Modified carbon sequestration material as well as preparation method and application thereof

By coating silica particles on the surface of the steel slag and using chemical precipitation reaction, the iron release rate is controlled, and the problems of energy consumption and low iron utilization in the carbon sequestration process are solved, and the efficient utilization of steel slag components and marine carbon are achieved. The carbon sequestration effect of sink.

CN119015867APending Publication Date: 2024-11-26SUN YAT SEN UNIV +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411119116.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art consumes a lot of energy in the carbon sequestration process and has low utilization of iron in steel slag. The component utilization rate of steel slag is low. A modified carbon sequestration material that can effectively release iron elements is needed to improve the carbon sequestration effect.

Method used

By coating silica particles on the surface of the steel slag, nanoscale silica precipitation is generated by chemical precipitation reaction, controlling the release rate of iron elements, improving the utilization rate of various components in the steel slag, and fixing through photosynthesis of marine plankton carbon dioxide.

Benefits of technology

The effective utilization of iron elements in steel slag is achieved, the utilization rate of steel slag components is improved, the growth of marine plankton is promoted, the carbon sequestration capacity of marine carbon sinks is enhanced, and carbon dioxide is prevented from re-entering the biological carbon circulation system.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119015867A_ABST
    Figure CN119015867A_ABST
Patent Text Reader

Abstract

The invention discloses a modified carbon sequestration material as well as a preparation method and application thereof, and belongs to the technical field of environment-friendly materials. The modified carbon sequestration material provided by the invention comprises steel slag and silicon dioxide particles, wherein the silicon dioxide particles are coated on the surface of the steel slag. The surface of the steel slag is coated with the silicon dioxide particles, the obtained modified carbon sequestration material has a moderate dissolution rate, and particularly, the release rate of an iron element is controllable, so that the iron element in the steel slag is effectively utilized, the utilization rate of each component in the steel slag is high, and dissolved substances of the material are beneficial to growth and reproduction of marine planktons; the modified carbon sequestration material disclosed by the invention is widely applied to fixation of carbon dioxide, especially fixation of carbon dioxide in a marine environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of environmentally friendly materials, and in particular relates to a modified carbon-fixing material and a preparation method and application thereof. Background Art

[0002] Steel slag is a solid waste produced during the steelmaking process. It is composed of various oxides formed by the oxidation of impurities such as silicon, manganese, phosphorus, and sulfur in pig iron during the smelting process, as well as salts generated by the reaction of these oxides with solvents. The output of steel slag is very large, accounting for about 8% to 15% of crude steel output. With the continuous growth of steel production, the output of steel slag is also increasing rapidly. Steel slag contains a variety of useful components: 2% to 8% of metallic iron, 40% to 60% of calcium oxide, 3% to 10% of magnesium oxide, 1% to 8% of manganese oxide, etc. However, the current secondary utilization of steel slag is not optimistic. Steel slag is mainly used in road engineering, building materials and other fields. Many steel slags have to be piled up in the open air, occupying a large amount of land while polluting the environment, and insufficient utilization of the rich metal elements in steel slag.

[0003] Steel slag contains a large amount of metal oxides and has great application potential in the field of carbon fixation. At present, the research and utilization of steel slag in the field of carbon fixation is mainly focused on steel slag carbonization technology, which uses the large amount of calcium and magnesium oxides contained in steel slag to combine with carbon dioxide to form carbonates for carbon fixation. The current scheme mainly utilizes alkali metal elements such as calcium and magnesium in steel slag, while the iron element, which is also rich in content, has not been well utilized, and it usually requires a certain high temperature and high pressure environment, and the reaction conditions are relatively harsh.

