≥100% in the transverse direction;
[0140] The release force of the innermost layer is 10±2g / inch.
[0141] Specifically, through step S2, the innermost layer parameters are set according to the type of the elastic patch coated with multiple layers, and the innermost layer is prepared according to the innermost layer parameters to improve the functionality of the innermost layer.
[0142] Specifically, in step S3, the intermediate layer is composed of a preset number n of intermediate unit layers, including a first preset intermediate unit layer A, a second preset intermediate unit layer B, ..., an nth preset intermediate unit layer M, where the preset number n≥2 and n is an integer.
[0143] Specifically, in step S3, the middle layer ingredients are set to preset types of hot melt adhesive and specific materials, the preset types of hot melt adhesive include low-temperature hot melt adhesive, sweat-resistant hot melt adhesive and high-temperature hot melt adhesive, and the specific materials include pregelatinized starch, ginger extract, bisabolol, menthol, BHT, far-infrared ceramic powder, neodymium iron boron magnetic powder, PVPk30, wintergreen oil, essence, eucalyptus oil and magnesium sulfate.
[0144] Specifically, in step S3, when setting the ingredients of the middle layer, the ingredients of the middle layer are set according to the type of elastic patch for multi-layer coating, wherein:
[0145] When the type of the elastic plaster with laminated multilayer coating is layered coating with organic / inorganic additives, the intermediate layer ingredients are set to include intermediate unit layer A ingredients, intermediate unit layer B ingredients and intermediate unit layer C ingredients, wherein:
[0146] The ingredients of the intermediate unit layer A include: sweat-resistant hot melt adhesive accounts for M1, use temperature is T1, PVPk30 accounts for M2, pregelatinized starch accounts for M3, ginger extract accounts for M4, bisabolol accounts for M5, menthol accounts for M6, BHT accounts for M7, wherein 50%<M1<98%, 100℃<T1<140℃, 0.1%<M2<15%, 0.1%<M3<5%, 0.1%<M4<15%, 0.1%<M5<3%, 0.2%<M6<6%, 0.1%<M7<3%;
[0147] The ingredients of the intermediate unit layer B include: low-temperature hot melt adhesive accounts for N1, the use temperature is T2, far-infrared ceramic powder accounts for N2, and BHT accounts for N3, wherein 50%<N1<98%, 90℃<T2<130℃, 2%<N2<50%, and 0.1%<N3<3%;
[0148] The ingredients of the intermediate unit layer C include: a high-temperature hot melt adhesive ratio of P1, a use temperature of T3, and a NdFeB magnetic powder ratio of P2, wherein 50%<P1<98%, 140℃<T3<180℃, and 2%<P2<50%;
[0149] When the type of the laminated multi-layer coated elastic patch is layered coating with odor / fragrance additives, the middle layer ingredients are set to include the middle unit layer A ingredients and the middle unit layer B ingredients:
[0150] The ingredients of the middle unit layer A include: sweat-resistant hot melt adhesive accounts for M1, use temperature is T1, PVPk30 accounts for M2, pregelatinized starch accounts for M3, wintergreen oil accounts for M4, bisabolol accounts for M5, menthol accounts for M6, BHT accounts for M7, wherein 50%<M1<98%, 100℃<T1<140℃, 0.1%<M2<15%, 0.1%<M3<5%, 0.1%<M4<15%, 0.1%<M5<3%, 0.2%<M6<6%, 0.1%<M7<3%;
[0151] The ingredients of the intermediate unit layer B include: low-temperature hot melt adhesive accounts for N1, use temperature is T2, flavor accounts for N2, BHT accounts for N3, among which 92%<N1<98%, 90℃<T2<130℃, 2%<N2<5%, 0.1%<N3<3%;
[0152] When the type of the laminated multi-layer coated elastic patch is multi-layer drug segmented effective layered coating, the intermediate layer ingredients are set to include the intermediate unit layer A ingredients, the intermediate unit layer B ingredients and the intermediate unit layer C ingredients:
[0153] The ingredients of the intermediate unit layer A include: intermediate unit layer A: sweat-resistant hot melt adhesive accounts for M1, use temperature is T1, PVPk30 accounts for M2, pregelatinized starch accounts for M3, eucalyptus oil accounts for M4, bisabolol accounts for M5, menthol accounts for M6, BHT accounts for M7, wherein 50%<M1<98%, 100℃<T1<140℃, 0.1%<M2<15%, 0.1%<M3<5%, 0.1%<M4<15%, 0.1%<M5<3%, 0.2%<M6<6%, 0.1%<M7<3%;
[0154] The ingredients of the intermediate unit layer B include: low-temperature hot melt adhesive accounts for N1, the use temperature is T2, far-infrared ceramic powder accounts for N2, magnesium sulfate accounts for N3, BHT accounts for N4, among which 50%<N1<98%, 90℃<T2<130℃, 2%<N2<50%, 0.5%<N3<10%, 0.1%<N4<3%;
[0155] The ingredients of the middle unit layer C include: high-temperature hot melt adhesive accounting for 100%, and the use temperature is T3, wherein 140°C<T3<180°C.
