Efficient demercuration adsorbent as well as preparation method and application thereof

By adopting a core-shell structure, the high-efficiency demercury adsorbent is used to utilize magnetic particles containing iron oxide and carbon layers containing chlorine, the problems of low efficiency and poor environmental protection performance of biochar adsorbents are solved, and the efficient removal of flue gas and Mercury in wastewater has good magnetic desorption performance and recycling ability.

CN119016020APending Publication Date: 2024-11-26SANHE POWER GENERATION +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411222721.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing biochar demercury adsorbent has low adsorption efficiency and is difficult to separate after mixing with fly ash, resulting in poor environmental protection performance and difficult to effectively remove elemental mercury from flue gas.

Method used

The high-efficiency demercury adsorbent adopts a core-shell structure. The core is a magnetic particle containing iron oxide, and the outer shell is a carbon layer containing chlorine. It is formed by temperature-controlled pyrolysis and magnetic field treatment to improve adsorption and desorption performance.

Benefits of technology

It significantly improves the removal efficiency of mercury in flue gas and sewage, enhances the magnetic desorption performance of adsorbents, promotes its recycling and recycling, and the raw materials are waste, which is green and environmentally friendly, economical and practical.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016020A_ABST
    Figure CN119016020A_ABST
Patent Text Reader

Abstract

The invention relates to an efficient demercuration adsorbent as well as a preparation method and application thereof. The adsorbent has a core-shell structure, and the core-shell structure comprises a core and a shell layer coating the outer surface of the core; the core comprises magnetic particles, and the magnetic particles contain iron oxide; the shell layer comprises a carbon layer, and the carbon layer contains a chlorine element. The adsorbent is relatively high in adsorption efficiency, and raw materials for preparing the adsorbent are green, environment-friendly, economical and practical.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the technical field of mercury adsorbents, and in particular, to a high-efficiency mercury removal adsorbent and a preparation method and application thereof. Background Art

[0002] Mercury emissions not only seriously harm the ecological environment, but also endanger human health through the ecological cycle. Therefore, the objective demand for strict prevention and control of mercury emissions in social production is increasing. At present, coal combustion in thermal power plants is one of the main sources of man-made mercury pollution. Among them, the mercury in the combustion flue gas is mainly in the form of elemental mercury (Hg 0 ), ionic mercury (Hg 2+ ) and particulate mercury (Hg p ) exists in three forms. 2+ Soluble in water, it can be removed by wet desulfurization device at the end of combustion system. p It can be removed by electrostatic trapping equipment. 0 Due to its insoluble in water, volatile, and stable chemical properties, it is difficult to remove through the above methods, thus becoming the focus of current flue gas mercury removal research. At the same time, it is worth noting that Hg dissolved in water after wet desulfurization equipment 2+ If not treated, it is still possible to enter the ecosystem through the sewage discharge pathway, causing secondary pollution. Therefore, in coal-fired power plants, the main pressure for mercury removal is concentrated on flue gas mercury removal and wastewater mercury removal.

[0003] Biochar is considered to have the potential to be used as a carrier in the field of mercury removal due to its high specific surface area and rich functional groups. However, biochar mercury removal adsorbents still face many problems, mainly including: 1) the pore structure of pure biochar itself is still not superior to that of activated carbon, and further activation is required, and the adsorption efficiency is low; 2) mercury-enriched biochar particles are difficult to separate after mixing with fly ash, which will lead to a decrease in the quality of fly ash and limited utilization. There is still a risk of mercury re-emission during the recycling process of fly ash, and the environmental performance is poor. Summary of the invention

[0004] In order to solve the problems existing in the prior art, the present invention provides a high-efficiency mercury removal adsorbent and a preparation method and application thereof. The adsorption efficiency of the adsorbent is high, and the raw materials for preparing the adsorbent are green, environmentally friendly, economical and practical.

