Method for preparing hydrogenated bisphenol A through catalytic hydrogenation in waste fan blade epoxy resin pyrolytic oil
Through the combined use of metal-oxide catalyst and n-hexane, hydrogenation reaction under a reducing atmosphere, the waste epoxy resin pyrolytic oil is converted into high added value hydrogenated bisphenol A, which solves the waste epoxy resin pyrolytic oil The problem of low recycling efficiency has achieved a win-win situation for environmental protection and economic win-win results.
Patent Information
- Application Number
- CN202411122741.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
The recycling benefits of waste epoxy resin pyrolytic oil are low and difficult to effectively convert into high value-added compounds. The existing treatment methods have problems with carbon emissions and secondary pollution.
The metal-oxide catalyst and n-hexane are used as solvents to conduct hydrogenation reaction under a reducing atmosphere to convert the pyrolytic oil of the epoxy resin in the waste fan blade into hydrogenated bisphenol A, retaining the ring structure and improving catalytic activity.
High added value hydrogenated bisphenol A preparation is achieved, the economic benefits of recycling of waste epoxy resin pyrolytic oils are improved, and environmentally friendly and harmless treatment is carried out.
Smart Images

Figure CN119016044A_ABST
Abstract
Description
Technical field:
[0001] The invention relates to the technical field of solid organic waste pyrolysis oil treatment, and in particular to a method for preparing hydrogenated bisphenol A by catalytic hydrogenation in waste fan blade epoxy resin pyrolysis oil. Background technology:
[0002] Curable epoxy resin is a kind of insoluble and infusible chemical cross-linked polymer with aliphatic or aromatic main chain structure as the basic skeleton, containing two or more reactive epoxy groups and other functional groups in the structure, which is formed by irreversible curing reaction under appropriate conditions. Epoxy resin has many excellent comprehensive properties. After being compounded with carbon fiber or glass fiber, epoxy resin-based fiber-reinforced composite materials have the advantages of light weight, durability, high strength, and strong performance designability. They are often used in coatings, adhesives, composite materials and other fields. However, the treatment of waste epoxy resin has become an important issue in environmental protection. Due to the unique three-dimensional network cross-linked structure of epoxy resin after curing, it is difficult to degrade and recycle, which poses potential harm to the environment. At present, the large-scale treatment methods of waste epoxy resin and its composite materials include mechanical processing, direct landfill, incineration and pyrolysis. Direct landfill and incineration are not limited by the type of resin, but they will lead to larger carbon emissions and potential secondary pollution. The resin particles recovered by mechanical processing can be used for other mixed materials such as concrete fillers, but the performance of recycled composite materials may be reduced due to multiple processing, making it difficult to recycle them physically. Therefore, it is still necessary to adopt a reasonable and effective way to recycle the ultimate waste and achieve harmless treatment. Pyrolysis treatment of waste epoxy resin is currently a relatively environmentally friendly technology that can improve economic value. After pyrolysis of waste epoxy resin, a large amount of monocyclic and bicyclic phenol derivatives will be produced. These monocyclic and bicyclic phenol derivatives can be used as fuel for energy recovery and pyrolysis heating.
[0003] Waste epoxy resin pyrolysis oil contains a large amount of phenolic compounds and can be regarded as a valuable hydrocarbon resource. Therefore, exploring a method that can retain the ring structure and convert it into hydrogenated bisphenol A can upgrade and recycle waste epoxy resin pyrolysis oil into high value-added compounds, which can effectively improve the economic benefits of recycling waste epoxy resin pyrolysis oil. Summary of the invention:
[0004] The invention solves the problem of low recovery efficiency of waste epoxy resin pyrolysis oil and provides a method for preparing hydrogenated bisphenol A by catalytic hydrogenation in waste fan blade epoxy resin pyrolysis oil. The invention fully retains the cyclic structure and -OH functional group of phenol derivatives in epoxy resin pyrolysis oil. n-hexane as a reaction solvent can not only improve the solubility of hydrogen, but also promote the transfer of active hydrogen in the catalyst-pyrolysis oil, thereby improving the activity of hydrogenation reaction. The problem of high-value recovery of mixed phenol derivatives in low-value epoxy resin pyrolysis oil is solved, and the epoxy resin pyrolysis oil is catalyzed to be converted into high-value-added hydrogenated bisphenol A.
