Sulfydryl modified MXene adsorbent for recycling silver electrolysis waste liquid as well as preparation method and application of sulfydryl modified MXene adsorbent
Through the preparation of thiol-modified MXene adsorbent, the problem of low recycling efficiency of the electrolytic waste liquid in the prior art was solved, and efficient recycling of silver ions and silver particles was achieved, significantly improving the silver recovery rate and reducing precious metal waste.
Patent Information
- Application Number
- CN202411228550.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-26
AI Technical Summary
In the existing silver electrolytic waste liquid recycling method, the reaction rate slows down when the reactant concentration is low, resulting in difficulty in enriching and recycling of metal silver particles, resulting in waste of precious metals. The common materials have low specific surface area and poor adsorption activity, making it difficult to efficiently recover silver ions. .
The thiol-modified MXene adsorbent is used to mix low-priced titanium-containing minerals with aluminum powder and titanium powder by hydrogen-rich reduction to form a carbon nitride ceramic precursor with aluminum intercalation, and then react with an interface inducer to prepare low-dimensional MXene, and The thiol modification is carried out in the acetic acid solution to form an adsorbent with high hydrophilicity and selective adsorption properties, which is used for silver recovery in acidic electrolytic waste liquid.
It has achieved efficient and selective adsorption of silver ions and silver particles, with a recovery rate of 98% to 99%, effectively reducing the waste of precious metals and improving the silver recycling efficiency.
Smart Images

Figure CN119016029A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of silver electrolysis waste liquid recovery, and specifically relates to a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid, and a preparation method and application thereof. Background Art
[0002] As one of the transition metals, silver has relatively stable physical and chemical properties, good thermal and electrical conductivity, is soft, ductile, and has extremely high reflectivity.
[0003] During the silver smelting process, the silver electrolytic waste liquid produced contains a large amount of silver. However, the chemical reaction rates of the commonly used methods for recovering silver, such as copper replacement and sodium hydroxide neutralization, are affected by the concentration of reactants. When the concentration of reactants in the solution is as low as a certain value, the reaction rate will approach zero, and the produced silver particles will be extremely small, making them difficult to enrich and recover, resulting in a huge waste of precious metals.
[0004] MXene is a typical two-dimensional quasi-layered structure compound, including transition metal carbides, nitrides, carbonitrides with large specific surface areas, and abundant oxygen-containing functional groups such as carboxyl and hydroxyl groups. MXene has good hydrophilicity, compatibility, stability and dispersibility, can form a uniform dispersion in a solvent, and has a good adsorption effect on heavy metal ions, but it is rarely used in the field of silver metal ion recovery.
[0005] Moreover, the activated carbon materials commonly used in the field of silver metal ion recovery also have typical defects such as low specific surface area, poor adsorption activity, and underdeveloped nanostructure. Therefore, there is an urgent need for an efficient and highly adsorbable silver recovery adsorption material. Summary of the invention
[0006] In view of this, some embodiments disclose a method for preparing a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid, comprising the steps of:
[0007] S1, reducing a low-valent titanium-containing mineral to obtain a carbonitride composite precursor;
[0008] S2, mixing the carbonitride composite precursor with aluminum powder and titanium powder according to a set ratio, and sintering without pressure in an inert atmosphere to obtain a carbonitride ceramic precursor with an aluminum intercalation layer;
[0009] S3, reacting a carbonitride ceramic precursor having an aluminum intercalation layer with an interface inducing agent, wherein the aluminum intercalation layer in the carbonitride ceramic precursor is ionized and released, and the titanium and vanadium sites form oxygen-containing end grains to obtain a low-dimensional MXene;
[0010] S4. Evenly disperse the low-dimensional MXene in an acetic acid solution, add 1,3-mercaptopropyltrimethoxysilane, and control the pH value at 6.5 to 8 to obtain a mixed suspension; add glutaraldehyde to the mixed suspension, and react at low temperature for 18 to 30 hours to obtain a thiol-modified MXene adsorbent.