[0005] In order to achieve the above-mentioned object, the first aspect of the present disclosure provides a high-efficiency mercury removal adsorbent, which has a core-shell structure, wherein the core-shell structure includes a core and an outer shell layer coated on the outer surface of the core; the core includes magnetic particles, and the magnetic particles contain iron oxide; the outer shell layer includes a carbon layer, and the carbon layer contains chlorine.

[0006] Optionally, in the core, the content of the iron oxide is 40-60 wt % based on the total weight of the magnetic particles.

[0007] Optionally, based on the total weight of the adsorbent, the content of the carbon layer is 50-70wt%; based on the total weight of the carbon layer, the content of the chlorine element is 0.5-1.0wt%.

[0008] Optionally, the average particle size of the adsorbent is 75-150 μm; the saturation magnetization intensity of the adsorbent is 30-50 emu / g.

[0009] The second aspect of the present disclosure provides a method for preparing a highly efficient mercury removal adsorbent, the method comprising the following steps: S1, mixing magnetic particles, a carbon source and a chlorine source and then subjecting the mixture to ball milling to obtain a first material; S2, subjecting the first material to a first heating treatment, a first pyrolysis treatment and a first cooling treatment in a tube furnace to obtain a second material; during the first heating treatment and the first pyrolysis treatment, introducing an inert atmosphere into the tube furnace; S3, subjecting the second material to a second heating treatment, a second pyrolysis treatment, and a second cooling treatment in a tube furnace to obtain a third material; during the second pyrolysis treatment, introducing water vapor into the tube furnace; S4, subjecting the third material to a drying treatment and a magnetic field adsorption treatment to obtain the adsorbent.

[0010] Optionally, in step S1, the weight ratio of the magnetic particles, carbon source and chlorine source is (1-2): (1-3): 1; the magnetic particles contain iron oxide, and the content of the iron oxide is 40-60wt% based on the total weight of the magnetic particles; the carbon source is rubber; and the chlorine source is polyvinyl chloride.

[0011] Optionally, in step S1, the conditions of the ball milling treatment include: a rotation speed of 800-1000r / min, and a time of 0.5-1.5h; in step S2, the heating rate of the first temperature heating treatment is 5-20℃ / min; the conditions of the first pyrolysis treatment include: a temperature of 400-550℃, and a time of 0.5-2.0h; the flow rate of the inert atmosphere is greater than 100mL / min, and the inert atmosphere is selected from nitrogen and / or argon; in step S3, the heating rate of the second temperature heating treatment is 5-20℃ / min; the conditions of the second pyrolysis treatment include: a temperature of 600-900℃, and a time of 1-2h; the flow rate of the water vapor is greater than 30mL / min; in step S4, the conditions of the drying treatment include: a temperature of 80-110℃, and a time of 6-12h; the magnetic field strength of the magnetic field adsorption treatment is 4000-8000A / m.

[0012] Optionally, the method further comprises: before step S1, the magnetic particles, the carbon source and the chlorine source are each independently subjected to crushing and screening treatment; the mesh size of the crushing and screening treatment is 100-200 meshes.

[0013] A third aspect of the present disclosure provides a high-efficiency mercury removal adsorbent prepared by the method described in the second aspect.

[0014] A fourth aspect of the present disclosure provides use of the adsorbent described in the first aspect or the third aspect in the treatment of mercury-containing flue gas and exhaust gas and / or mercury-containing wastewater.

[0015] Through the above technical scheme, the present disclosure provides a highly efficient mercury removal adsorbent and its preparation method and application. The present disclosure forms a core-shell structure with magnetic particles containing iron oxide as the core and a carbon layer as the shell by pyrolyzing the raw materials, wherein the carbon layer contains chlorine elements, which can significantly improve the mercury removal efficiency of the adsorbent for mercury-containing flue gas and / or mercury-containing wastewater. In addition, the adsorbent has magnetism, which can not only improve the adsorption performance of the adsorbent, but also make the adsorbent have better magnetic desorption performance, which is conducive to the regeneration and recycling of the adsorbent. The raw materials used in the present disclosure are all waste, which is green, environmentally friendly, economical and practical.