[0005] The first object of the present invention is to provide a method for preparing a metal-oxide catalyst, comprising the following steps: using an ion exchange method, adding a metal oxide carrier or a zeolite carrier to an active metal salt solution, filtering and drying after sufficient ion exchange to obtain a catalyst precursor, and then activating the catalyst precursor in a reducing atmosphere to obtain the metal-oxide catalyst.
[0006] Preferably, the active metal is Ru, and the active metal loading is 0.5% to 5% based on the mass of the metal oxide carrier or the zeolite carrier. The active metal salt solution is a RuCl3 aqueous solution, the amount of water added in the RuCl3 aqueous solution is fixed at 25 mL, and the mass of the RuCl3 solid is changed to obtain active metal salt solutions of different concentrations.
[0007] The metal oxide carrier or zeolite carrier is added to the active metal salt solution, and the ion exchange is fully carried out before filtering and drying. The specific steps are as follows: under stirring, the metal oxide or zeolite carrier is slowly added to the active metal salt solution, and stirring is continued for several hours after the complete addition, and the ion exchange is followed by filtering, and the solution is transferred to an oven for overnight drying.
[0008] Preferably, the metal oxide carrier is selected from one or more of CeO2, γ-Al2O3, and ZrO2, and the zeolite carrier is ZSM-5.
[0009] Preferably, the activation conditions are: H2 atmosphere, activation temperature 450°C to 650°C, heating rate 2 to 5°C / min, and activation time 3 to 5h.
[0010] The second object of the present invention is to provide a metal-oxide catalyst obtained by the preparation method.
[0011] The third object of the present invention is to provide a method for preparing hydrogenated bisphenol A by catalytic hydrogenation in waste fan blade epoxy resin pyrolysis oil, comprising the following steps: mixing the waste fan blade epoxy resin pyrolysis oil, the metal-oxide catalyst and n-hexane in a reaction container, stirring and reacting under a reducing atmosphere to obtain a liquid product containing hydrogenated bisphenol A.
[0012] The method proposed by the present invention can quickly convert low-value mixed waste epoxy resin pyrolysis oil into high-value hydrogenated bisphenol A. The present invention introduces n-hexane as a solvent and uses a metal-oxide catalyst to promote the hydrogenation reaction. It is feasible to convert waste epoxy resin pyrolysis oil into high-value hydrogenated bisphenol A in a targeted manner, achieving a win-win situation for green and economic development.
[0013] Preferably, the mass ratio of the waste fan blade epoxy resin pyrolysis oil to the catalyst is 1 to 5:1, and the mass volume ratio of the waste fan blade epoxy resin pyrolysis oil to n-hexane is 1:20 to 60 g / mL.
[0014] Preferably, the reaction conditions are: H2 atmosphere, reaction temperature 150°C to 250°C, stirring rate 500 to 800 rpm, and reaction time 0.5 to 1.5 h.
[0015] Preferably, the liquid phase product also includes cyclohexanol and isopropyl cyclohexanol.
[0016] Compared with the prior art, the present invention has the following advantages:
[0017] 1. The present invention uses n-hexane as a solvent, which can not only improve the solubility of hydrogen, but also promote the transfer of active hydrogen in the catalyst-pyrolysis oil, thereby improving the activity of the hydrogenation reaction.
[0018] 2. The metal-oxide catalyst prepared by the present invention is directly reduced in a reducing gas after loading the metal to obtain large particles of Ru with high catalytic activity. 0 Species can help promote the intra-ring hydrogenation of bisphenol A and improve the catalytic efficiency.
[0019] 3. The 3% Ru / CeO2 catalyst prepared by the present invention has a synergistic effect with the n-hexane solvent. The catalyst and bisphenol A are separated from n-hexane, which improves the accessibility of the catalyst active sites during the reaction. The hydrogenated bisphenol A product can be dissolved in n-hexane, which helps to extract the hydrogenated bisphenol A from the catalyst and improve the yield of hydrogenated bisphenol A.
[0020] 4. The waste epoxy resin pyrolysis oil is converted into high value-added hydrogenated bisphenol A. The metal-oxide catalyst used in the present invention has a high hydrogenation activity, which can retain the cyclic structure of the phenolic compound while inhibiting the cracking of the -OH functional group.
[0021] 5. The present invention achieves the quality improvement and utilization of low-value-added waste epoxy resin pyrolysis oil, solves the difficult problems of selective intracyclic hydrogenation of mixed phenol pyrolysis oil and inhibition of -OH functional group cracking, and improves the economic benefits of waste epoxy resin pyrolysis oil recovery. Description of the drawings:
[0022] Figure 1 This is the product spectrum obtained in Example 1.