[0004] The ocean is the largest carbon reservoir on Earth, absorbing about 2 billion tons of CO2 from the atmosphere each year, accounting for 1 / 3 of the world's annual CO2 emissions. The algae in the ocean have the strongest carbon fixation capacity, and about 90% of photosynthesis on Earth is completed by marine algae. Therefore, artificially promoting the growth of marine algae is also a very promising carbon sink. From the existing literature "Zhang Wuchang, Sun Song. Iron hypothesis and field iron enrichment experiment in HNLC sea area [J]. Progress in Earth Science, 2002 (04): 612-615." It can be seen that there are many high-nutrient low-chlorophyll (HNLC) areas in the ocean. The nutrient content in this part of the ocean is excessive, while the iron content is extremely low. The growth of algae is mainly limited by the iron content. In addition, researchers have conducted multiple iron enrichment experiments in many places, confirming the effectiveness of iron addition for phytoplankton growth. However, the iron source used in these experiments was mainly soluble iron, and the element was released too quickly. A large amount of iron in the seawater was oxidized into trivalent iron and quickly precipitated, resulting in low utilization of the iron.

[0005] Therefore, in the prior art, the carbon fixation process consumes a large amount of energy, and the utilization rate of the components contained in the steel slag is not high. There is a large loss of iron elements in the carbon fixation process, and the utilization rate is not high. It is necessary to find another effective carbon fixation material. Summary of the invention

[0006] In order to overcome at least one of the problems existing in the above-mentioned prior art, one of the objects of the present invention is to provide a modified carbon-fixing material, in which the release rate of iron elements is moderate, the utilization rate of each component in the steel slag is high, and a good carbon-fixing effect can be achieved.

[0007] A second object of the present invention is to provide a method for preparing the above-mentioned modified carbon-fixing material.

[0008] The third object of the present invention is to provide an application of the above-mentioned modified carbon-fixing material in fixing carbon dioxide.

[0009] In order to achieve the above object, the technical solution adopted by the present invention is:

[0010] A first aspect of the present invention provides a modified carbon-fixing material, comprising steel slag and silicon dioxide particles, wherein the silicon dioxide particles are coated on the surface of the steel slag.

[0011] In some specific embodiments of the present invention, the silicon dioxide particles are coated on the surface of the steel slag by in-situ growth.

[0012] Preferably, the average particle size of the silicon dioxide particles is 100 to 1000 nm; more preferably 300 to 800 nm; and even more preferably 400 to 700 nm.

[0013] Preferably, the average particle size of the steel slag is 50 to 400 μm; more preferably, it is 75 to 375 μm; and even more preferably, it is 75 to 100 μm.

[0014] Preferably, the iron content in the steel slag is 15-40wt%; more preferably, it is 20-35wt%.

[0015] In some specific embodiments of the present invention, the composition of the steel slag includes at least one of CaO, FeO, SiO2, Al2O3, MgO and P2O3; in some more specific embodiments of the present invention, the composition of the steel slag includes CaO, FeO, SiO2, Al2O3, MgO and P2O3.

[0016] The second aspect of the present invention provides a method for preparing the modified carbon-fixing material described in the first aspect of the present invention, comprising the following steps: subjecting a mixed solution containing a silicon source, a surfactant, water and steel slag to a precipitation reaction with an acid to obtain the modified carbon-fixing material.

[0017] The principle of the precipitation reaction adopted in the preparation method of the present invention is that a silicon source reacts with an acid to generate a nano-scale silica precipitate. In the presence of a surfactant, the silica will not agglomerate quickly and can exist relatively stably in the solution. Since the steel slag has a rough surface and high chemical activity, the nano-silicon dioxide can easily use the steel slag surface as a nucleation site, adhere to and grow on the steel slag surface, and achieve coating of the steel slag surface.

[0018] Taking silicate as the silicon source as an example, the specific precipitation reaction equation is as follows: nSiO 3- +2mH + →nSiO2·mH2O↓+(m-3n)H2O.

[0019] Preferably, the silicon source includes at least one of sodium silicate, potassium silicate or sodium metasilicate; further preferably, the silicon source is selected from sodium silicate.

[0020] Preferably, the surfactant comprises at least one of polyethylene glycol, poloxamer or Tween; further preferably, the surfactant is selected from polyethylene glycol.

[0021] Preferably, the average molecular weight of the polyethylene glycol is 4000-8000; more preferably 5000-7000.

[0022] In some specific embodiments of the present invention, the surfactant is selected from polyethylene glycol with an average molecular weight of 6000, namely PEG-6000.