[0016] Other features and advantages of the present disclosure will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] The accompanying drawings are used to provide a further understanding of the present disclosure and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present disclosure but do not constitute a limitation of the present disclosure. In the accompanying drawings: Figure 1 is a flow chart of the preparation of the adsorbent disclosed in the present invention. DETAILED DESCRIPTION

[0018] The specific implementation of the present disclosure is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described herein is only used to illustrate and explain the present disclosure, and is not used to limit the present disclosure.

[0019] The first aspect of the present disclosure provides a highly efficient mercury removal adsorbent, the adsorbent having a core-shell structure, the core-shell structure comprising a core and an outer shell layer coated on the outer surface of the core; The core includes magnetic particles, and the magnetic particles contain iron oxide; The outer shell layer includes a carbon layer, and the carbon layer contains chlorine element.

[0020] The adsorbent disclosed in the present invention has magnetic particles containing iron oxide as the core of the adsorbent particles, which gives the adsorbent high magnetic properties. When used for the treatment of mercury-containing flue gas and / or mercury-containing wastewater, the catalyst not only has good adsorption performance, but also has good magnetic desorption performance, which is conducive to the regeneration and recycling of the adsorbent. The adsorbent has a carbon layer containing chlorine as the outer shell of the adsorbent particles. Specifically, the outer shell is a protective shell formed by an aromatic compound, and the carbon element therein is connected to the chlorine element; in addition, the strong chemical interaction between the chlorine element and mercury improves the demercuration efficiency of the adsorbent for mercury-containing flue gas and / or mercury-containing wastewater.

[0021] According to the present disclosure, the content of iron oxide can vary within a wide range. In one embodiment of the present disclosure, in the core, the content of iron oxide is 40-60wt% based on the total weight of the magnetic particles. When the content of iron oxide is within the range of the above embodiment, the adsorption and desorption properties of the adsorbent can be further improved, which is beneficial to the regeneration and recycling of the adsorbent particles.

[0022] According to the present disclosure, the content of the carbon layer and the chlorine element can vary within a wide range. In one embodiment of the present disclosure, based on the total weight of the adsorbent, the content of the carbon layer is 50-70wt%; based on the total weight of the carbon layer, the content of the chlorine element is 0.5-1.0wt%. In the above embodiment, the chlorine element is loaded on the carbon layer through the "C-Cl" bond between the chlorine element and the carbon, so that the adsorbent has a higher mercury removal efficiency when treating mercury-containing flue gas and / or mercury-containing wastewater.

[0023] According to the present disclosure, the average particle size of the adsorbent may vary within a wide range. For example, the average particle size of the adsorbent may be 75-150 μm.

[0024] According to the present disclosure, the saturation magnetization of the adsorbent can vary within a wide range. For example, the saturation magnetization of the adsorbent can be 30-50 emu / g.

[0025] The second aspect of the present disclosure provides a method for preparing a highly efficient mercury removal adsorbent, the method comprising the following steps: S1, mixing magnetic particles, a carbon source and a chlorine source and then subjecting the mixture to ball milling to obtain a first material; S2, subjecting the first material to a first heating treatment, a first pyrolysis treatment and a first cooling treatment in a tube furnace to obtain a second material; during the first heating treatment and the first pyrolysis treatment, introducing an inert atmosphere into the tube furnace; S3, subjecting the second material to a second heating treatment, a second pyrolysis treatment, and a second cooling treatment in a tube furnace to obtain a third material; during the second pyrolysis treatment, introducing water vapor into the tube furnace; S4, subjecting the third material to a drying treatment and a magnetic field adsorption treatment to obtain the adsorbent.