[0023] Figure 2 This is the mass transfer state of bisphenol A and 3% Ru / CeO2 catalyst in different solvents. Specific implementation method:
[0024] The following examples are provided to further illustrate the present invention, rather than to limit the present invention.
[0025] Unless otherwise defined, all professional terms used hereinafter have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the experimental materials and reagents herein are conventional commercial products in the art.
[0026] In the following example, the waste fan blade epoxy resin pyrolysis oil is obtained by the following steps: the waste fan blade is pyrolyzed at 350°C and N2 atmosphere for 30 minutes, the liquid phase product is collected to obtain the waste fan blade epoxy resin pyrolysis oil, and the bisphenol A product is obtained after separation.
[0027] Example 1
[0028] A method for preparing hydrogenated bisphenol A by catalytic hydrogenation in waste fan blade epoxy resin pyrolysis oil comprises the following steps:
[0029] S1: Weigh the active metal salt RuCl3 and dissolve it in a certain amount of water. Stir it thoroughly to form an active metal salt RuCl3 solution. Weigh an appropriate amount of CeO2, with a Ru loading of 3%. Add the CeO2 carrier to the active metal salt solution under stirring and continue stirring for 2 hours to ensure sufficient ion exchange. After stirring, filter it and transfer it to an oven for overnight drying. After sufficient grinding, the catalyst precursor is obtained. The ground catalyst precursor is heated to 500°C in a H2 atmosphere at a heating rate of 2°C / min for 4 hours to obtain a 3% Ru / CeO2 catalyst.
[0030] S2: Bisphenol A obtained by separation of epoxy resin pyrolysis oil from waste fan blades and 3% Ru / CeO2 catalyst (the mass ratio of bisphenol A to catalyst is 5:1) are placed in a reactor and a certain amount of n-hexane (the mass volume ratio of bisphenol A to n-hexane is 1:60 g / mL) is added. The temperature is raised to 250°C at 5°C / min under H2 atmosphere for 60 min, and the stirring rate is 700 rpm. After the reaction, the liquid phase product is collected, a certain amount of internal standard dodecane is added, and qualitative and quantitative analysis is performed by GC-MS. The results are as follows Figure 1 The calculated yield of hydrogenated bisphenol A is 95.43%.
[0031] Comparative Example 1:
[0032] Same as Example 1, except that:
[0033] S2: waste fan blade epoxy resin pyrolysis oil and 3% Ru / CeO2 catalyst (bisphenol A to catalyst mass ratio of 5:1) were placed in a reactor and a certain amount of water (bisphenol A to water mass volume ratio of 1:60g / mL) was added, and the temperature was raised to 250℃ at 5℃ / min under H2 atmosphere for 60min, and the stirring rate was 700rpm. After the reaction, the liquid phase product was collected, a certain amount of internal standard dodecane was added, and qualitative and quantitative analysis was performed by GC-MS. The yield of hydrogenated bisphenol A was calculated to be 72.56%.
[0034] Comparative Example 2:
[0035] Same as Example 1, except that:
[0036] S2: waste fan blade epoxy resin pyrolysis oil and 3% Ru / CeO2 catalyst (bisphenol A to catalyst mass ratio of 5:1) were placed in a reactor and a certain amount of isopropanol (bisphenol A to isopropanol mass volume ratio of 1:60g / mL) was added, and the temperature was raised to 250℃ at 5℃ / min under H2 atmosphere for 60min, and the stirring rate was 700rpm. After the reaction, the liquid phase product was collected, a certain amount of internal standard dodecane was added, and qualitative and quantitative analysis was performed by GC-MS. The yield of hydrogenated bisphenol A was calculated to be 69.53%.
[0037] Comparative Example 3:
[0038] Same as Example 1, except that:
[0039] S1: Weigh a certain amount of active metal salt RuCl3 and dissolve it in a certain amount of water. Stir thoroughly to form an active metal salt RuCl3 solution. Weigh an appropriate amount of ZSM-5 with a Ru loading of 3%. Add the ZSM-5 carrier to the active metal salt solution under stirring and continue stirring for 2 hours to ensure sufficient ion exchange. After stirring, filter and transfer to an oven for overnight drying. After sufficient grinding, obtain a catalyst precursor. The ground catalyst precursor is activated at 500°C in a H2 atmosphere at a heating rate of 2°C / min for 4 hours to obtain a 3% Ru / ZSM-5 catalyst.