[0011] Some embodiments disclose a method for preparing a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid, wherein the low-valent titanium-containing minerals include one or more of vanadium-titanium magnetite, titanium concentrate, titanium dioxide, and waste denitrification catalysts.
[0012] Some embodiments disclose a method for preparing a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid. In step S1, the hydrogen-rich reducing atmosphere is composed of hydrogen and one or more of methane, ammonia, and nitrogen, wherein the volume content of hydrogen is 80 to 98%; the temperature of the hydrogen-rich reduction is 1200 to 1500°C, and the time is 2 to 10 hours.
[0013] Some embodiments disclose a method for preparing a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid, wherein the molar ratio of the carbonitride composite precursor, the aluminum powder, and the titanium powder is 2:1 to 2:1 to 2.
[0014] Some embodiments disclose a method for preparing a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid, wherein the interfacial inducer is hydrofluoric acid, a hydrogen chloride-lithium chloride mixed solution, or a lithium hydroxide solution.
[0015] Some embodiments disclose a method for preparing a mercapto-modified MXene adsorbent for recovering silver electrolysis waste liquid, wherein the volume ratio of 1,3-mercaptopropyltrimethoxysilane to acetic acid is 5:4.
[0016] Some embodiments disclose a method for preparing a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid, wherein the solid-liquid ratio in the mixed suspension is 1:1-2.
[0017] In some embodiments, the method for preparing a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid is disclosed, wherein the volume ratio of glutaraldehyde to the mixed suspension is 1:5-6.
[0018] Some embodiments disclose a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid, which is prepared by the above preparation method.
[0019] Some embodiments disclose an application of a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid, wherein the thiol-modified MXene adsorbent is used to enrich silver in the silver electrolysis waste liquid.
[0020] The preparation method of the thiol-modified MXene adsorbent for recovering silver electrolytic waste liquid disclosed in the embodiment of the present invention is to first reduce and carbonize the low-valent titanium-containing mineral in a hydrogen-rich reduction system, and then mix and control it with aluminum powder and titanium powder to prepare a carbonitride ceramic precursor with an aluminum intercalation layer, and then introduce an interface inducer to react with it to prepare a low-dimensional MXene material, and then use a solvent thermal reaction to perform thiol modification in an acetic acid solution, while retaining hydrophilicity, while enhancing the selectivity for silver, which is suitable for efficient recovery of silver in acidic electrolytic waste liquid. The thiol-modified MXene adsorbent for recovering silver electrolytic waste liquid disclosed in the embodiment of the present invention has hydrophilicity and selective adsorption, and can efficiently and selectively adsorb silver ions and silver particles. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 SEM results of carbonitride composite precursor in Example 1;
[0022] Figure 2 XPS result diagram of thiol-modified MXene adsorbent in Example 2. DETAILED DESCRIPTION
[0023] The word "embodiment" used here as an "exemplary" does not necessarily mean that any embodiment described is superior to or better than other embodiments. Unless otherwise specified, the performance index tests in the embodiments of this application are performed using conventional test methods in the art. It should be understood that the terms described in this application are only used to describe specific implementation methods and are not used to limit the content disclosed in this application.
[0024] Unless otherwise specified, the technical and scientific terms used in this document have the same meanings as commonly understood by ordinary technicians in the technical field to which this application belongs; other experimental methods and technical means not specifically specified in this application refer to experimental methods and technical means commonly used by ordinary technicians in this field.