[0026] The present invention adopts temperature-controlled pyrolysis treatment of magnetic particles, carbon sources and chlorine sources, so that volatile organic carbon from the carbon source can adhere to the magnetic particles, forming a carbon layer that can wrap the magnetic particles, and can also load the chlorine element in the chlorine source on the carbon layer through chemical bonds. The prepared adsorbent particles have a core-shell structure, and the core is a magnetic particle containing iron oxide, which gives the adsorbent a higher magnetic property. When used for mercury-containing flue gas exhaust treatment and / or mercury-containing sewage treatment, the catalyst not only has good adsorption performance, but also has good magnetic desorption performance, which is conducive to the regeneration and recycling of the adsorbent. The outer shell is a carbon layer containing chlorine elements. The strong chemical interaction between chlorine elements and mercury improves the demercurization efficiency of the adsorbent for mercury-containing flue gas exhaust and / or mercury-containing sewage. Furthermore, the magnetic particles, carbon sources and chlorine sources used in the present invention are all wastes, which are green, environmentally friendly, economical and practical.

[0027] According to the present disclosure, the weight ratio of the magnetic particles, the carbon source and the chlorine source can vary within a wide range. In one embodiment, the weight ratio of the magnetic particles, the carbon source and the chlorine source is (1-2): (1-3): 1. The magnetic particles contain iron oxide, and the content of the iron oxide is 40-60wt% based on the total weight of the magnetic particles.

[0028] In the present disclosure, the magnetic particles can be magnetic particles formed by the enrichment of iron in the process of coal combustion. The carbon source is rubber; specifically, the rubber can be rubber products such as waste tires. The chlorine source is polyvinyl chloride; specifically, polyvinyl chloride can be waste plastic products, etc. The magnetic particles, carbon source and chlorine source used in the present disclosure are all wastes, which are green, environmentally friendly, economical and practical.

[0029] In one embodiment of the present disclosure, in step S1, the conditions of the ball milling treatment include: a rotation speed of 800-1000 r / min and a time of 0.5-1.5 h. The ball milling treatment can be performed using a ball milling device conventionally used by those skilled in the art, which will not be described in detail here.

[0030] In one embodiment of the present disclosure, in step S2, the heating rate of the first heating treatment is 5-20°C / min; the conditions of the first pyrolysis treatment include: temperature of 400-550°C, time of 0.5-2.0h; the flow rate of the inert atmosphere is greater than 100mL / min, and the inert atmosphere is selected from nitrogen and / or argon.

[0031] In one embodiment of the present disclosure, in step S3, the heating rate of the second heating treatment is 5-20°C / min; the conditions of the second pyrolysis treatment include: temperature of 600-900°C, time of 1-2h; wherein, water vapor is present during the second heating treatment, and the flow rate of the water vapor is greater than 30mL / min; the specific surface area of ​​the adsorbent can be further increased, thereby improving the adsorption performance of the adsorbent.

[0032] In one embodiment of the present disclosure, in step S4, the drying conditions include: a temperature of 80-110° C. and a time of 6-12 hours. The drying process may be performed using a drying machine commonly used by those skilled in the art.

[0033] In one embodiment of the present disclosure, the magnetic field strength of the magnetic field adsorption treatment may be 4000-8000 A / m.

[0034] According to the present disclosure, the method further includes: before step S1, the magnetic particles, the carbon source and the chlorine source are crushed and screened independently. The crushing and screening process can be performed using a crushing and screening integrated machine conventionally used by those skilled in the art. In the present disclosure, the crushing and screening process has a mesh size of 100-200 meshes.

[0035] A third aspect of the present disclosure provides a high-efficiency mercury removal adsorbent prepared by the method described in the second aspect.

[0036] A fourth aspect of the present disclosure provides use of the adsorbent described in the first aspect or the third aspect in the treatment of mercury-containing flue gas and exhaust gas and / or mercury-containing wastewater.

[0037] In the present disclosure, 30-100 mg of adsorbent is taken to the flue gas containing mercury in the reactor, the mercury generation temperature is set to 40-70°C, and simulated flue gas is introduced into the reactor at a flow rate of 500-1500L / min, gaseous mercury is captured at 90-200°C, the mercury concentration in the flue gas containing mercury or mercury-containing wastewater before and after adsorption is recorded, and the mercury removal efficiency is calculated.