[0040] S2: Bisphenol A obtained by separation of waste epoxy resin pyrolysis oil and 3% Ru / ZSM-5 catalyst (the mass ratio of bisphenol A to catalyst is 5:1) are placed in a reactor and a certain amount of n-hexane (the mass volume ratio of bisphenol A to n-hexane is 1:60 g / mL) is added. The temperature is raised to 250°C at 5°C / min under H2 atmosphere for 60 min, and the stirring rate is 700 rpm. After the reaction, the liquid product is collected, a certain amount of internal standard dodecane is added, and qualitative and quantitative analysis is performed by GC-MS. The yields of hydrogenated bisphenol A and 1,1'-(1-methylethylidene)bicyclohexane are calculated to be 46.97% and 20.83%, respectively.
[0041] Comparison of Comparative Examples 1, 2 and 3 with Example 1 shows that the common reaction solvent water has insufficient hydrogen solubility, resulting in low hydrogenation reaction activity and low hydrogenated bisphenol A yield. Isopropanol with high hydrogen solubility affects the adsorption state of the benzene ring on the catalyst, resulting in the catalyst being unable to effectively hydrogenate within the bisphenol A ring, reducing the yield of hydrogenated bisphenol A. The acidic ZSM-5 zeolite carrier easily causes the -OH functional group to crack and produce alkane products. Therefore, in order to increase the yield of hydrogenated bisphenol A in the product, selecting n-hexane solvent to increase hydrogen solubility helps to increase the hydrogenation reaction activity of the catalyst; selecting a metal-oxide catalyst with weaker acidity and stronger hydrogenation deoxygenation ability to inhibit the cracking of the -OH functional group.
[0042] Embodiment 2:
[0043] A method for preparing hydrogenated bisphenol A by catalytic hydrogenation in waste fan blade epoxy resin pyrolysis oil comprises the following steps:
[0044] S1: Weigh a certain amount of active metal salt RuCl3 and dissolve it in a certain amount of water. Stir thoroughly to form an active metal salt RuCl3 solution. Weigh an appropriate amount of γ-Al2O3 with a Ru loading of 3%. Add the γ-Al2O3 carrier to the active metal salt solution under stirring and continue stirring for 2 hours to ensure sufficient ion exchange. After stirring, filter and transfer to an oven for overnight drying. After sufficient grinding, obtain a catalyst precursor. The ground catalyst precursor is activated at 500°C in a H2 atmosphere at a heating rate of 2°C / min for 4 hours to obtain a 3% Ru / γ-Al2O3 catalyst.
[0045] S2: Bisphenol A obtained by separation of waste epoxy resin pyrolysis oil and 3% Ru / γ-Al2O3 catalyst (the mass ratio of bisphenol A to catalyst is 5:1) are placed in a reactor and a certain amount of n-hexane (the mass volume ratio of bisphenol A to n-hexane is 1:60 g / mL) is added. The temperature is raised to 250°C at 5°C / min under H2 atmosphere for 60 minutes, and the stirring rate is 700 rpm. After the reaction, the liquid product is collected, a certain amount of internal standard dodecane is added, and qualitative and quantitative analysis is performed by GC-MS. The yield of hydrogenated bisphenol A is calculated to be 81.58%.
[0046] Embodiment 3:
[0047] A method for preparing hydrogenated bisphenol A by catalytic hydrogenation in waste fan blade epoxy resin pyrolysis oil comprises the following steps:
[0048] S1: Weigh a certain amount of active metal salt RuCl3 and dissolve it in a certain amount of water. After sufficient stirring, form an active metal salt RuCl3 solution. Weigh an appropriate amount of ZrO2, with a Ru loading of 3%. Under stirring conditions, add the ZrO2 carrier to the active metal salt solution and continue stirring for 2 hours to ensure sufficient ion exchange. After stirring, filter and transfer to an oven for overnight drying. After sufficient grinding, obtain a catalyst precursor. The ground catalyst precursor is activated at 500°C in a H2 atmosphere at a heating rate of 2°C / min for 4 hours to obtain a 3% Ru / ZrO2 catalyst.