[0156] See also Figure 2As shown, it is a schematic flow chart of the intermediate layer mixing method in this embodiment. In the step S3, the intermediate layer mixing method includes:
[0157] Step S30, adding a preset type of hot melt adhesive into a mixing kettle;
[0158] Step S31, in a mixing kettle, performing a curing treatment on a preset type of hot melt adhesive according to a rated curing temperature and a rated curing time to obtain a cured raw material;
[0159] Step S32, in a mixing kettle, stirring the gelled raw material according to a rated rotation speed and a rated stirring time and adding specific materials to obtain a mixed raw material;
[0160] Step S33, in a mixing kettle, stirring the mixed raw materials at a constant standby temperature to obtain the intermediate unit layer raw materials.
[0161] Specifically, in step S31, the rated gluing time refers to the duration of the gluing process set according to the preset type of hot melt adhesive. This embodiment does not limit the rated gluing time, and relevant personnel in this field can set it by themselves, as long as it meets the requirements for the preset type of hot melt adhesive.
[0162] Specifically, in step S32, the rated speed refers to the preset speed of the mixer. This embodiment does not limit the rated speed, and relevant personnel in this field can set it by themselves, as long as it meets the requirements of the preset type of hot melt adhesive. For example, the rated speed can be set to 50rpm.
[0163] Specifically, in step S32, the rated stirring time refers to the stirring and mixing time of each material in the specific material. For example, the stirring and mixing time of each material in the specific material can be set to 0.5h.
[0164] Specifically, in step S33, the constant standby temperature refers to the temperature of the mixing kettle when it is ready for use after the mixing is completed. For example, the constant standby temperature can be set equal to the rated gelling temperature.
[0165] Specifically, in step S3, when preparing the intermediate unit layer raw material, the intermediate unit layer raw material is prepared according to the intermediate layer batching and intermediate layer mixing method parameters, wherein:
[0166] When the type of the elastic patch for laminated multilayer coating is layered coating with organic / inorganic additives, the intermediate layer mixing method parameters are set to include the intermediate unit layer A mixing method parameters, the intermediate unit layer B mixing method parameters and the intermediate unit layer C mixing method parameters, wherein:
[0167] The parameters of the mixing method of the intermediate unit layer A include: a rated curing temperature of 110°C, a rated curing time of 2h, a rated rotation speed of 50rpm, a rated stirring time of 0.5h, and a constant temperature standby temperature of 110°C;
[0168] The parameters of the mixing method of the intermediate unit layer B include: a rated curing temperature of 100°C, a rated curing time of 2h, a rated rotation speed of 50rpm, a rated stirring time of 0.5h, and a constant temperature standby temperature of 100°C;
[0169] The parameters of the mixing method of the intermediate unit layer C include: a rated curing temperature of 150°C, a rated curing time of 2h, a rated rotation speed of 50rpm, a rated stirring time of 0.5h, and a constant temperature standby temperature of 150°C;
[0170] When the type of the elastic patch for laminated multilayer coating is layered coating with odor / fragrance additives, the intermediate layer mixing method parameters are set to include the intermediate unit layer A mixing method parameters and the intermediate unit layer B mixing method parameters.