[0025] The terms "substantially" and "approximately" used herein are used to describe small fluctuations. For example, they can refer to less than or equal to ±5%, such as less than or equal to ±2%, such as less than or equal to ±1%, such as less than or equal to ±0.5%, such as less than or equal to ±0.2%, such as less than or equal to ±0.1%, such as less than or equal to ±0.05%. The numerical data represented or presented in the range format herein are used only for convenience and brevity, and should therefore be flexibly interpreted as including not only the values clearly listed as the limits of the range, but also all independent values or sub-ranges contained in the range. For example, the numerical range of "1-5%" should be interpreted as including not only the clearly listed values of 1% to 5%, but also the independent values and sub-ranges within the range shown. Therefore, independent values such as 2%, 3.5% and 4% and sub-ranges such as 1%-3%, 2%-4% and 3%-5% are included in this numerical range. This principle also applies to the range of only one numerical value. In addition, such an interpretation applies regardless of the width of the range or the characteristics described.
[0026] In this document, including in the claims, transitional words such as "comprises," "includes," "with," "having," "containing," "involving," "accommodating," etc. are understood to be open-ended, i.e., meaning "including but not limited to." Only the transitional words "consisting of" and "composed of" are closed transitional words.
[0027] In order to better illustrate the content of the present application, numerous specific details are provided in the specific examples below. It should be understood by those skilled in the art that the present application can also be implemented without certain specific details. In the embodiments, some methods, means, instruments, equipment, etc. well known to those skilled in the art are not described in detail in order to highlight the main purpose of the present application.
[0028] Under the premise of no conflict, the technical features disclosed in the embodiments of the present application can be arbitrarily combined, and the obtained technical solutions belong to the contents disclosed in the embodiments of the present application. It should be noted that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like mentioned in the present application indicate the orientation or position relationship based on the orientation or position relationship shown in the accompanying drawings, which is only for the convenience of describing the technical features and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation of the present invention, unless it conflicts with the context. The term "solid-to-liquid ratio" mentioned in the present application refers to the ratio of the mass of the solid material to the volume of the treated liquid. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance, unless it conflicts with the context.
[0029] In some embodiments, the method for preparing a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid comprises the steps of:
[0030] S1. The low-valent titanium-containing mineral is subjected to hydrogen-rich reduction to obtain a carbonitride composite precursor. The metal oxide is rapidly deoxidized under the action of atomic-level H, C, and N. In addition, the H2O and CO generated by the gas-solid reaction under the multiple effects of flow field and self-diffusion can be quickly taken away from the particle surface, further promoting the reaction. One or more processes of carburization and nitriding of low-valent oxides or metal surfaces occur, thereby promoting the formation of a carbonitride composite precursor.
[0031] S2, grinding the carbonitride composite precursor, and mixing it with aluminum powder and titanium powder in a set ratio, and sintering it without pressure in an inert atmosphere to obtain a carbonitride ceramic precursor with aluminum intercalation. Under high temperature conditions, aluminum exists in liquid form, which adheres different particles, thereby promoting the solid-solid-liquid diffusion process at high temperature. At the same time, at high temperature, carbides will decompose in small amounts to produce non-stoichiometric compounds or metals, which react rapidly under the support of liquid aluminum to form a layered ceramic with a sandwich structure;
[0032] S3. A carbonitride ceramic precursor with an aluminum intercalation layer is reacted with an interfacial inducer, and the aluminum intercalation layer in the carbonitride ceramic precursor is ionized and released, and oxygen-containing end grains are formed at the titanium and vanadium sites to obtain a low-dimensional MXene; the aluminum intercalation layer with high reactivity in the carbonitride ceramic precursor undergoes affinity reaction with the interfacial inducer at the solid-liquid interface and is released in the form of ions, and the titanium and vanadium sites with oxygen-affinity characteristics in the carbonitride ceramic precursor are in situ anchored to form oxygen-containing end grains such as carboxyl and hydroxyl groups. Due to the difference in reactivity, the more active and amphoteric metal aluminum is very easy to react with strong acids or strong bases, while the carbonitride ceramic has good stability under such conditions, thereby causing aluminum to lose electrons and dissolve into the solution in an ionic state, promoting the production of low-dimensional structures, and the atomic activity of titanium and vanadium on the particle surface is second only to aluminum, and will slowly undergo oxidation affinity with the medium, promoting the introduction of oxygen-containing end grains such as surface carboxyl and hydroxyl groups;
[0033] S4, evenly disperse the low-dimensional MXene in the acetic acid solution, add 1,3-mercaptopropyltrimethoxysilane, control the pH at 6.5-8, and obtain a mixed suspension; add glutaraldehyde to the mixed suspension, react at low temperature for 18-30 hours, and obtain a thiol-modified MXene adsorbent. Generally, the reaction temperature is below 5°C. The surface functional groups of nanomaterials have good processability and design ability, which also gives the potential for directional design of low-dimensional MXene functional groups. Under this condition, the oxygen-containing functional groups such as carboxyl and hydroxyl of the original low-dimensional MXene will gradually be replaced by thiol chelation to form a thiol-modified MXene adsorbent.