[0038] The present invention is further illustrated by the following examples, but the present invention is not limited thereto.

[0039] Example 1 The rubber, polyvinyl chloride and magnetic particles in the waste gas are crushed and screened by a crushing and screening machine, and the screening mesh is 200 mesh. Among them, the magnetic particles contain 50wt% iron oxide.

[0040] The magnetic particles, the carbon source and the chlorine source were mixed in a weight ratio of 1:1:1, put into a ball mill and subjected to ball milling treatment at a rotation speed of 900 r / min for 1.5 hours to obtain a first material.

[0041] The first material is placed in a tubular furnace, nitrogen is introduced at a flow rate of 200 mL / min, the temperature is raised from room temperature to 550°C at a rate of 20°C / min, and a first pyrolysis treatment is performed at 550°C for 2.0 h; the temperature is then lowered to room temperature to obtain a second material.

[0042] The second material is heated from room temperature to 800°C at a rate of 10°C / min in a tubular furnace, and then water vapor is introduced at a flow rate of 30 mL / min, and a second pyrolysis treatment is performed at 800°C for 1 hour; the temperature is cooled to room temperature to obtain a third material.

[0043] The third material was dried at 90° C. for 12 h, and then the obtained sample was subjected to a magnetic field strength of 6000 A / m to select magnetic adsorbent particles, which were recorded as S-1.

[0044] Example 2 The rubber, polyvinyl chloride and magnetic particles in the waste gas are crushed and screened by a crushing and screening machine, and the screening mesh is 100 mesh. Among them, the magnetic particles contain 50wt% iron oxide.

[0045] The magnetic particles, the carbon source and the chlorine source were mixed in a weight ratio of 1:1:1, put into a ball mill and subjected to ball milling treatment at a rotation speed of 800 r / min for 1 hour to obtain a first material.

[0046] The first material is placed in a tube furnace, nitrogen is introduced at a flow rate of 200 mL / min, the temperature is raised from room temperature to 450°C at a rate of 20°C / min, and a first pyrolysis treatment is performed at 450°C for 1 hour; the temperature is then lowered to room temperature to obtain a second material.

[0047] The second material is heated from room temperature to 700°C at a rate of 10°C / min in a tubular furnace, and then water vapor is introduced at a flow rate of 30 mL / min, and a second pyrolysis treatment is performed at 700°C for 2 hours; the temperature is cooled to room temperature to obtain a third material.

[0048] The third material was dried at 80° C. for 24 hours, and then the obtained sample was subjected to a magnetic field strength of 4000 A / m to select magnetic adsorbent particles, which were recorded as S-2.

[0049] Test Example 1 50 mg of the adsorbents in Examples 1-2 were respectively taken and placed in a fixed bed reactor for flue gas mercury removal experiments. The mercury concentration in the flue gas before adsorption was 85 μg / m 3The mercury generation temperature was set at 58°C, and flue gas was introduced into the fixed bed reactor at a flow rate of 1000L / min. Gaseous mercury was captured at 150°C. The mercury concentration in the flue gas after adsorption was 0-4μg / m 3 .

[0050] The calculation method of mercury removal efficiency is: mercury removal efficiency = (mercury concentration in flue gas before adsorption - mercury concentration in flue gas after adsorption) / mercury concentration in flue gas before adsorption × 100%.

[0051] The mercury removal efficiency is reported in Table 1.

[0052] Table 1

[0053] It can be seen from the above data that the adsorbent disclosed in the present invention has a high mercury removal efficiency.

[0054] The preferred embodiments of the present disclosure are described in detail above in conjunction with the accompanying drawings; however, the present disclosure is not limited to the specific details in the above embodiments. Within the technical concept of the present disclosure, a variety of simple modifications can be made to the technical solution of the present disclosure, and these simple modifications all fall within the protection scope of the present disclosure.

[0055] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present disclosure will not further describe various possible combinations.

[0056] In addition, various embodiments of the present disclosure may be arbitrarily combined, and as long as they do not violate the concept of the present disclosure, they should also be regarded as the contents disclosed by the present disclosure.