[0171] The parameters of the mixing method of the intermediate unit layer A include: a rated curing temperature of 110°C, a rated curing time of 2h, a rated rotation speed of 50rpm, a rated stirring time of 0.5h, and a constant temperature standby temperature of 110°C;
[0172] The parameters of the mixing method of the intermediate unit layer B include: a rated curing temperature of 100°C, a rated curing time of 2h, a rated rotation speed of 50rpm, a rated stirring time of 0.5h, and a constant temperature standby temperature of 100°C;
[0173] When the type of the elastic patch with laminated multi-layer coating is multi-layer drug segmented effective layer coating, the intermediate layer mixing method parameters are set to include the intermediate unit layer A mixing method parameters, the intermediate unit layer B mixing method parameters and the intermediate unit layer C mixing method parameters, wherein:
[0174] The parameters of the mixing method of the middle unit layer A are as follows: the rated curing temperature is 110°C, the rated curing time is 2h, the rated speed is 50rpm, the rated stirring time is 0.5h, and the constant temperature standby temperature is 110°C;
[0175] Parameters of the mixing method of the intermediate unit layer B: rated curing temperature is 100°C, rated curing time is 2h, rated speed is 50rpm, rated stirring time is 0.5h, and constant temperature standby temperature is 100°C;
[0176] The parameters of the mixing method of the intermediate unit layer C are as follows: the rated curing temperature is 150°C, the rated curing time is 2h, the rated rotation speed is 50rpm, the rated stirring time is 0.5h, and the constant temperature standby temperature is 150°C.
[0177] Specifically, through step S3, the intermediate layer ingredients and intermediate layer mixing method parameters are set according to the type of laminated and multi-layer coated elastic patch, and the intermediate unit layer raw materials are prepared according to the intermediate layer ingredients and intermediate layer mixing method parameters. Different intermediate layer ingredients and mixing method parameters are used to solve the problems of mutual reaction failure between raw materials of single-layer patches and poor odor isolation of patches, so as to increase the comfort of use.
[0178] See also Figure 3 As shown, in step S4, it is a schematic flow chart of the coating method of this embodiment. In step S4, the coating method includes:
[0179] Step S40, starting coating with the innermost layer as the bottom layer;
[0180] Step S41, performing layered coating to obtain a combination of an innermost layer and an intermediate layer;
[0181] Step S42, preparing a roll of plaster according to the combination of the innermost layer and the middle layer and the outermost layer;
[0182] Step S43, aging overnight, packaging the rolled plaster pieces to obtain a laminated multi-layer coated elastic plaster, the laminated multi-layer coated elastic plaster comprising an organic / inorganic additive layered coating, an odor / fragrance additive layered coating and a multi-layer drug segmented effect layered coating.
[0183] Specifically, in step S41, when performing layered coating, the intermediate unit layer raw material is coated on the innermost layer according to the intermediate unit layer sequence, coating rated temperature and coating rated gram weight, and the coating layer temperature is waited to drop to room temperature, and the above steps are repeated until the intermediate unit layer coating is completed.
[0184] Specifically, in step S41, the sequence of the intermediate unit layers is the inner and outer order of the intermediate unit layers. For example, the intermediate unit layer A can be connected to the outermost layer, and the sequence from outside to inside is: intermediate unit layer A, intermediate unit layer B, ..., intermediate unit layer M.
[0185] Specifically, in step S41, the rated coating temperature is the preset temperature of each intermediate unit layer during coating. This embodiment does not limit the preset temperature of the intermediate unit layer, and relevant personnel in this field can set it by themselves, such as setting the rated coating temperature to 150°C.
[0186] Specifically, in step S41, the rated coating weight is the weight of each intermediate unit layer of raw material during coating.
[0187] Specifically, in step S41, the room temperature is the temperature in the room where the coating is performed, and generally 24°C can be used as the room temperature.
[0188] Specifically, in step S42, when preparing the rolled plaster, the innermost layer and the middle layer combination are compounded with the outermost layer into a roll according to the rated compounding temperature to obtain the rolled plaster.
[0189] Specifically, in step S42, the composite temperature refers to the preset temperature when the middle layer and the outermost layer are synthesized. This embodiment does not limit the composite temperature, and relevant personnel in this field can set it by themselves, such as setting the coating composite temperature to 80±10°C.
[0190] Specifically, in step S43, the overnight aging means placing the rolled patch for 12 hours to allow the innermost layer, the middle layer and the outermost layer to be fully adhered.
