Catalyst for enhancing oxidation of benzyl alcohol as well as preparation method and application of catalyst
By introducing Pd and Bimetals on the surface of Bi4TaO8Cl, the Pd-Bi-Bi4TaO8Cl catalyst is formed, and the existing bismuth-based photocatalysts are solved, the catalytic efficiency and selectivity of benzyl alcohol oxidation are improved, and the secondary Product generation and production costs improve the efficiency and economicality of industrial applications.
Patent Information
- Application Number
- CN202411140735.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-20
AI Technical Summary
The existing bismuth-based photocatalysts have insufficient activity and stability during the oxidation process of benzyl alcohol, resulting in low catalytic efficiency and high by-product generation, affecting the economic and efficiency of industrial applications.
By introducing Pd and Bimetallic on the surface of Bi4TaO8Cl, it is combined with polyvinylpyrrolidone and NaBH4/PdCl2 by a specific preparation method to form a Pd-Bi-Bi4TaO8Cl catalyst, which improves catalytic activity and stability.
It significantly improves the oxidation reaction rate of benzyl alcohol and the selectivity of catalysts, reduces by-product generation, reduces production costs and energy consumption, and improves the efficiency and economic benefits of industrial applications.
Smart Images

Figure CN119016072A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of photocatalytic oxidation, and specifically relates to a catalyst for enhancing the oxidation of benzyl alcohol, and a preparation method and application thereof. Background Art
[0002] The selective conversion process of aromatic alcohols is a key functional group conversion process in organic synthesis and an important organic chemical reaction in modern technology and fine chemicals. Benzaldehyde corresponding to aromatic alcohols such as benzyl alcohol is the most commonly used chemical raw material and can be widely used in technical fields such as dyes, medicines and fragrances. The classic industrial production of benzaldehyde is to obtain benzyl chloride by chlorination of toluene, and then hydrolyze to obtain benzaldehyde. Although the process is simple to operate and the output of benzaldehyde is large, a large amount of corrosive products will be produced during the production process, causing serious corrosion to the equipment. The preparation of benzaldehyde by photocatalytic selective oxidation of benzyl alcohol can be carried out under mild conditions using economical and clean solar energy, and has great prospects.
[0003] In recent years, bismuth-based composite oxide photocatalysts have attracted great interest from researchers due to their unique electronic structure, excellent visible light absorption capacity and high organic matter degradation ability. However, due to their own structural and functional defects, the photocatalytic activity and stability of reported bismuth-based photocatalysts still need to be improved. Summary of the invention
[0004] In view of the above-mentioned shortcomings of the prior art, the present invention provides a catalyst for enhancing the oxidation of benzyl alcohol and a preparation method and application thereof.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] A method for preparing a catalyst for enhancing the oxidation of benzyl alcohol comprises the following steps:
[0007] (1) dissolving bismuth nitrate in ethylene glycol to obtain solution A; dissolving potassium chloride in water to obtain solution B; pouring solution B into solution A and stirring at room temperature, washing, drying and collecting the precipitate to obtain BiOCl;
[0008] (2) Grind and mix BiOCl, Bi2O3, Ta2O5, KCl and NaCl, and then calcine in a muffle furnace. After cooling, add the obtained product into water, stir at room temperature, wash and dry the precipitate to obtain Bi4TaO8Cl;
[0009] (3) Dissolve Bi4TaO8Cl and polyvinyl pyrrolidone in water, then add NaBH4 and PdCl2, stir, wash and dry to obtain Pd-Bi-Bi4TaO8Cl.
[0010] As a preferred embodiment of the present invention, the concentration of bismuth nitrate in the A solution is 0.2-0.6 mol / L, the concentration of KCl in the B solution is 0.2-0.6 mol / L; and the volume ratio of the A solution to the B solution is 1:1.
[0011] As a preferred embodiment of the present invention, the molar ratio of BiOCl, Bi2O3, Ta2O5, KCl and NaCl is (2-5):(3-8):(1-3):(150-180):(180-220).
[0012] As a preferred embodiment of the present invention, the calcination temperature is 600-800°C and the calcination time is 8-14h.
[0013] As a preferred embodiment of the present invention, the Bi4TaO8Cl and polyvinyl pyrrolidone are dissolved in water, the concentration of Bi4TaO8Cl is 1-4 g / L, and the concentration of polyvinyl pyrrolidone is 3-10 g / L.