[0023] Preferably, the acid comprises at least one of hydrochloric acid, sulfuric acid or nitric acid; further preferably, the acid comprises hydrochloric acid, sulfuric acid or a combination thereof; further preferably, the acid is selected from hydrochloric acid.

[0024] Preferably, in the mixed solution, the molar concentration of the silicon source is 0.01 to 1 mol / L; more preferably, it is 0.05 to 0.7 mol / L; and even more preferably, it is 0.1 to 0.4 mol / L.

[0025] Preferably, the mass ratio of the silicon source to the surfactant is (10-100):1; more preferably (20-90):1; and even more preferably (40-80):1.

[0026] Preferably, the mass ratio of the surfactant to the steel slag is 1:(80-120); more preferably 1:(85-115); and even more preferably 1:(90-110).

[0027] Preferably, the concentration of the acid is 0.1 to 3 mol / L; more preferably, it is 0.3 to 2 mol / L; and even more preferably, it is 0.5 to 1 mol / L.

[0028] In some specific embodiments of the present invention, the ratio of the mixed solution to the acid is adjusted according to actual conditions so that the pH value during the reaction meets the requirements.

[0029] Preferably, the pH value of the precipitation reaction is 7-10; more preferably 7.5-9.5; further preferably 8-9.

[0030] Preferably, the temperature of the precipitation reaction is 30-100°C; more preferably 40-90°C; and even more preferably 50-80°C.

[0031] Preferably, the precipitation reaction time is 5 to 200 min; more preferably, it is 10 to 180 min; and even more preferably, it is 10 to 40 min.

[0032] The third aspect of the present invention provides a use of the modified carbon-fixing material described in the first aspect of the present invention for fixing carbon dioxide in a marine environment.

[0033] The fixing of carbon dioxide or carbon sequestration mentioned in the present invention refers to fixing carbon dioxide in the form of organic carbon in the ocean to prevent it from re-entering the biological carbon circulation system.

[0034] Preferably, the modified carbon-fixing material fixes carbon dioxide by promoting photosynthesis of marine plankton; further preferably, the marine plankton is seaweed; further preferably, the seaweed is diatom; more preferably, the diatom is Phaeodactylum tricornutum.

[0035] The beneficial effects of the present invention are as follows: the present invention coats the surface of steel slag with silicon dioxide particles, and the obtained modified carbon-fixing material has a moderate dissolution rate, especially the release rate of iron element is controllable, so that the iron element in the steel slag is effectively utilized, the utilization rate of each component in the steel slag is high, and the dissolution of the material is beneficial to the growth and reproduction of marine plankton, and is beneficial to promoting its photosynthesis to achieve the effect of carbon fixation. The modified carbon-fixing material of the present invention has a wide range of applications in fixing carbon dioxide in the marine environment.

[0036] Specifically, compared with the prior art, the present invention has the following advantages:

[0037] (1) The modification method of steel slag of the present invention is simple, the raw materials are low-cost, and various components in the steel slag can be fully utilized. In addition, the problem that industrial waste steel slag cannot be disposed of can be solved, thereby achieving the effect of waste utilization.

[0038] (2) The modification method of steel slag in the present invention can change the leaching process of steel slag. By controlling the conditions such as silicon source concentration, reaction temperature and time, the content of silicon dioxide particles coated on the surface of steel slag can be controlled, thereby achieving the purpose of controlling the dissolution rate of steel slag, thereby making effective use of various components in steel slag.

[0039] (3) The modified carbon-fixing material provided by the present invention can increase the nutrient release rate of steel slag in the marine carbon sink, fully promote the growth of marine plankton such as seaweed, especially diatoms, and their photosynthetic carbon fixation process. Marine plankton sinks to the seabed after death, and can fix carbon dioxide in the ocean in the form of organic carbon, avoiding re-entry into the biological carbon circulation system. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is the SEM image of the uncoated steel slag in Example 1.

[0041] Figure 2 This is the SEM image of the modified carbon-fixing material in Example 1.

[0042] Figure 3 This is the SEM image of silica on the surface of the modified carbon-fixing material in Example 1.

