Preparation method and application of manganese-based amorphous / nanocrystalline wide-temperature-range catalyst

Manganese-based amorphous/nano-crystalline alloy tape prepared by copper roller fast quenching method solves the temperature sensitivity of amorphous alloy catalyst, realizes efficient degradation of dye wastewater in a wide temperature zone, and demonstrates excellent thermal stability and Catalytic properties.

CN119016062APending Publication Date: 2024-11-26GUANGDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411114445.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing amorphous alloy catalysts have a narrow reaction temperature range during the degradation of dye wastewater, which limits their practical application, especially the catalytic degradation capacity below room temperature is insufficient.

Method used

The copper roller fast quenching method is used to prepare manganese-based amorphous/nano-crystal alloy tape. By controlling the copper roller speed and the aperture size of the quartz tube port, a multi-element amorphous/nano-crystal biphasic structure is formed, and used as a catalyst for dye wastewater. degradation.

Benefits of technology

It has achieved efficient catalytic degradation of dye wastewater in a wide temperature zone. The surface of the material is bright and not easy to oxidize, and has high thermal stability and catalytic performance, especially at room temperature. It still maintains a high catalytic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016062A_ABST
    Figure CN119016062A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a manganese-based amorphous / nanocrystalline wide-temperature-range catalyst. The invention relates to a manganese-based amorphous alloy. The chemical general formula of the manganese-based amorphous alloy is MnbasSix1Bx2PyMz, in the general formula, Mnbas represents an alloy system with Mn as a matrix, the atomic mole number of the Mnbas is as follows: bass is greater than or equal to 50, x1 is greater than or equal to 10 and less than 30, x2 is greater than or equal to 2 and less than 20, y is greater than or equal to 0 and less than 10, z is greater than or equal to 0 and less than 20, and bass + x1 + x2 + y + z is equal to 100; m is selected from one or more of Cu, Nb, Fe, Mo, Ni and Co. The manganese-based amorphous alloy material disclosed by the invention has excellent dye wastewater degradation capability in a wide reaction temperature zone.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of amorphous / nanocrystalline alloy catalysis, and in particular to a preparation method and application of a manganese-based amorphous / nanocrystalline wide temperature range catalyst. Background Art

[0002] Metallic glasses (MGs), also known as amorphous alloys, have been widely used in various functional fields due to their unique chemical and structural homogeneity. In recent years, MGs have received widespread attention as a rising star in the field of catalysis, such as catalytic hydrogen evolution, oxygen evolution, and oxidation of methanol and ethanol. In general, the catalytic activity and stability of MGs are superior to those of crystalline materials because they have a large number of unsaturated coordinated atoms, highly concentrated active sites, metastable induced high Gibbs free energy, and uniform atomic structure without crystal defects. Therefore, they are considered to be advanced substitutes for crystalline materials in many catalytic applications. Studies have shown that Fe-based amorphous alloys show significant advantages in catalytic degradation of dye wastewater. However, due to the narrow pH range of Fe-based amorphous catalysts, their corrosion resistance is poor. In recent years, the research focus in the field of wastewater treatment has also begun to shift to other amorphous alloy catalysts, such as Co-based, Al-based, Mg-based, etc. It is found without exception that although these matrix amorphous alloys have their own advantages, they can only effectively degrade dye wastewater at reaction temperatures above 25°C. The limitation of the catalytic reaction temperature zone reduces the production practicality of amorphous alloys. Broadening the temperature range of catalytic degradation of alloy materials and finding an alloy material that can catalytically degrade below room temperature (25°C) are issues that need to be addressed urgently. Summary of the invention

[0003] In order to solve the problem of narrow reaction temperature range for catalytic degradation of wastewater by amorphous alloys in the prior art, the present invention provides a preparation method and application of a manganese-based amorphous / nanocrystalline wide temperature range catalyst.