[0014] As a preferred embodiment of the present invention, the mass ratio of Bi4TaO8Cl, NaBH4 and PdCl2 is (0.05-0.15):(0.01-0.05):(0.001-0.005).
[0015] The present invention also claims protection for the catalyst for enhancing benzyl alcohol oxidation prepared by the preparation method of the catalyst for enhancing benzyl alcohol oxidation.
[0016] The present invention also claims the use of the catalyst for enhancing benzyl alcohol oxidation in photocatalytic benzyl alcohol oxidation.
[0017] Compared with the prior art, the present invention has the following beneficial effects: the present invention accelerates the oxidation reaction rate of benzyl alcohol by introducing Pd and Bi bimetallics on the surface of Bi4TaO8Cl, thereby improving the catalytic efficiency and stability. Moreover, the catalyst has extremely high selectivity for benzaldehyde during the oxidation of benzyl alcohol, effectively reducing the generation of by-products. In addition, the high efficiency and stability of the catalyst of the present invention can significantly reduce production costs, reduce energy consumption, and improve production efficiency in industrial applications, thus having obvious economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The XRD patterns of the catalysts prepared in Example 1 and Comparative Examples 1 and 2 are shown.
[0019] Figure 2 is a morphology image of the material prepared in Example 1; a is a SEM image; b is a HRTEM image; c is an EDX element mapping image.
[0020] Figure 3The benzyl alcohol conversion and benzaldehyde selectivity performance diagram of the catalysts prepared in Example 1 and Comparative Examples 1 and 2.
[0021] Figure 4 DRS diagrams of the catalysts prepared in Example 1 and Comparative Examples 1 and 2.
[0022] Figure 5 Benzyl alcohol conversion and benzaldehyde selectivity performance diagram of the catalysts prepared in Examples 1 to 5.
[0023] Figure 6 This is a test graph of the cyclic stability of photocatalytic selective benzyl alcohol oxidation under the same reaction conditions in Example 1.
[0024] In the figure, BTC is the Bi4TaO8Cl catalyst prepared in Comparative Example 1, Bi-BTC is the Bi-Bi4TaO8Cl catalyst prepared in Comparative Example 2, and Pd-Bi-BTC is the Pd-Bi-Bi4TaO8Cl catalyst prepared in Example 1. DETAILED DESCRIPTION
[0025] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.
[0026] Example 1
[0027] A method for preparing a catalyst for enhancing the oxidation of benzyl alcohol comprises the following steps:
[0028] (1) Dissolve 10 mmol of bismuth nitrate (Bi(NO3)3·5H2O) in 25 mL of ethylene glycol to obtain solution A; dissolve 10 mmol of potassium chloride (KCl) in 25 mL of deionized water to obtain solution B; pour solution B into solution A, stir at room temperature for 1 hour, and then stand to separate the layers. Pour out the supernatant, wash the obtained suspension thoroughly with distilled water and anhydrous ethanol three times, filter and separate to remove other ions, and then dry at 80°C overnight to collect BiOCl.
[0029] (2) 0.5 mmol BiOCl, 0.75 mmol Bi2O3, 0.25 mmol Ta2O5, 40 mmol KCl and 50 mmol NaCl were ground and mixed, and then calcined in a muffle furnace at 700°C for 14 h. After the product was cooled, it was added into 60 mL deionized water, stirred at room temperature for 1 h, and then allowed to stand for stratification. The supernatant was poured out, and the obtained suspension was thoroughly washed three times with distilled water and anhydrous ethanol, respectively, filtered and separated, and then dried at 80°C overnight to obtain Bi4TaO8Cl nanosheets.
[0030] (3) 0.10 g Bi4TaO8Cl and 0.20 g polyvinyl pyrrolidone were dissolved in 40 mL deionized water, and then 0.025 g NaBH4 and 0.003 g PdCl2 were added and stirred at a rate of 350 r / min for 0.5 h. The mixture was washed three times with 60 °C deionized water and ethanol respectively, filtered and separated, and then dried at 80 °C overnight to obtain the Pd-Bi-Bi4TaO8Cl bimetallic site photocatalyst.