[0191] Specifically, in step S4, when setting the unit layer parameters of the coating method, the unit layer parameters of the coating method are set according to the type of elastic patch for laminated multilayer coating, wherein:
[0192] When the type of the elastic patch of the laminated multilayer coating is layered coating with organic / inorganic additives, the coating method unit layer parameters are set to include the coating parameters of the middle unit layer A, the coating parameters of the middle unit layer B and the coating parameters of the middle unit layer C, wherein:
[0193] The coating parameters of the intermediate unit layer A include:
[0194] The rated temperature of the middle unit layer A during coating is 110°C.
[0195] The rated weight of the coating of the middle unit layer A is 50g / m 2 ,
[0196] The coating and compounding temperature of the middle unit layer A is 80±10℃;
[0197] The coating parameters of the intermediate unit layer B include:
[0198] The rated temperature of the middle unit layer B during coating is 100°C.
[0199] The rated weight of the coating of the middle unit layer B is 50g / m 2 ,
[0200] The coating temperature of the middle unit layer B is 80±10℃;
[0201] The coating parameters of the intermediate unit layer C include:
[0202] The rated temperature of the intermediate unit layer C coating is 150°C.
[0203] The rated weight of the middle unit layer C coating is 80g / m 2 ,
[0204] The coating temperature of the middle unit layer C is 80±10℃;
[0205] When the type of the elastic patch for laminated multilayer coating is layered coating of odor / fragrance additives, the coating method unit layer parameters are set to include the coating parameters of the middle unit layer A and the coating parameters of the middle unit layer B, wherein:
[0206] The coating parameters of the intermediate unit layer A include:
[0207] The rated temperature of the middle unit layer A during coating is 110°C.
[0208] The rated weight of the coating of the middle unit layer A is 80g / m2.
[0209] The coating and compounding temperature of the middle unit layer A is 80±10℃;
[0210] The coating parameters of the intermediate unit layer B include:
[0211] The rated temperature of the middle unit layer B during coating is 100°C.
[0212] The rated weight of the middle unit layer B coating is 100g / m 2 ,
[0213] The coating temperature of the middle unit layer B is 80±10℃;
[0214] When the type of the elastic patch with laminated multi-layer coating is multi-layer drug segmented effective layered coating, the coating method unit layer parameters are set to include the coating parameters of the middle unit layer A, the coating parameters of the middle unit layer B and the coating parameters of the middle unit layer C, wherein:
[0215] The coating parameters of the intermediate unit layer A include:
[0216] The rated temperature of the middle unit layer A during coating is 110°C.
[0217] The rated weight of the coating of the middle unit layer A is 50g / m 2 ,
[0218] The coating and compounding temperature of the middle unit layer A is 80±10℃;
[0219] The coating parameters of the intermediate unit layer B include:
[0220] The rated temperature of the middle unit layer B during coating is 100°C.
[0221] The rated weight of the middle unit layer B coating is 100g / m 2 ,
[0222] The coating temperature of the middle unit layer B is 80±10℃;
[0223] The coating parameters of the intermediate unit layer C include:
[0224] The rated temperature of the intermediate unit layer C coating is 150°C.
[0225] The middle unit layer C coating rated weight is 50g / m 2 ,
[0226] The coating temperature of the middle unit layer B is 80±10°C.
[0227] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.
Claims
1. A method for producing a laminated multi-layer coated elastic plaster, characterized in that: include: Step S1, setting the outermost layer parameters according to the type of the elastic patch to be laminated and multi-layered, and preparing the outermost layer according to the outermost layer parameters; Step S2, setting the innermost layer parameters according to the type of the elastic patch to be laminated and coated with multiple layers, and preparing the innermost layer according to the innermost layer parameters; Step S3, setting the parameters of the intermediate layer ingredients and the intermediate layer mixing method according to the type of the elastic patch to be laminated and multi-layered, and preparing the intermediate unit layer raw materials according to the parameters of the intermediate layer ingredients and the intermediate layer mixing method; Step S4: setting the unit layer parameters of the coating method according to the type of laminated multi-layer coated elastic patch, and connecting the outermost layer, the middle unit layer raw materials and the innermost layer according to the coating method to obtain a laminated multi-layer coated elastic patch; the types of laminated multi-layer coated elastic patches include layered coating with organic / inorganic additives, layered coating with odor / fragrance additives and layered coating with multi-layer drugs in sections.