[0004] Previous research on Mn-based catalysts has mainly focused on manganese oxides of different valence states and multi-metal manganese oxide heterostructures. Although significant progress has been made in these areas, the application and performance research of Mn-based amorphous / nanocrystalline in the field of catalysis is still insufficient. In particular, there are relatively few research literatures on Mn-based amorphous alloys, and their preparation methods mainly focus on magnetron sputtering and ball milling, which to a certain extent limits the research progress of Mn-based amorphous / nanocrystalline alloys in the field of catalysis. In addition, experiments have found that Mn-based amorphous alloys have lower activation energy, which means that they are easier to activate and have fewer energy barriers to overcome when the reaction occurs. In addition, the alloy material is insensitive to the reaction temperature, which enables the alloy to achieve catalytic degradation in a wider temperature range.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] The first aspect of the present invention provides a manganese-based amorphous alloy, the chemical formula of the manganese-based amorphous alloy is: bas Si x1 B x2 P y M z ;

[0007] In the general formula, Mn bas It represents an alloy system based on Mn, whose atomic mole number bas≥50, 10≤x1<30, 2≤x2<20, 0≤y<10, 0≤z<20, bas+x1+x2+y+z=100;

[0008] M is selected from one or more of Cu, Nb, Fe, Mo, Ni and Co.

[0009] Preferably, M is selected from one of Cu, Nb, Ni, Mo and Fe.

[0010] Preferably, the M is Fe and Cu existing simultaneously.

[0011] Preferably, the M is Cu and Mo existing simultaneously.

[0012] Preferably, the M is Cu and Nb existing simultaneously.

[0013] In some preferred embodiments of the present invention, when M is Fe and y is 0, the thermal stability and catalytic performance of the manganese-based amorphous alloy are improved.

[0014] Preferably, the chemical formula of the manganese-based amorphous alloy is Mn 67 Si 12 B 11 Fe 10 , Mn 69 Si 12 B 11 Fe8、Mn 71 Si 12 B 11 Fe6、Mn 73 Si 12 B 11 Fe4、Mn 74 Si 15 One of B7Cu1Nb3.

[0015] The second aspect of the present invention provides a method for preparing the manganese-based amorphous alloy, comprising the following steps:

[0016] (1) mixing raw materials according to the ratio of the manganese-based amorphous alloy, and then smelting to obtain a master alloy ingot;

[0017] (2) The master alloy ingot is crushed and placed in a quartz tube, and an amorphous alloy strip is prepared by a strip spinning machine. The rotation speed of the copper roller and the aperture size of the quartz tube port are controlled to prepare the master alloy ingot into a manganese-based amorphous alloy.

[0018] Preferably, in step (1), the smelting current is 70-140A.

[0019] Preferably, in step (2), the port aperture of the quartz tube is 0.1-0.6 mm, and the linear speed of the copper roller is 40-60 m / s.

[0020] The second aspect of the present invention provides the use of the manganese-based amorphous alloy and / or the manganese-based amorphous alloy prepared by the preparation method in catalytic degradation of dye wastewater.

[0021] The third aspect of the present invention provides a method for treating dye wastewater, comprising the following steps: adding the manganese-based amorphous alloy and / or the manganese-based amorphous alloy prepared by the preparation method as a catalyst to the dye wastewater to be treated, adding H2O2, stirring, and achieving pollutant degradation.

[0022] Preferably, the temperature of the dye wastewater to be treated is 0-45°C.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The manganese-based amorphous alloy material of the present invention has excellent dye wastewater degradation ability in a wide reaction temperature range.

[0025] The manganese-based amorphous-nanocrystalline alloy strip prepared by the copper roller rapid quenching method of the present invention has the characteristics of simple preparation process and high production efficiency; at the same time, the amorphous-nanocrystalline composite structure makes it easy to form a primary cell when catalyzing the degradation of dyes, accelerates the degradation of dye wastewater, and can especially maintain a high catalytic efficiency in a wider temperature range.