[0031] Figure 2 The scanning electron microscope (SEM), transmission electron microscope (TEM) and energy dispersive x-ray spectroscopy (EDX) element mapping diagrams of the bimetallic site photocatalyst prepared in Example 1 are shown in FIG. Figure 2 In a, it can be seen that the Pd-Bi-Bi4TaO8Cl bimetallic site photocatalyst consists of well-grown square nanoplates with an appropriate amount of nanodots evenly distributed on the surface; Figure 2 Obvious lattice fringes are shown in b. The lattice spacing on the nanosheet is 0.386 nm, corresponding to the (110) crystal plane of Bi4TaO8Cl. The lattice spacings of the supported particles are 0.227 nm and 0.237 nm, corresponding to the (111) crystal plane of Pd and the (104) crystal plane of Bi, respectively. Figure 2 c It can be seen that Pd and Bi elements are evenly distributed on the Bi4TaO8Cl carrier.
[0032] Example 2
[0033] A method for preparing a catalyst for enhancing the oxidation of benzyl alcohol comprises the following steps:
[0034] (1) Dissolve 5 mmol bismuth nitrate (Bi(NO3)3·5H2O) in 25 mL ethylene glycol to obtain solution A; dissolve 5 mmol potassium chloride (KCl) in 25 mL deionized water to obtain solution B; pour solution B into solution A, stir at room temperature for 1 hour, and then stand to separate the layers, discard the supernatant, and wash the resulting suspension thoroughly with distilled water and anhydrous ethanol three times, respectively, and filter and separate to remove other ions, and then dry at 80°C overnight to collect BiOCl.
[0035] (2) 0.5 mmol BiOCl, 0.75 mmol Bi2O3, 0.25 mmol Ta2O5, 40 mmol KCl and 50 mmol NaCl were ground and mixed, and then calcined in a muffle furnace at 600°C for 12 h. After the product was cooled, it was added into 100 mL deionized water, stirred at room temperature for 3 h, and then allowed to stand for stratification. The supernatant was poured out, and the obtained suspension was thoroughly washed three times with distilled water and anhydrous ethanol, respectively, filtered and separated, and then dried at 80°C overnight to obtain Bi4TaO8Cl nanosheets.
[0036] (3) 0.05 g Bi4TaO8Cl and 0.40 g polyvinyl pyrrolidone were dissolved in 40 mL deionized water, and then 0.05 g NaBH4 and 0.001 g PdCl2 were added and stirred at a rate of 450 r / min for 2 h. The mixture was washed three times with 60°C deionized water and ethanol respectively, filtered and separated, and then dried at 80°C overnight to obtain a 1% Pd-Bi-Bi4TaO8Cl bimetallic site photocatalyst.
[0037] Example 3
[0038] A method for preparing a catalyst for enhancing the oxidation of benzyl alcohol comprises the following steps:
[0039] (1) Dissolve 15 mmol bismuth nitrate (Bi(NO3)3·5H2O) in 25 mL ethylene glycol to obtain solution A; dissolve 15 mmol potassium chloride (KCl) in 25 mL deionized water to obtain solution B; pour solution B into solution A, stir at room temperature for 1 hour, and then stand to separate the layers, discard the supernatant, and wash the resulting suspension thoroughly with distilled water and anhydrous ethanol three times, respectively, and filter and separate to remove other ions, and then dry at 80°C overnight to collect BiOCl.
[0040] (2) 0.5 mmol BiOCl, 0.75 mmol Bi2O3, 0.25 mmol Ta2O5, 40 mmol KCl and 50 mmol NaCl were ground and mixed, and then calcined in a muffle furnace at 800°C for 10 h. After the product was cooled, it was added into 100 mL deionized water, stirred at room temperature for 3 h, and then allowed to stand for stratification. The supernatant was poured out, and the obtained suspension was thoroughly washed three times with distilled water and anhydrous ethanol, respectively, filtered and separated, and then dried at 80°C overnight to obtain Bi4TaO8Cl nanosheets.
[0041] (3) 0.15 g Bi4TaO8Cl and 0.12 g polyvinyl pyrrolidone were dissolved in 40 mL deionized water, and then 0.01 g NaBH4 and 0.002 g PdCl2 were added and stirred at a rate of 250 r / min for 1 h. The mixture was washed three times with 60°C deionized water and ethanol respectively, filtered and separated, and then dried at 80°C overnight to obtain a 2% Pd-Bi-Bi4TaO8Cl bimetallic site photocatalyst.