[0043] Figure 4 This is the XRD diagram of the steel slag in Example 1 before and after coating.

[0044] Figure 5 This is a comparison curve of the biomass of P. triangularis and the absorbance of the algae liquid.

[0045] Figure 6 This is a graph showing the effects of Examples 1 to 3 and the control group on the biomass of P. tricornutum for 7 days.

[0046] Figure 7 This is a graph showing the effects of Examples 2, 4, 5 and the control group on the biomass of P. triangularis at 7 days.

[0047] Figure 8 The HCO3 of Examples 1 to 3 and the control group on Phaeodactylum triangularis for 7 days 2- Absorption diagram. DETAILED DESCRIPTION

[0048] The content of the present invention is further described in detail below through specific examples. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the principles set forth in the present invention all belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific data exemplified below. The raw materials, reagents or devices used in the following examples and comparative examples, unless otherwise specified, can all be obtained from conventional commercial sources, or can be obtained by existing known methods.

[0049] It should be noted that the steel slag used in the embodiments of the present invention comes from Zhuhai Xinrui Trading Co., Ltd., item number 019, and its main components are CaO, FeO, SiO2 and part of Al2O3, MgO and P2O3, among which the iron element in the steel slag accounts for about 22% to 30% by mass.

[0050] Example 1

[0051] A modified carbon-fixing material comprises steel slag and silicon dioxide particles, wherein the silicon dioxide particles are coated on the surface of the steel slag. The modified carbon-fixing material is prepared by a chemical precipitation method, which specifically comprises the following steps:

[0052] (1) Prepare 500 mL of a sodium silicate solution with a concentration of 0.1 mol / L, weigh 0.1 g of a surfactant polyethylene glycol (PEG-6000) and add it to the solution to prepare solution A, and keep the solution at a constant temperature of 30° C.;

[0053] (2) Weighing 10 g of steel slag with an average particle size of 75 μm, stirring the solution A obtained in step (1) at a speed of 200 rpm, adding the steel slag to the solution A and stirring for 5 min to obtain steel slag slurry A;

[0054] (3) 0.5 mol / L hydrochloric acid was added dropwise to the steel slag slurry A, stirred at a speed of 200 rpm and kept warm at 50°C, and hydrochloric acid was added dropwise until the pH of the slurry was 9, and then continued to stir and keep warm for 30 minutes. Then, the mixture was filtered, washed, and dried in an oven at 80°C to obtain the modified carbon-fixing material.

[0055] Example 2

[0056] A modified carbon-fixing material comprises steel slag and silicon dioxide particles, wherein the silicon dioxide particles are coated on the surface of the steel slag. The modified carbon-fixing material is prepared by a chemical precipitation method, which specifically comprises the following steps:

[0057] (1) Prepare 500 mL of a sodium silicate solution with a concentration of 0.2 mol / L, weigh 0.1 g of a surfactant polyethylene glycol (PEG-6000) and add it to the solution to prepare solution A, and keep the solution at a constant temperature of 30° C.;

[0058] (2) Weighing 10 g of steel slag with an average particle size of 75 μm, stirring the solution A obtained in step (1) at a speed of 200 rpm, adding the steel slag to the solution A and stirring for 5 min to obtain steel slag slurry A;

[0059] (3) 0.5 mol / L hydrochloric acid was added dropwise to the steel slag slurry A, stirred at a speed of 200 rpm and kept warm at 50°C, and hydrochloric acid was added dropwise until the pH of the slurry was 9, and then continued to stir and keep warm for 30 minutes. Then, the mixture was filtered, washed, and dried in an oven at 80°C to obtain the modified carbon-fixing material.