Claims

1. A highly efficient mercury removal adsorbent, characterized in that: The adsorbent has a core-shell structure, which includes a core and a shell layer covering the outer surface of the core; The core includes magnetic particles, and the magnetic particles contain iron oxide; The outer shell layer includes a carbon layer, and the carbon layer contains chlorine element.

2. The adsorbent according to claim 1, wherein In the core, the content of the iron oxide is 40-60 wt % based on the total weight of the magnetic particles.

3. The adsorbent according to claim 1, wherein Based on the total weight of the adsorbent, the content of the carbon layer is 50-70wt%; Based on the total weight of the carbon layer, the content of the chlorine element is 0.5-1.0wt%.

4. The adsorbent according to claim 1, wherein The average particle size of the adsorbent is 75-150 μm; The adsorbent has a saturation magnetization intensity of 30-50emu / g.

5. A method for preparing an efficient mercury removal adsorbent, characterized in that: The method comprises the following steps: S1, mixing magnetic particles, a carbon source and a chlorine source and then subjecting the mixture to ball milling to obtain a first material; S2, subjecting the first material to a first heating treatment, a first pyrolysis treatment and a first cooling treatment in a tube furnace to obtain a second material; during the first heating treatment and the first pyrolysis treatment, introducing an inert atmosphere into the tube furnace; S3, subjecting the second material to a second heating treatment, a second pyrolysis treatment, and a second cooling treatment in a tube furnace to obtain a third material; during the second pyrolysis treatment, introducing water vapor into the tube furnace; S4, subjecting the third material to a drying treatment and a magnetic field adsorption treatment to obtain the adsorbent.

6. The method according to claim 5, wherein: In step S1, the weight ratio of the magnetic particles, the carbon source and the chlorine source is (1-2): (1-3): 1; The magnetic particles contain iron oxide, and the content of the iron oxide is 40-60wt% based on the total weight of the magnetic particles; The carbon source is rubber; the chlorine source is polyvinyl chloride.

7. The method according to claim 5, wherein: In step S1, the conditions of the ball milling treatment include: a rotation speed of 800-1000 r / min and a time of 0.5-1.5 h; In step S2, the heating rate of the first heating treatment is 5-20°C / min; the conditions of the first pyrolysis treatment include: temperature of 400-550°C, time of 0.5-2.0h; the flow rate of the inert atmosphere is greater than 100mL / min, and the inert atmosphere is selected from nitrogen and / or argon; In step S3, the heating rate of the second heating treatment is 5-20°C / min; the conditions of the second pyrolysis treatment include: temperature of 600-900°C, time of 1-2h; the flow rate of the water vapor is greater than 30mL / min; In step S4, the drying conditions include: temperature of 80-110°C and time of 6-12h; The magnetic field intensity of the magnetic field adsorption treatment is 4000-8000A / m.

8. The method according to claim 5, wherein: The method further comprises: before step S1, the magnetic particles, the carbon source and the chlorine source are subjected to crushing and screening treatments independently; The mesh size of the crushing and screening process is 100-200 meshes.

9. A highly efficient mercury removal adsorbent prepared by the method according to any one of claims 5 to 8.

10. Use of the adsorbent according to any one of claims 1 to 4 or claim 9 in the treatment of flue gas and tail gas containing mercury and / or the treatment of wastewater containing mercury.

Citation Information

Patent Citations

  • Method for preparing mercury removal agent by utilizing modified waste tire pyrolysis residue

    CN102580674A

  • Nanometer magnetic compound iron copper oxide dearsenization adsorbing agent and preparation method and application thereof

    CN110280213A

  • Modified carbon-based / non-carbon-based mercury removal adsorbent and preparation method thereof

    CN111604031A

  • Biochar adsorbent prepared from wastes and used for mercury removal and preparation method thereof

    CN112705162A

  • Porous carbon coated ferroferric oxide nanoparticles and solid-phase preparation method thereof

    CN114275824A