[0026] The present invention successfully prepares manganese-based amorphous and manganese-based amorphous-nanocrystalline alloy strips by using a specific element ratio and accurately controlling the copper roller rotation speed and the quartz tube port aperture size. Compared with the traditional annealing method, the amorphous-nanocrystalline dual-phase structure prepared by this method has the characteristics of bright surface, not easy to oxidize, stable structure, etc., and the atoms maintain a higher energy state. This makes the manganese-based amorphous-nanocrystalline alloy strip have great potential in catalytic applications.

[0027] The present invention combines the advantages of manganese-based catalysts and amorphous / nanocrystalline catalysis to successfully prepare manganese-based amorphous / nanocrystalline alloy strips. Compared with magnetron sputtering and ball milling, multiple elements are successfully added into the manganese-based substrate. The prepared multi-element manganese-based catalyst has high catalytic efficiency and is green and pollution-free. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 Mn is the Mn of the embodiment bas Si x1 B x2 P y M z XRD spectrum of amorphous alloy strip;

[0029] Figure 2 Mn is the Mn of the embodiment bas Si x1 B x2 P y M z DSC curve of amorphous alloy strip;

[0030] Figure 3 Mn is the Mn of the embodiment bas Si x1 B x2 P y M z The catalytic degradation rate diagram of amorphous alloy strip to dye RhB solution at room temperature (25℃);

[0031] Figure 4 Mn is the Mn of the embodiment bas Si x1 B x2 P y M z The catalytic degradation rate diagram of amorphous alloy strip to dye RhB solution in a wide temperature range;

[0032] Figure 5 Mn is the Mn of the embodiment 74 Si 15 XRD spectrum of B7Cu1Nb3 amorphous-nanocrystalline alloy strip;

[0033] Figure 6 Mn is the Mn of the embodiment 74 Si 15 TEM analysis of B7Cu1Nb3 amorphous-nanocrystalline alloy strip;

[0034] Figure 7 Mn is the Mn of the embodiment 74 Si 15 UV-visible spectra of B7Cu1Nb3 amorphous-nanocrystalline alloy strips in low-temperature ice-water bath (0℃, RE0) and room temperature (25℃, RE25) to dye RhB solution;

[0035] Figure 8 Mn is the Mn of the embodiment 74 Si 15Comparison of the catalytic degradation rate of B7Cu1Nb3 amorphous-nanocrystalline alloy strip to dye RhB solution in a wide temperature range;

[0036] Fig. 9 Mn is the Mn of the embodiment 74 Si 15 Comparison of the catalytic degradation rate constants of B7Cu1Nb3 amorphous-nanocrystalline alloy strips to dye RhB solution at low temperature ice water bath (0℃, RE0) and room temperature (25℃, RE25);

[0037] Fig.10 Mn of the embodiment 74 Si 15 Arrhenius equation fitting curve of B7Cu1Nb3 amorphous-nanocrystalline alloy strip;

[0038] Fig.11 Mn of the embodiment 74 Si 15 B7Cu1Nb3 amorphous-nanocrystalline alloy strip cyclic degradation efficiency diagram. DETAILED DESCRIPTION

[0039] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0040] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.

[0041] A manganese-based amorphous alloy, the chemical formula of the manganese-based amorphous alloy is: Mn bas Si x1 B x2 P y M z ; In the general formula, Mn bas It represents an alloy system with Mn as the matrix, whose atomic molar number bas≥50, 10≤x1<30, 2≤x2<20, 0≤y<10, 0≤z<20, bas+x1+x2+y+z=100; M is selected from one or more of Cu, Nb, Fe, Mo, Ni, and Co.

[0042] The manganese-based amorphous alloy is prepared by the following preparation method:

[0043] Step 1: mixing the raw materials of the manganese-based amorphous alloy according to the ratio of the manganese-based amorphous alloy, and then smelting to obtain a master alloy ingot;

[0044] Step 2: by controlling the rotation speed of the copper roller and the aperture size of the quartz tube port, the master alloy ingot is prepared into an amorphous or amorphous-nanocrystalline alloy strip, wherein the proportion of the amorphous phase to the nanocrystalline phase in the amorphous-nanocrystalline alloy strip can be controlled by this process.