[0034] In some embodiments, the low-valent titanium-containing mineral includes one or more of vanadium-titanium magnetite, titanium concentrate, titanium dioxide, and spent denitrification catalyst.
[0035] In some embodiments, in step S1, the hydrogen-rich reducing atmosphere is composed of hydrogen and one or more of methane, ammonia, and nitrogen, wherein the volume content of hydrogen is 80-98%; the temperature of hydrogen-rich reduction is 1200-1500° C., and the time is 2-10 h.
[0036] In some embodiments, the molar ratio of the carbonitride composite precursor, the aluminum powder, and the titanium powder is 2:1 to 2:1 to 2.
[0037] In some embodiments, the interface inducing agent is hydrofluoric acid, a hydrogen chloride-lithium chloride mixed solution or a lithium hydroxide solution.
[0038] In some embodiments, the volume ratio of 1,3-mercaptopropyltrimethoxysilane to acetic acid is 5:4.
[0039] In some embodiments, the solid-liquid ratio in the mixed suspension is 1:1-2.
[0040] In some embodiments, the volume ratio of glutaraldehyde to the mixed suspension is 1:5-6.
[0041] In some embodiments, the thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid is prepared by the above preparation method.
[0042] In some embodiments, the use of a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid, the thiol-modified MXene adsorbent is used to enrich silver in the silver electrolysis waste liquid, for example:
[0043] 10-100 mg / L of thiol-modified MXene adsorbent is added to the silver electrolysis waste liquid and stirred for 20-180 min to allow the thiol-modified MXene adsorbent to fully contact with the ultrafine silver particles or low-concentration silver ions in the silver electrolysis waste liquid. Under the coupling effect of physical adsorption and chemical adsorption, the recovery of silver resources in the silver electrolysis waste liquid is convenient and fast.
[0044] The technical details are further illustrated below in conjunction with embodiments.
[0045] Example 1
[0046] Example 1 discloses a method for preparing a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid, comprising:
[0047] The spent denitrification catalyst was reduced in a methane-hydrogen mixed atmosphere with hydrogen, methane accounting for 10% of the total gas content, the reduction temperature was set to 1200°C, and the reduction time was 5h to obtain the following Figure 1 The carbonitride composite precursor shown, Figure 1 The medium-light grey lumps are metallic iron formed by reduction, and the dark grey granular substances dispersed around them are carbides. In order to reduce the reaction temperature, 5% solid mass of ferric oxide is added as an additive during the hydrogen-rich reduction process.