2. The method for making a laminated multi-layer coated elastic patch according to claim 1, characterized in that: In the step S3, the intermediate layer is composed of intermediate unit layers of a preset number n, including a first preset intermediate unit layer A, a second preset intermediate unit layer B, ..., an nth preset intermediate unit layer M, wherein the preset number n≥2 and n is an integer.
3. The method for making a laminated multi-layer coated elastic patch according to claim 2, characterized in that: In step S3, the middle layer ingredients are set to preset types of hot melt adhesive and specific materials, the preset types of hot melt adhesive include low-temperature hot melt adhesive, sweat-resistant hot melt adhesive and high-temperature hot melt adhesive, and the specific materials include pregelatinized starch, ginger extract, bisabolol, menthol, BHT, far-infrared ceramic powder, neodymium iron boron magnetic powder, PVPk30, wintergreen oil, essence, eucalyptus oil and magnesium sulfate.
4. The method for making a laminated multi-layer coated elastic patch according to claim 3, characterized in that: In step S3, when setting the ingredients of the middle layer, the ingredients of the middle layer are set according to the type of elastic plaster to be laminated and coated with multiple layers, wherein: When the type of the elastic plaster with laminated multilayer coating is layered coating with organic / inorganic additives, the intermediate layer ingredients are set to include intermediate unit layer A ingredients, intermediate unit layer B ingredients and intermediate unit layer C ingredients, wherein: The ingredients of the intermediate unit layer A include: sweat-resistant hot melt adhesive accounts for M1, use temperature is T1, PVPk30 accounts for M2, pregelatinized starch accounts for M3, ginger extract accounts for M4, bisabolol accounts for M5, menthol accounts for M6, BHT accounts for M7, wherein 50%<M1<98%, 100℃<T1<140℃, 0.1%<M2<15%, 0.1%<M3<5%, 0.1%<M4<15%, 0.1%<M5<3%, 0.2%<M6<6%, 0.1%<M7<3%; The ingredients of the intermediate unit layer B include: low-temperature hot melt adhesive accounts for N1, the use temperature is T2, far-infrared ceramic powder accounts for N2, and BHT accounts for N3, wherein 50%<N1<98%, 90℃<T2<130℃, 2%<N2<50%, and 0.1%<N3<3%; The ingredients of the intermediate unit layer C include: a high-temperature hot melt adhesive ratio of P1, a use temperature of T3, and a NdFeB magnetic powder ratio of P2, wherein 50%<P1<98%, 140℃<T3<180℃, and 2%<P2<50%; When the type of the laminated multi-layer coated elastic patch is layered coating with odor / fragrance additives, the middle layer ingredients are set to include the middle unit layer A ingredients and the middle unit layer B ingredients: The ingredients of the middle unit layer A include: sweat-resistant hot melt adhesive accounts for M1, use temperature is T1, PVPk30 accounts for M2, pregelatinized starch accounts for M3, wintergreen oil accounts for M4, bisabolol accounts for M5, menthol accounts for M6, BHT accounts for M7, wherein 50%<M1<98%, 100℃<T1<140℃, 0.1%<M2<15%, 0.1%<M3<5%, 0.1%<M4<15%, 0.1%<M5<3%, 0.2%<M6<6%, 0.1%<M7<3%; The ingredients of the intermediate unit layer B include: low-temperature hot melt adhesive accounts for N1, use temperature is T2, flavor accounts for N2, BHT accounts for N3, among which 92%<N1<98%, 90℃<T2<130℃, 2%<N2<5%, 0.1%<N3<3%; When the type of the laminated multi-layer coated elastic patch is multi-layer drug segmented effective layered coating, the intermediate layer ingredients are set to include the intermediate unit layer A ingredients, the intermediate unit layer B ingredients and the intermediate unit layer C ingredients: The ingredients of the intermediate unit layer A include: intermediate unit layer A: sweat-resistant hot melt adhesive accounts for M1, use temperature is T1, PVPk30 accounts for M2, pregelatinized starch accounts for M3, eucalyptus oil accounts for M4, bisabolol accounts for M5, menthol accounts for M6, BHT accounts for M7, wherein 50%<M1<98%, 100℃<T1<140℃, 0.1%<M2<15%, 0.1%<M3<5%, 0.1%<M4<15%, 0.1%<M5<3%, 0.2%<M6<6%, 0.1%<M7<3%; The ingredients of the intermediate unit layer B include: low-temperature hot melt adhesive accounts for N1, the use temperature is T2, far-infrared ceramic powder accounts for N2, magnesium sulfate accounts for N3, BHT accounts for N4, among which 50%<N1<98%, 90℃<T2<130℃, 2%<N2<50%, 0.5%<N3<10%, 0.1%<N4<3%; The ingredients of the middle unit layer C include: high-temperature hot melt adhesive accounting for 100%, and the use temperature is T3, wherein 140°C<T3<180°C.