[0049] S2: Bisphenol A obtained by separation of waste epoxy resin pyrolysis oil and 3% Ru / ZrO2 catalyst (the mass ratio of bisphenol A to catalyst is 5:1) are placed in a reactor and a certain amount of n-hexane (the mass volume ratio of bisphenol A to n-hexane is 1:60 g / mL) is added. The temperature is raised to 250°C at 5°C / min under H2 atmosphere for 60 min, and the stirring rate is 700 rpm. After the reaction, the liquid product is collected, a certain amount of internal standard is added, and qualitative and quantitative analysis is performed by GC-MS. The yield of hydrogenated bisphenol A is calculated to be 69.94%.
[0050] Embodiment 4:
[0051] Same as Example 1, except that:
[0052] The active metal loading in S1 is 0.5%; the activation conditions are: H2 atmosphere, activation temperature 650°C, heating rate 2°C / min, and activation time 5h.
[0053] The mass ratio of waste fan blade epoxy resin pyrolysis oil to 0.5% Ru / CeO2 catalyst in S2 is 1:1, and the mass volume ratio of waste fan blade epoxy resin pyrolysis oil to n-hexane is 1:20 g / mL; the reaction conditions are: reaction temperature 150°C, stirring rate 500 rpm, reaction time 1.5 h, and after the reaction, the liquid product is collected, a certain amount of internal standard dodecane is added, and qualitative and quantitative analysis is performed by GC-MS, and the yield of hydrogenated bisphenol A is calculated to be 43.71%.
[0054] Embodiment 5:
[0055] Same as Example 1, except that:
[0056] The active metal loading in S1 is 5%; the activation conditions are: H2 atmosphere, activation temperature 450°C, heating rate 5°C / min, and activation time 3h.
[0057] The mass ratio of waste fan blade epoxy resin pyrolysis oil to 5% Ru / CeO2 catalyst in S2 is 5:1, and the mass volume ratio of waste fan blade epoxy resin pyrolysis oil to n-hexane is 1:60 g / mL; the reaction conditions are: reaction temperature 250°C, stirring rate 800 rpm, reaction time 0.5 h, and after the reaction, the liquid product is collected, a certain amount of internal standard dodecane is added, and qualitative and quantitative analysis is performed by GC-MS, and the yield of hydrogenated bisphenol A is calculated to be 88.95%.
[0058] The description of the above embodiments is only used to help understand the technical solution and core ideas of the present invention. It should be pointed out that for technicians in this technical field, several improvements and modifications can be made to the present invention without departing from the principles of the present invention. These improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A method for preparing a metal-oxide catalyst, characterized in that: The method comprises the following steps: using an ion exchange method, adding a metal oxide carrier or a zeolite carrier to an active metal salt solution, filtering and drying after sufficient ion exchange to obtain a catalyst precursor, and then activating the catalyst precursor in a reducing atmosphere to obtain the metal-oxide catalyst.
2. The preparation method according to claim 1, characterized in that: The active metal is Ru, and the active metal loading is 0.5% to 5% based on the mass of the metal oxide carrier or the zeolite carrier.
3. The preparation method according to claim 1 or 2, characterized in that: The metal oxide carrier is selected from one or more of CeO2, γ-Al2O3, and ZrO2, and the zeolite carrier is selected from ZSM-5.
4. The preparation method according to claim 1 or 2, characterized in that: The activation conditions are: H2 atmosphere, activation temperature 450°C to 650°C, heating rate 2 to 5°C / min, and activation time 3 to 5h.
5. The metal-oxide catalyst obtained by the preparation method according to any one of claims 1 to 4.
6. A method for preparing hydrogenated bisphenol A by catalytic hydrogenation of epoxy resin pyrolysis oil from waste fan blades, characterized in that: The method comprises the following steps: mixing waste fan blade epoxy resin pyrolysis oil, the metal-oxide catalyst according to claim 5 and n-hexane in a reaction container, stirring and reacting under a reducing atmosphere to obtain a liquid phase product containing hydrogenated bisphenol A.
7. The method according to claim 6, characterized in that The mass ratio of the waste fan blade epoxy resin pyrolysis oil to the catalyst is 1-5:1, and the mass volume ratio of the waste fan blade epoxy resin pyrolysis oil to n-hexane is 1:20-60 g / mL.
8. The method according to claim 6, characterized in that The reaction conditions are: H2 atmosphere, reaction temperature 150°C to 250°C, stirring rate 500 to 800 rpm, and reaction time 0.5 to 1.5 h.
9. The method according to claim 6, characterized in that The liquid phase product also includes cyclohexanol and isopropyl cyclohexanol.