[0048] The carbonitride composite precursor is ground, mixed with aluminum powder and titanium powder in a molar ratio of 2:1:2, and pressurelessly sintered in an argon atmosphere to obtain a carbonitride ceramic precursor with an aluminum intercalation layer; wherein the sintering temperature is 1500°C and the sintering time is 8 hours;
[0049] 1g of carbonitride ceramic precursor with aluminum intercalation was reacted with 20mL of hydrofluoric acid solution, the aluminum intercalation in the carbonitride ceramic precursor was ionized and released, and the titanium and vanadium sites formed oxygen-containing end grains to obtain low-dimensional MXene;
[0050] The low-dimensional MXene is uniformly dispersed in an acetic acid solution, 1,3-mercaptopropyltrimethoxysilane is added, and the pH is controlled at 6.5 to obtain a mixed suspension; glutaraldehyde is added to the mixed suspension, and the mixture is reacted at a low temperature below 5°C for 18 hours to obtain a thiol-modified MXene adsorbent; wherein the volume ratio of 1,3-mercaptopropyltrimethoxysilane to acetic acid is 5:4, the solid-liquid ratio in the mixed suspension is 1:1, and the volume ratio of glutaraldehyde to the mixed suspension is 1:5.
[0051] The thiol-modified MXene adsorbent prepared in Example 1 is used to recover silver from silver electrolysis waste liquid, specifically comprising:
[0052] 50 mg / L of thiol-modified MXene adsorbent was added to the silver electrolysis waste liquid and stirred for 100 minutes to allow the thiol-modified MXene adsorbent to fully contact the ultrafine silver particles or low-concentration silver ions in the silver electrolysis waste liquid. Under the coupling effect of physical adsorption and chemical adsorption, the silver resources in the silver electrolysis waste liquid were recovered quickly and conveniently, with a recovery rate of 98%.
[0053] Example 2
[0054] Example 2 discloses a method for preparing a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid, comprising:
[0055] The titanium concentrate is subjected to hydrogen-rich reduction in a methane-hydrogen mixed atmosphere, where methane accounts for 8% of the total gas content, the reduction temperature is set to 1200°C, and the reduction time is 8 hours to obtain a carbonitride composite precursor;
[0056] The carbonitride composite precursor is ground, mixed with aluminum powder and titanium powder in a molar ratio of 1:1:1, and pressurelessly sintered in an argon atmosphere to obtain a carbonitride ceramic precursor with an aluminum intercalation layer; wherein the sintering temperature is 1600°C and the sintering time is 6 hours;
[0057] 1g of carbonitride ceramic precursor with aluminum intercalation was reacted with 20mL of hydrogen chloride-lithium chloride mixed solution, the aluminum intercalation in the carbonitride ceramic precursor was ionized and released, and the titanium and vanadium sites formed oxygen-containing end grains to obtain low-dimensional MXene;
[0058] The low-dimensional MXene is uniformly dispersed in an acetic acid solution, 1,3-mercaptopropyltrimethoxysilane is added, and the pH is controlled at 7 to obtain a mixed suspension; glutaraldehyde is added to the mixed suspension, and the mixture is reacted at a low temperature below 5°C for 25 hours to obtain a thiol-modified MXene adsorbent; wherein the volume ratio of 1,3-mercaptopropyltrimethoxysilane to acetic acid is 5:4, the solid-liquid ratio in the mixed suspension is 1:2, and the volume ratio of glutaraldehyde to the mixed suspension is 1:6.
[0059] The XPS results of the thiol-modified MXene adsorbent prepared in Example 2 are as follows: Figure 2 As shown, from Figure 2 It can be seen that chemical bonds such as Ti-C and Ti-O still exist in the thiol-modified MXene adsorbent, confirming that the low-dimensional MXene structure is completely retained after modification.
[0060] The thiol-modified MXene adsorbent prepared in Example 2 is used to recover silver from silver electrolysis waste liquid, specifically comprising:
[0061] 100 mg / L of thiol-modified MXene adsorbent was added to the silver electrolysis waste liquid and stirred for 180 minutes to allow the thiol-modified MXene adsorbent to fully contact the ultrafine silver particles or low-concentration silver ions in the silver electrolysis waste liquid. Under the coupling effect of physical adsorption and chemical adsorption, the silver resources in the silver electrolysis waste liquid were recovered quickly and conveniently, with a recovery rate of 99%.