[0045] In step 1, the smelting is high arc smelting.

[0046] Specifically, the industrial raw materials required for preparing alloy ingots include metal or non-metallic elements such as Mn, Fe, Cu, Mo, Nb, Ni, Co, Si, compounds Fe-B, Fe-P, and intermediate alloys Mn-Si and Mn-B. Before smelting, the raw materials are placed in a smelting pot in a certain proportion, and then vacuumed. The vacuum degree is controlled at 3.6×10 -3 Pa, and then high-purity argon (99.999%) is filled into the furnace. At this time, the argon mainly acts as a protective gas and has the function of arc initiation. Before smelting the target metal ingot each time, the titanium ingot is first smelted to ensure that the oxygen in the furnace is completely exhausted to obtain a high vacuum furnace environment. In addition, during the re-smelting process, each sample is repeatedly smelted four times in succession to ensure that the composition of the prepared alloy ingot is uniform, and the current during smelting is controlled at 70-140A.

[0047] In step 2, the preparation method is a copper roller rapid quenching and strip spinning method.

[0048] Specifically, the amorphous / nanocrystalline alloy strips in step 2 are all prepared by a high vacuum NMS-Ⅱ type induction melt quenching strip spinning machine. In order to ensure the high thermal conductivity of the copper roller itself, the surface of the copper roller is first polished to effectively remove the copper oxide attached to the surface of the copper roller, thereby ensuring that the surface of the copper roller is clean to achieve better cooling capacity. The quartz tube containing the master alloy ingot is fixed in the induction coil above the copper roller. After adjusting the distance between the nozzle and the copper roller, the furnace door is closed and high-purity argon is injected. After controlling the copper roller to rotate smoothly, the master alloy in the quartz tube is heated by induction coil heating. After it is in a completely molten state, the switch of the pressure chamber gas cylinder is pressed in time. The pressure difference formed sprays the molten liquid in the quartz tube onto the high-speed rotating copper roller, and the melt is instantly thrown out by centrifugal force, thereby obtaining a continuous amorphous / nanocrystalline alloy strip. The strip spinning parameters used in this experiment are: copper roller speed: 40-60 m / s, nozzle-copper roller distance: 1-2 mm, port aperture size: 0.1-0.6 mm, pressure difference between quartz tube and furnace chamber: 0.05 MPa, and the obtained strip parameters are: thickness: 20-25 μm, width: 1.0-1.5 mm.

[0049] Specifically, the D / Max-ⅢA X-ray diffraction analyzer produced by Rigaku Corporation of Japan was used to detect the prepared manganese-based amorphous alloy strip. The amorphous strip showed a broad "mantou peak", and the phase structure of the nanocrystalline strip was determined by comparing it with the standard PDF card. The test used a monochromatic Cu-Kα target, the X-ray wavelength was 0.1540nm, the working voltage U was 40kV, the working current was 30mA, and without special instructions, the scanning angle was 20-90°, the step length was 0.02°, and the rate was 3-10° / min. The DSC equipment used in the present invention is a TA SDT Q600 heat flow differential scanning calorimeter, equipped with a DSC-TGA mode, which can simultaneously record heat flow curves and thermogravimetric change curves. The specific parameters of the test are: sample weight: 10-20mg, gas flow rate: 100mL / min high-purity nitrogen atmosphere, heating rate 10℃ / min, temperature range: 200-900℃.

[0050] Specifically, the transmission electron microscope model used is FEI Tecnai G2 F20, equipped with Oxford X-Max 80T spectrometer, and its acceleration voltage is 200KV. Its resolution can reach 0.1-0.2nm, and it can achieve a magnification effect of up to one million times, further revealing the microstructural details of manganese-based amorphous-nanocrystalline alloy strips.