5. The method for making a laminated multi-layer coated elastic patch according to claim 4, characterized in that: In step S3, the intermediate layer mixing method includes: Step S30, adding a preset type of hot melt adhesive into a mixing kettle; Step S31, in a mixing kettle, performing a curing treatment on a preset type of hot melt adhesive according to a rated curing temperature and a rated curing time to obtain a cured raw material; Step S32, in a mixing kettle, stirring the gelled raw material according to a rated rotation speed and a rated stirring time and adding specific materials to obtain a mixed raw material; Step S33, in a mixing kettle, stirring the mixed raw materials at a constant standby temperature to obtain the intermediate unit layer raw materials.
6. The method for making a laminated multi-layer coated elastic patch according to claim 5, characterized in that: In the step S3, when preparing the intermediate unit layer raw material, the intermediate unit layer raw material is prepared according to the intermediate layer batching and intermediate layer mixing method parameters, wherein: When the type of the elastic patch for laminated multilayer coating is layered coating with organic / inorganic additives, the intermediate layer mixing method parameters are set to include the intermediate unit layer A mixing method parameters, the intermediate unit layer B mixing method parameters and the intermediate unit layer C mixing method parameters, wherein: The parameters of the mixing method of the intermediate unit layer A include: a rated curing temperature of 110°C, a rated curing time of 2h, a rated rotation speed of 50rpm, a rated stirring time of 0.5h, and a constant temperature standby temperature of 110°C; The parameters of the mixing method of the intermediate unit layer B include: a rated curing temperature of 100°C, a rated curing time of 2h, a rated rotation speed of 50rpm, a rated stirring time of 0.5h, and a constant temperature standby temperature of 100°C; The parameters of the mixing method of the intermediate unit layer C include: a rated curing temperature of 150°C, a rated curing time of 2h, a rated rotation speed of 50rpm, a rated stirring time of 0.5h, and a constant temperature standby temperature of 150°C; When the type of the elastic patch for laminated multilayer coating is layered coating with odor / fragrance additives, the intermediate layer mixing method parameters are set to include the intermediate unit layer A mixing method parameters and the intermediate unit layer B mixing method parameters. The parameters of the mixing method of the intermediate unit layer A include: a rated curing temperature of 110°C, a rated curing time of 2h, a rated rotation speed of 50rpm, a rated stirring time of 0.5h, and a constant temperature standby temperature of 110°C; The parameters of the mixing method of the intermediate unit layer B include: a rated curing temperature of 100°C, a rated curing time of 2h, a rated rotation speed of 50rpm, a rated stirring time of 0.5h, and a constant temperature standby temperature of 100°C; When the type of the elastic patch with laminated multi-layer coating is multi-layer drug segmented effective layer coating, the intermediate layer mixing method parameters are set to include the intermediate unit layer A mixing method parameters, the intermediate unit layer B mixing method parameters and the intermediate unit layer C mixing method parameters, wherein: The parameters of the mixing method of the middle unit layer A are as follows: the rated curing temperature is 110°C, the rated curing time is 2h, the rated speed is 50rpm, the rated stirring time is 0.5h, and the constant temperature standby temperature is 110°C; Parameters of the mixing method of the intermediate unit layer B: rated curing temperature is 100°C, rated curing time is 2h, rated speed is 50rpm, rated stirring time is 0.5h, and constant temperature standby temperature is 100°C; The parameters of the mixing method of the intermediate unit layer C are as follows: the rated curing temperature is 150°C, the rated curing time is 2h, the rated rotation speed is 50rpm, the rated stirring time is 0.5h, and the constant temperature standby temperature is 150°C.