[0060] Example 3

[0061] A modified carbon-fixing material comprises steel slag and silicon dioxide particles, wherein the silicon dioxide particles are coated on the surface of the steel slag. The modified carbon-fixing material is prepared by a chemical precipitation method, which specifically comprises the following steps:

[0062] (1) Prepare 500 mL of a sodium silicate solution with a concentration of 0.4 mol / L, weigh 0.1 g of a surfactant polyethylene glycol (PEG-6000) and add it to the solution to prepare solution A, and keep the solution at a constant temperature of 30° C.;

[0063] (2) Weighing 10 g of steel slag with an average particle size of 75 μm, stirring the solution A obtained in step (1) at a speed of 200 rpm, adding the steel slag to the solution A and stirring for 5 min to obtain steel slag slurry A;

[0064] (3) 0.5 mol / L hydrochloric acid was added dropwise to the steel slag slurry A, stirred at a speed of 200 rpm and kept warm at 50°C, and hydrochloric acid was added dropwise until the pH of the slurry was 9, and then continued to stir and keep warm for 30 minutes. Then, the mixture was filtered, washed, and dried in an oven at 80°C to obtain the modified carbon-fixing material.

[0065] Example 4

[0066] A modified carbon-fixing material comprises steel slag and silicon dioxide particles, wherein the silicon dioxide particles are coated on the surface of the steel slag. The modified carbon-fixing material is prepared by a chemical precipitation method, which specifically comprises the following steps:

[0067] (1) Prepare 500 mL of a sodium silicate solution with a concentration of 0.2 mol / L, weigh 0.1 g of a surfactant polyethylene glycol (PEG-6000) and add it to the solution to prepare solution A, and keep the solution at a constant temperature of 30° C.;

[0068] (2) Weighing 10 g of steel slag with an average particle size of 75 μm, stirring the solution A obtained in step (1) at a speed of 200 rpm, adding the steel slag to the solution A and stirring for 5 min to obtain steel slag slurry A;

[0069] (3) 0.5 mol / L hydrochloric acid was added dropwise to the steel slag slurry A, stirred at a speed of 200 rpm and kept warm at 50°C, and hydrochloric acid was added dropwise until the pH of the slurry was 9, and then continued to stir and keep warm for 10 minutes. Then, the mixture was filtered, washed, and dried in an oven at 80°C to obtain the modified carbon-fixing material.

[0070] Example 5

[0071] A modified carbon-fixing material comprises steel slag and silicon dioxide particles, wherein the silicon dioxide particles are coated on the surface of the steel slag. The modified carbon-fixing material is prepared by a chemical precipitation method, which specifically comprises the following steps:

[0072] (1) Prepare 500 mL of a sodium silicate solution with a concentration of 0.2 mol / L, weigh 0.1 g of a surfactant polyethylene glycol (PEG-6000) and add it to the solution to prepare solution A, and keep the solution at a constant temperature of 30° C.;

[0073] (2) Weighing 10 g of steel slag with an average particle size of 75 μm, stirring the solution A obtained in step (1) at a speed of 200 rpm, adding the steel slag to the solution A and stirring for 5 min to obtain steel slag slurry A;

[0074] (3) 0.5 mol / L hydrochloric acid was added dropwise to the steel slag slurry A, stirred at a speed of 200 rpm and kept warm at 50°C, and hydrochloric acid was added dropwise until the pH of the slurry was 9, and then continued to stir and keep warm for 40 minutes. Then, the mixture was filtered, washed, and dried in an oven at 80°C to obtain the modified carbon-fixing material.

[0075] Performance Testing

[0076] The modified carbon-fixing materials obtained in Examples 1 to 5 were characterized and tested as follows:

[0077] (1) Morphology and structure characterization:

[0078] Scanning electron microscopy (SEM) and X-ray diffraction (XRD) were used for characterization.

[0079] Figure 1 This is the SEM image of the uncoated steel slag in Example 1. It can be observed that at a magnification of 25,000 times, the surface of the steel slag is relatively smooth without obvious excess protrusions. Figure 2 This is the SEM image of the modified carbon-fixing material in Example 1. It can be seen that after being coated with nano-silicon dioxide, spherical nanoparticles exist on the surface of the material, and these particles are evenly dispersed on the surface of the steel slag and are tightly combined. Figure 3 This is a SEM image of silicon dioxide on the surface of the modified carbon-fixing material in Example 1. It can be seen that the particle size of the silicon dioxide particles coated on the surface of the steel slag is approximately 400-700 nm. Figure 4 The XRD diagram of the steel slag before and after coating in Example 1 confirms that the chemical composition of the material coated on the surface of the steel slag is silicon dioxide. The SEM and XRD diagrams of Examples 2 to 5 are similar to those of Example 1.