[0051] The manganese-based amorphous alloy is used to catalyze the degradation of dye wastewater, which specifically includes the following process:

[0052] Prepare 100 mL of Rhodamine B solution in a 250 mL beaker (the concentration of the solution is 20 mg L unless otherwise specified). -1 ), put the prepared solution into a constant temperature water bath and set the corresponding insulation temperature (0℃~45℃), adjust the pH to the required experimental value (pH=3 by default unless otherwise specified) with 0.1M sulfuric acid and 0.1M sodium hydroxide solution. Cut the strip into strips with a length of 10mm and weigh the required weight for the experiment, put it into the prepared solution, and stir it with a mechanical stirring device at a stirring rate of 500rpm. During the degradation process, 3mL of solution is extracted with a disposable syringe at specific time intervals, and impurities are filtered through a filter membrane with a filter diameter of 0.45μm. The filtered solution is immediately placed in a UV-visible photometer for testing.

[0053] Specifically, the UV-Visible photometer model used is TU-1810 produced by Beijing Puxi General, which can measure the relative intensity of light absorption by the molecules of a substance, thereby obtaining a UV-Vis spectrum. In view of the close relationship between electronic transitions and the internal structure of the material, different materials have different light absorption characteristics. Therefore, the structure, composition and content of the substance can be effectively inferred through the UV-Vis spectrum. The test parameters of this experiment are: cuvette optical path: 10mm, test wavelength range: 200~800mm. According to Lambert-Beer's law:

[0054]

[0055] Where A is the absorbance; I0 is the incident light intensity, I t is the intensity of transmitted light, a dimensionless number; ω is the molar absorption coefficient; b is the optical path length; and c is the molar concentration of the solution. ω is usually a fixed value, so A is positively correlated with c, so the change in dye concentration in the solution can be determined by the change in absorbance intensity.

[0056] D=[(C0-C t ) / C0]×100%

[0057] Where D is the degradation rate; C0 is the initial concentration of the dye; C t is the concentration of the dye at reaction time t.

[0058] Example 1

[0059] This embodiment provides Mn bas Si x1 B x2 P y M z Preparation of amorphous alloy structure and degradation performance test of dye wastewater RhB solution at room temperature, the specific steps include:

[0060] 1. Mn 67 Si 12 B 11 Fe 10 , Mn 69 Si 12 B 11 Fe8、Mn 71 Si 12 B 11 Fe6、Mn 73 Si 12 B 11 Fe4、Mn 73 Si 16 B 11 , Mn 73 Si13 B 11 Nb3、Mn 73 Si 13 B 11 Cu3、Mn 57 Si 20 B4F 15 Cu1P3、Mn 74 Si 15 The atomic molar percentage of each element in the B7Cu1Mo3 composition is converted into the atomic weight percentage. For example, Mn 69 Si 12 B 11 The raw materials required to prepare Fe8 into a 10g master alloy ingot are: Mn is 8.0766g, Si is 0.7181g, B is 0.2534g, and Fe is 0.9520g.

[0061] 2. Put the above raw materials into a vacuum arc melting furnace for arc melting. The melting current is preferably 90A. Turn the alloy ingot over and over for 4 times to ensure that the composition of the master alloy ingot is uniform.

[0062] 3. The master alloy is broken into small alloy blocks with a diameter of about 6 to 9 mm, placed in a quartz tube, and an induction melt rapid quenching belt spinning machine is used to prepare Mn 67 Si 12 B 11 Fe 10 , Mn 69 Si 12 B 11 Fe8、Mn 71 Si 12 B 11 Fe6、Mn 73 Si 12 B 11 Fe4、Mn 73 Si 13 B 11 Nb3、Mn 73 Si 13 B 11 Cu3、Mn 57 Si 20 B4F 15 Cu1P3、Mn 73 Si 15B7Cu1Mo3 amorphous alloy strip. The process for preparing amorphous alloy strip is as follows: the height of the quartz nozzle from the copper roller is 0.20mm, the port aperture of the quartz tube is 0.1-0.2mm, the linear speed of the copper roller is 55m / s, and the pressure difference of the spray strip is 0.05MPa. When the strip is thrown, a supersonic high-frequency induction heating power supply with a frequency of 20kHz is used to induction heat the master alloy block placed in the quartz tube. The heating current is 15A, and the heating holding time is about 30s. At this time, the alloy block has been completely melted into a liquid with good flow. At this time, press the spray strip button, and use the pressure difference between the quartz tube and the furnace body to press the alloy liquid out of the quartz tube nozzle and spray it onto the rapidly rotating copper roller. The copper roller is rapidly cooled and solidified into an amorphous alloy strip.