7. The method for making a laminated multi-layer coated elastic patch according to claim 6, characterized in that: In the step S4, the coating method comprises: Step S40, starting coating with the innermost layer as the bottom layer; Step S41, performing layered coating to obtain a combination of an innermost layer and an intermediate layer; Step S42, preparing a roll of plaster according to the combination of the innermost layer and the middle layer and the outermost layer; Step S43, aging overnight, packaging the rolled plaster pieces, and obtaining a laminated multi-layer coated elastic plaster.
8. The method for making a laminated multi-layer coated elastic patch according to claim 7, characterized in that: In step S41, when performing layered coating, the intermediate unit layer raw material is coated on the innermost layer according to the intermediate unit layer sequence, coating rated temperature and coating rated gram weight, and the coating layer temperature is waited to drop to room temperature, and the above steps are repeated until the intermediate unit layer coating is completed.
9. The method for making a laminated multi-layer coated elastic patch according to claim 8, characterized in that: In the step S42, when preparing the rolled plaster, the innermost layer and the middle layer combination are compounded with the outermost layer into a roll according to the rated compounding temperature to obtain the rolled plaster.
10. The method for making a laminated multi-layer coated elastic patch according to claim 9, characterized in that: In step S4, when setting the unit layer parameters of the coating method, the unit layer parameters of the coating method are set according to the type of elastic patch for laminated multilayer coating, wherein: When the type of the elastic patch of the laminated multilayer coating is layered coating with organic / inorganic additives, the coating method unit layer parameters are set to include the coating parameters of the middle unit layer A, the coating parameters of the middle unit layer B and the coating parameters of the middle unit layer C, wherein: The coating parameters of the intermediate unit layer A include: The rated temperature of the middle unit layer A during coating is 110°C. The rated weight of the coating of the middle unit layer A is 50g / m 2 , The coating and compounding temperature of the middle unit layer A is 80±10℃; The coating parameters of the intermediate unit layer B include: The rated temperature of the middle unit layer B during coating is 100°C. The rated weight of the coating of the middle unit layer B is 50g / m 2 , The coating temperature of the middle unit layer B is 80±10℃; The coating parameters of the intermediate unit layer C include: The rated temperature of the intermediate unit layer C coating is 150°C. The rated weight of the middle unit layer C coating is 80g / m 2 , The coating temperature of the middle unit layer C is 80±10℃; When the type of the elastic patch for laminated multilayer coating is layered coating of odor / fragrance additives, the coating method unit layer parameters are set to include the coating parameters of the middle unit layer A and the coating parameters of the middle unit layer B, wherein: The coating parameters of the intermediate unit layer A include: The rated temperature of the middle unit layer A during coating is 110°C. The rated weight of the coating of the middle unit layer A is 80g / m2. The coating and compounding temperature of the middle unit layer A is 80±10℃; The coating parameters of the intermediate unit layer B include: The rated temperature of the middle unit layer B during coating is 100°C. The rated weight of the middle unit layer B coating is 100g / m 2 , The coating temperature of the middle unit layer B is 80±10℃; When the type of the elastic patch with laminated multi-layer coating is multi-layer drug segmented effective layered coating, the coating method unit layer parameters are set to include the coating parameters of the middle unit layer A, the coating parameters of the middle unit layer B and the coating parameters of the middle unit layer C, wherein: The coating parameters of the intermediate unit layer A include: The rated temperature of the middle unit layer A during coating is 110°C. The rated weight of the coating of the middle unit layer A is 50g / m 2 , The coating and compounding temperature of the middle unit layer A is 80±10℃; The coating parameters of the intermediate unit layer B include: The rated temperature of the middle unit layer B during coating is 100°C. The rated weight of the middle unit layer B coating is 100g / m 2 , The coating temperature of the middle unit layer B is 80±10℃; The coating parameters of the intermediate unit layer C include: The rated temperature of the intermediate unit layer C coating is 150°C. The middle unit layer C coating rated weight is 50g / m 2 , The coating temperature of the middle unit layer B is 80±10°C.