[0080] It can be seen that the chemical precipitation method of Examples 1 to 5 of the present invention can uniformly coat the surface of the steel slag with nano-silicon dioxide particles.

[0081] (2) Carbon fixation effect test:

[0082] The modified carbon-fixing materials obtained in Examples 1 to 5 were added to the culture environment of P. triangularis to test the effects of the modified materials on the growth and carbon fixation of P. triangularis. During the culture of P. triangularis, the algae solution was sampled daily, and the algae cells were counted under a microscope using a blood cell counting plate, and then the absorbance of the P. triangularis algae solution at a wavelength of λ=420nm was tested using an ultraviolet spectrophotometer at different culture times.

[0083] Figure 5 This is a comparison curve of the biomass of P. triangularis and the absorbance of the algae solution. It can be found that the biomass of the algae cells is linearly correlated with the absorbance of the algae solution at λ=420nm. Therefore, the biomass of P. triangularis can be counted by measuring the absorbance of the algae solution with an ultraviolet spectrophotometer.

[0084] The modified carbon-fixing materials of Examples 1 to 5 were added to the culture environment of P. triangularis (temperature 25°C, light 1200 lux, light: dark = 12h: 12h, static water experiment) at a solid-liquid ratio of 1g / L, and the 6-day change of biomass in the algae solution containing the materials of Examples 1 to 5 was tested. Examples 1 to 3 explored the effects of modified steel slag materials with different silicon source concentrations on the growth of algae, and Examples 2, 4, and 5 explored the effects of modified carbon-fixing materials obtained by using different insulation times in step (2) of the modification method on the growth of algae. Blank control group 1 is a control group in which P. triangularis is cultured in a set environment without adding any materials, and control group 2 is a control group in which P. triangularis is cultured after adding the original steel slag that has not been treated by the chemical precipitation method of the embodiment.

[0085] Figure 6 The figure is a graph showing the effect of Examples 1 to 3 and the control group on the biomass of P. triangularis for 7 days, wherein (A) shows the changes in the interval of 1 to 6 days, and (B) shows the changes in the interval around the 6th day. Specifically, Figure 6 (B) is Figure 6 The enlarged image of the yellow box in (A). Figure 6It can be seen that compared with the blank control group 1, the algae biomass increases of Examples 1 to 3 and the control group 2 are all increased, and the effect of Examples 1 to 3 on the algae biomass is higher than that of the control group 2.

[0086] Figure 7 The figure is the effect of Examples 2, 4, 5 and the control group on the biomass of Phaeodactylum triangularis in 7 days. Figure 7 It can be seen that the algae biomass increases in Examples 2, 4, and 5 are all increased compared to Control Group 2. The results show that steel slag extracts are beneficial to the growth and reproduction of algae, thereby achieving the effect of promoting marine carbon fixation, and the modified coating method in the embodiment of the present invention can further improve the marine carbon fixation effect of steel slag.

[0087] The modified carbon-fixing material obtained in the embodiment of the present invention is placed in an artificial seawater solution, and the remaining HCO3 in the solution is determined by hydrochloric acid titration. 2- concentration to verify the carbon fixation efficiency of the modified carbon fixation material obtained by the embodiment of the present invention in converting inorganic carbon in the environment into its own organic carbon using the marine biological pump. Figure 8 The HCO3 of Examples 1 to 3 and the control group on Phaeodactylum triangularis for 7 days 2- The results show that compared with control group 1 and control group 2, the HCO3 in Examples 1 to 3 2- The content change values ​​are all relatively high, and the carbon fixation content is all increased. It can be seen that the carbon fixation effect of the modified carbon-fixing material in the embodiment of the present invention is good.