[0063] 4. The amorphous alloy strip prepared in step 3 is characterized by XRD, such as Figure 1 As shown, its XRD spectrum only shows a broad diffraction peak at the diffraction angle 2θ=44°, namely the "mantou peak", indicating that the sample is an amorphous alloy strip sample with an amorphous structure under rapid quenching.

[0064] 5. Perform DSC thermal analysis on the amorphous alloy strip prepared in step 3. Figure 2 As shown, there is an obvious exothermic peak on the DSC curve of the sample, and the crystallization temperature is 578.21°C, indicating that the amorphous strip has excellent thermal stability.

[0065] The amorphous alloy strip prepared in step 3 was tested for its catalytic performance in dye wastewater. The specific experimental conditions were: reaction temperature: 25°C; pH = 3; Rh B concentration: 20ppm; strip dosage: 0.5g / L; H2O2 concentration: 1mM. The catalytic efficiency of Rh B dye solution at room temperature was as follows: Figure 3 As shown, Mn 67 Si 12 B 11 Fe 10 , Mn 69 Si 12 B 11 Fe8 has excellent catalytic degradation performance and can completely degrade dye wastewater within 10 minutes.

[0066] Figure 4 Mn 69 Si 12 B 11 The catalytic efficiency of Fe8 in RhB dye solution at different water temperatures, the specific experimental conditions are: pH = 3; Rh B concentration: 20ppm; tape dosage: 0.2g / L; H2O2 concentration: 1mM. As can be seen from the figure, it has good catalytic degradation performance in different reaction temperature zones, and when the reaction temperature is 15℃, it can also completely degrade the dye wastewater within 15 minutes.

[0067] Example 2

[0068] This embodiment provides Mn 74 Si 15 Preparation of B7Cu1Nb3 amorphous-nanocrystalline composite structure and degradation performance test of RhB solution in dye wastewater under a wide reaction temperature range, the specific steps include:

[0069] 1. Mn 74 Si 15 The atomic molar percentage of each element in the B7Cu1Nb3 component is calculated and converted into the atomic weight percentage, and the raw materials required to prepare a 10g master alloy ingot are: Mn is 8.2889g, Si is 0.8589g, B is 0.0.1543g, Cu is 0.1296g, and Nb is 0.5683g.

[0070] 2. Put the above raw materials into a vacuum arc melting furnace for arc melting. The melting current is preferably 90A. Turn the alloy ingot over and over for 4 times to ensure that the composition of the master alloy ingot is uniform.

[0071] 3. The master alloy is broken into small alloy blocks with a diameter of about 6 to 9 mm, placed in a quartz tube, and an induction melt rapid quenching belt spinning machine is used to prepare Mn 74 Si 15 B7Cu1Nb3 amorphous-nanocrystalline composite structure alloy strip. The process for preparing amorphous alloy strip is as follows: the height of the quartz nozzle from the copper roller is 0.20mm, the port aperture of the quartz tube is 0.3-0.4mm, the linear speed of the copper roller is 45m / s, and the pressure difference of the spray strip is 0.05MPa. When the strip is thrown, a supersonic high-frequency induction heating power supply with a frequency of 20kHz is used to induction heat the master alloy block placed in the quartz tube. The heating current is 15A, and the heating holding time is about 60s. At this time, the alloy block has completely melted into a liquid with good flow. At this time, the spray strip button is pressed, and the pressure difference between the quartz tube and the furnace body is used to press the alloy liquid out of the quartz tube nozzle and spray it onto the rapidly rotating copper roller. The copper roller is rapidly cooled and solidified into an amorphous-nanocrystalline alloy composite structure strip.