[0062] The preparation method of the thiol-modified MXene adsorbent for recovering silver electrolytic waste liquid disclosed in the embodiment of the present invention is to first reduce and carbonize the low-valent titanium-containing mineral in a hydrogen-rich reduction system, and then mix and control it with aluminum powder and titanium powder to prepare a carbonitride ceramic precursor with an aluminum intercalation layer, and then introduce an interface inducer to react with it to prepare a low-dimensional MXene material, and then use a solvent thermal reaction to perform thiol modification in an acetic acid solution, while retaining hydrophilicity, while enhancing the selectivity for silver, which is suitable for efficient recovery of silver in acidic electrolytic waste liquid. The thiol-modified MXene adsorbent for recovering silver electrolytic waste liquid disclosed in the embodiment of the present invention has hydrophilicity and selective adsorption, and can efficiently and selectively adsorb silver ions and silver particles.
[0063] The technical solutions disclosed in the present invention and the technical details disclosed in the embodiments are merely illustrative of the inventive concept of the present invention and do not constitute a limitation on the technical solutions of the present invention. Any conventional changes, substitutions or combinations of the technical details disclosed in the embodiments of the present invention have the same inventive concept as the present invention and are within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid, characterized in that: Includes steps: S1, reducing a low-valent titanium-containing mineral to obtain a carbonitride composite precursor; S2, mixing the carbonitride composite precursor with aluminum powder and titanium powder according to a set ratio, and sintering without pressure in an inert atmosphere to obtain a carbonitride ceramic precursor with an aluminum intercalation layer; S3, reacting a carbonitride ceramic precursor having an aluminum intercalation layer with an interface inducing agent, wherein the aluminum intercalation layer in the carbonitride ceramic precursor is ionized and released, and the titanium and vanadium sites form oxygen-containing end grains to obtain a low-dimensional MXene; S4. Evenly disperse the low-dimensional MXene in an acetic acid solution, add 1,3-mercaptopropyltrimethoxysilane, and control the pH value at 6.5 to 8 to obtain a mixed suspension; add glutaraldehyde to the mixed suspension, and react at low temperature for 18 to 30 hours to obtain a thiol-modified MXene adsorbent.
2. The method for preparing a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid according to claim 1, characterized in that: The low-valent titanium-containing minerals include one or more of vanadium-titanium magnetite, titanium concentrate, titanium dioxide, and waste denitrification catalysts.
3. The method for preparing a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid according to claim 1, characterized in that: In step S1, the hydrogen-rich reducing atmosphere is composed of hydrogen and one or more of methane, ammonia, and nitrogen, wherein the volume content of hydrogen is 80-98%; the temperature of hydrogen-rich reduction is 1200-1500° C., and the time is 2-10 hours.
4. The method for preparing a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid according to claim 1, characterized in that: The molar ratio of the carbonitride composite precursor, the aluminum powder and the titanium powder is 2:1 to 2:1 to 2.
5. The method for preparing a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid according to claim 1, characterized in that: The interface inducing agent is hydrofluoric acid, a hydrogen chloride-lithium chloride mixed solution or a lithium hydroxide solution.
6. The method for preparing a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid according to claim 1, characterized in that: The volume ratio of the 1,3-mercaptopropyltrimethoxysilane to the acetic acid is 5:
4.
7. The method for preparing a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid according to claim 1, characterized in that: The solid-liquid ratio in the mixed suspension is 1:1-2.
8. The method for preparing a thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid according to claim 1, characterized in that: The volume ratio of the glutaraldehyde to the mixed suspension is 1:5-6.
9. A thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 8.
10. The use of the thiol-modified MXene adsorbent for recovering silver electrolysis waste liquid according to claim 9, characterized in that: The thiol-modified MXene adsorbent is used to enrich silver in silver electrolysis waste liquid.