[0088] In addition, different iron contents in steel slag have a certain influence on the carbon fixation effect, but will not affect the precipitation of iron. The precipitation of iron is related to the overall dissolution effect of steel slag. The embodiment of the present invention mainly aims at changing the precipitation process of iron in steel slag without changing the steel slag, thereby affecting the carbon fixation effect.

[0089] The modification method of steel slag in the embodiment of the present invention is simple, the raw materials are low-cost, and the various components in the steel slag can be fully utilized. It can also solve the problem that industrial waste steel slag cannot be disposed of, and achieve the effect of waste utilization. In addition, the modification method of steel slag in the embodiment of the present invention can change the leaching process of steel slag. By controlling the conditions such as silicon source concentration, reaction temperature and time, the content of silicon dioxide particles coated on the surface of steel slag can be controlled to achieve the purpose of controlling the dissolution rate of steel slag, thereby effectively utilizing the various components in steel slag. The modified carbon-fixing material provided in the embodiment of the present invention can increase the nutrient release rate of steel slag in the marine carbon sink, fully promote the growth of marine plankton such as seaweed, especially diatoms, and their photosynthetic carbon fixation process. Marine plankton sinks to the seabed after death, which can achieve the effect of fixing carbon dioxide in the ocean in the form of organic carbon and avoiding re-entering the biological carbon circulation system.

[0090] In summary, the present invention coats silica particles on the surface of steel slag, and the obtained modified carbon-fixing material has a moderate dissolution rate, especially the release rate of iron element is controllable, so that the iron element in the steel slag is effectively utilized, the utilization rate of each component in the steel slag is high, and the dissolution of the material is beneficial to the growth and reproduction of marine plankton, and is beneficial to promoting its photosynthesis to achieve the effect of carbon fixation. The modified carbon-fixing material of the present invention has a wide range of applications in fixing carbon dioxide, especially fixing carbon dioxide in the marine environment.

Claims

1. A modified carbon-fixing material, characterized in that: The invention comprises steel slag and silicon dioxide particles, wherein the silicon dioxide particles are coated on the surface of the steel slag.

2. The modified carbon-fixing material according to claim 1, characterized in that: The average particle size of the silicon dioxide particles is 100 to 1000 nm; And / or, the average particle size of the steel slag is 50 to 400 μm.

3. The modified carbon-fixing material according to claim 1, characterized in that: The iron content in the steel slag is 15-40wt%.

4. The modified carbon-fixing material according to claim 1, characterized in that: The components of the steel slag include at least one of CaO, FeO, SiO2, Al2O3, MgO and P2O3.

5. A method for preparing a modified carbon-fixing material according to any one of claims 1 to 4, characterized in that: The following steps are involved: The mixed solution containing silicon source, surfactant, water and steel slag is subjected to precipitation reaction with acid to obtain the modified carbon-fixing material.

6. The preparation method according to claim 5, characterized in that: The silicon source includes at least one of sodium silicate, potassium silicate or sodium metasilicate; and / or, the surfactant comprises at least one of polyethylene glycol, poloxamer or Tween; And / or, the acid includes at least one of hydrochloric acid, sulfuric acid or nitric acid.

7. The preparation method according to claim 5, characterized in that: In the mixed solution, the molar concentration of the silicon source is 0.01 to 1 mol / L; And / or, the mass ratio of the silicon source to the surfactant is (10-100):1; and / or, the mass ratio of the surfactant to the steel slag is 1:(80-120); And / or, the concentration of the acid is 0.1-3 mol / L.

8. The preparation method according to claim 5, characterized in that: The pH value of the precipitation reaction is 7 to 10; And / or, the temperature of the precipitation reaction is 30 to 100° C.; And / or, the precipitation reaction time is 5 to 200 minutes.

9. Use of the modified carbon-fixing material according to any one of claims 1 to 4 for fixing carbon dioxide in a marine environment.

10. The use according to claim 9, characterized in that: The modified carbon-fixing material fixes carbon dioxide by promoting photosynthesis of marine plankton.

Citation Information

Cited By

  • Iron-rich slag derivative additive as well as preparation method and application thereof

    CN120172667A

  • An iron-rich slag-derived additive and its preparation method and application

    CN120172667B