[0072] 4. The amorphous-nanocrystalline alloy strip prepared in step 3 is characterized by XRD, such as Figure 5 As shown, its XRD spectrum shows that Mn 74 Si 15 The B7Cu1Nb3 amorphous-nanocrystalline alloy precipitates not pure Mn phase. By comparing the PDF cards, we can see that the precipitated phases are mainly α-Mn phase (PDF#89-2133) and Mn6Si phase (PDF#20-0725).

[0073] 5. The amorphous-nanocrystalline alloy strip prepared in step 3 is characterized by TEM, such as Figure 6 As shown, its HRTEM image further proves that Mn 74 Si 15 The B7Cu1Nb3 amorphous-nanocrystalline alloy is mainly precipitated with α-Mn phase, Mn6Si phase and amorphous phase.

[0074] 6. The amorphous-nanocrystalline alloy strip prepared in step 3 was used to catalyze the degradation of dye wastewater in low-temperature ice water (0°C, RE0) and room temperature (25°C, RE25). The specific experimental conditions are: reaction temperature: 0°C / 25°C; pH = 3; Rh B concentration: 20ppm; strip dosage: 0.5g / L; H2O2 concentration: 1mM. Its UV-visible spectrum, as shown in Figure 7 As shown in the figure, as the reaction proceeds, the main absorption peak intensity of the Rh B dye solution in the visible light region (554 mm) gradually decreases, indicating that the chromophore bond of the dye is effectively destroyed. During the degradation process, the main characteristic peak (554 mm) undergoes a slight blue shift, which may be caused by the deethylation of the Rh B dye solution and the decomposition of the carboxyphenyl group. After 15 minutes of catalysis by low-temperature ice water (0°C, RE0), the main characteristic peak in the visible light region disappears, indicating that the dye molecules are destroyed and the dye is effectively degraded. When the temperature rises to room temperature (25°C, RE25), the curve becomes flat in just 10 minutes, indicating that the degradation effect of the strip is more obvious at this time.

[0075] 7. The amorphous-nanocrystalline alloy strip prepared in step 3 is used to catalyze the degradation of dye wastewater in a wide temperature range (0°C to 45°C). The catalytic efficiency is as follows: Figure 8 As shown in the figure, the specific experimental conditions are: pH = 3; Rh B concentration: 20ppm; tape dosage: 0.5g / L; H2O2 concentration: 1mM. Regardless of the reaction temperature of 0℃, 15℃, 25℃, 35℃ or 45℃, Mn 74 Si 15 The B7Cu1Nb3 amorphous-nanocrystalline alloy strips all showed excellent catalytic efficiency, which indicated that the Mn-based amorphous-nanocrystalline catalyst was less sensitive to temperature, and provided great potential for the catalyst to catalyze in a wider reaction temperature range.

[0076] 8. The amorphous-nanocrystalline alloy strip prepared in step 3 was used to catalyze the degradation of dye wastewater in low-temperature ice water (0°C, RE0) and room temperature (25°C, RE25). The catalytic reaction rate constants were 0.243 min -1 、0.743min -1 ,like Fig. 9 As shown. It shows that under different reaction temperature conditions, Mn 74 Si 15 B7Cu1Nb3 amorphous-nanocrystalline alloy strips all show a faster reaction rate.

[0077] 9. The amorphous-nanocrystalline alloy strip prepared in step 3 is used to catalyze the degradation of dye wastewater under different temperature environments. The catalytic activation energy is as follows: Fig.10 As shown. Mn is calculated 74 Si 15 The activation energy Ea of B7Cu1Nb3 amorphous nanocrystalline ribbon is 32.99 kJ / mol, which is much lower than the activation energy of most crystals (60-250 kJ / mol). This means that when the amorphous ribbon is catalytically degraded at low temperature, the energy barrier to be overcome is small, thus making the reaction have sufficient conditions to proceed.

[0078] 9. Repeat the experiment on the amorphous-nanocrystalline alloy strip prepared in step 3 in low temperature ice water (0°C, RE0) and room temperature (25°C, RE25). Fig.11 After the first six cycles, Mn 74 Si 15 The degradation rate of B7Cu1Nb3 amorphous nanocrystalline ribbon can still reach more than 80%, indicating that the ribbon has good repeatability. It can still maintain a high degree of reusability at different temperatures, which makes the ribbon more industrially practical.

[0079] In summary, by controlling the rotation speed of the copper roller and the aperture size of the quartz tube port, multi-element manganese-based amorphous alloy or manganese-based amorphous nanocrystalline composite structure alloy strip is directly prepared. In a wide reaction temperature range, the prepared amorphous alloy has a relatively excellent catalytic degradation ability for RhB dye wastewater. In addition, unlike the traditional method of preparing nanocrystals by annealing, the method of directly precipitating different phases on the amorphous matrix by controlling the rotation speed of the copper roller and the aperture size of the quartz tube port, the prepared amorphous-nanocrystalline dual-phase structure material has a bright surface, is not easy to oxidize, and has a stable structure. At the same time, it was found that the prepared Mn 74 Si 15 B7Cu1Nb3 amorphous nanocrystalline ribbons still maintain good catalytic properties in a wider temperature range (0℃~45℃). This makes manganese amorphous / nanocrystalline materials have extremely high research value and practical application value in the field of catalysis.

[0080] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.

Claims

1. A manganese-based amorphous alloy, characterized in that: The chemical formula of the manganese-based amorphous alloy is: Mn bas Si x1 B x2 P y M z ; In the general formula, Mn bas It represents an alloy system based on Mn, whose atomic mole number bas≥50, 10≤x1<30, 2≤x2<20, 0≤y<10, 0≤z<20, bas+x1+x2+y+z=100; M is selected from one or more of Cu, Nb, Fe, Mo, Ni and Co.

2. The manganese-based amorphous alloy according to claim 1, characterized in that: The M is selected from one of Cu, Nb, Ni, Mo and Fe.

3. The manganese-based amorphous alloy according to claim 1, characterized in that: The M is Fe and Cu existing simultaneously.

4. The manganese-based amorphous alloy according to claim 1, characterized in that: The M is Cu and Mo existing simultaneously.

5. The manganese-based amorphous alloy according to claim 1, characterized in that: The M is Cu and Nb existing simultaneously.

6. The manganese-based amorphous alloy according to claim 1, characterized in that: The chemical formula of the manganese-based amorphous alloy is Mn 67 Si 12 B 11 Fe 10 , Mn 69 Si 12 B 11 Fe8、Mn 71 Si 12 B 11 Fe6、Mn 73 Si 12 B 11 Fe4、Mn 74 Si 15 One of B7Cu1Nb3.

7. A method for preparing the manganese-based amorphous alloy according to any one of claims 1 to 6, characterized in that: The following steps are involved: (1) mixing raw materials according to the ratio of the manganese-based amorphous alloy, and then smelting to obtain a master alloy ingot; (2) The master alloy ingot is crushed and placed in a quartz tube, and an amorphous alloy strip is prepared by a strip spinning machine. The rotation speed of the copper roller and the aperture size of the quartz tube port are controlled to prepare the master alloy ingot into a manganese-based amorphous alloy.

8. The method for preparing a manganese-based amorphous alloy according to claim 7, characterized in that: In step (2), the port aperture of the quartz tube is 0.1-0.6 mm, and the linear speed of the copper roller is 40-60 m / s.

9. Use of the manganese-based amorphous alloy according to any one of claims 1 to 6 and / or the manganese-based amorphous alloy prepared by the preparation method according to any one of claims 7 to 8 in catalytic degradation of dye wastewater.

10. A method for treating dye wastewater, characterized in that: The method comprises the following steps: using the manganese-based amorphous alloy described in any one of claims 1 to 6 and / or the manganese-based amorphous alloy prepared by the preparation method described in any one of claims 7 to 8 as a catalyst, adding it to the dye wastewater to be treated, adding H2O2, stirring, and achieving pollutant degradation.