[0042] Example 4
[0043] (1) Dissolve 10 mmol of bismuth nitrate (Bi(NO3)3·5H2O) in 25 mL of ethylene glycol to obtain solution A; dissolve 10 mmol of potassium chloride (KCl) in 25 mL of deionized water to obtain solution B; pour solution B into solution A, stir at room temperature for 1 hour, and then stand to separate the layers. Pour out the supernatant, wash the obtained suspension thoroughly with distilled water and anhydrous ethanol three times, filter and separate to remove other ions, and then dry at 80°C overnight to collect BiOCl.
[0044] (2) 0.5 mmol BiOCl, 0.75 mmol Bi2O3, 0.25 mmol Ta2O5, 40 mmol KCl and 50 mmol NaCl were ground and mixed, and then calcined in a muffle furnace at 700°C for 9 h. After the product was cooled, it was added into 60 mL deionized water, stirred at room temperature for 1 h, and then allowed to stand for stratification. The supernatant was poured out, and the obtained suspension was thoroughly washed three times with distilled water and anhydrous ethanol, respectively, filtered and separated, and then dried at 80°C overnight to obtain Bi4TaO8Cl nanosheets.
[0045] (3) 0.10 g Bi4TaO8Cl and 0.20 g polyvinyl pyrrolidone were dissolved in 40 mL deionized water, and then 0.025 g NaBH4 and 0.004 g PdCl2 were added and stirred at a rate of 350 r / min for 0.5 h. The mixture was washed three times with 60°C deionized water and ethanol respectively, filtered and separated, and then dried at 80°C overnight to obtain a 4% Pd-Bi-Bi4TaO8Cl bimetallic site photocatalyst.
[0046] Example 5
[0047] (1) Dissolve 10 mmol of bismuth nitrate (Bi(NO3)3·5H2O) in 25 mL of ethylene glycol to obtain solution A; dissolve 10 mmol of potassium chloride (KCl) in 25 mL of deionized water to obtain solution B; pour solution B into solution A, stir at room temperature for 1 hour, and then stand to separate the layers. Pour out the supernatant, wash the obtained suspension thoroughly with distilled water and anhydrous ethanol three times, filter and separate to remove other ions, and then dry at 80°C overnight to collect BiOCl.
[0048] (2) 0.5 mmol BiOCl, 0.75 mmol Bi2O3, 0.25 mmol Ta2O5, 40 mmol KCl and 50 mmol NaCl were ground and mixed, and then calcined in a muffle furnace at 700°C for 8 h. After the product was cooled, it was added into 60 mL deionized water, stirred at room temperature for 1 h, and then allowed to stand for stratification. The supernatant was poured out, and the obtained suspension was thoroughly washed three times with distilled water and anhydrous ethanol, respectively, filtered and separated, and then dried at 80°C overnight to obtain Bi4TaO8Cl nanosheets.
[0049] (3) 0.10 g Bi4TaO8Cl and 0.20 g polyvinyl pyrrolidone were dissolved in 40 mL deionized water, and then 0.025 g NaBH4 and 0.005 g PdCl2 were added and stirred at a rate of 350 r / min for 0.5 h. The mixture was washed three times with 60°C deionized water and ethanol respectively, filtered and separated, and then dried at 80°C overnight to obtain a 5% Pd-Bi-Bi4TaO8Cl bimetallic site photocatalyst.
[0050] Comparative Example 1
[0051] A method for preparing a Bi4TaO8Cl catalyst comprises the following steps:
[0052] (1) Dissolve 10 mmol of bismuth nitrate (Bi(NO3)3·5H2O) in 25 mL of ethylene glycol to obtain solution A; dissolve 10 mmol of potassium chloride (KCl) in 25 mL of deionized water to obtain solution B; pour solution B into solution A, stir at room temperature for 1 hour, and then stand to separate the layers. Pour out the supernatant, wash the obtained suspension thoroughly with distilled water and anhydrous ethanol three times, filter and separate to remove other ions, and then dry at 80°C overnight to collect BiOCl.
[0053] (2) 0.5 mmol BiOCl, 0.75 mmol Bi2O3, 0.25 mmol Ta2O5, 40 mmol KCl and 50 mmol NaCl were ground and mixed, and then calcined in a muffle furnace at 700°C for 14 h. After the product was cooled, it was added into 60-100 mL deionized water, stirred at room temperature for 1 h, and then allowed to stand for stratification. The supernatant was poured out, and the obtained suspension was thoroughly washed three times with distilled water and anhydrous ethanol respectively, filtered and separated, and then dried at 80°C overnight to obtain the Bi4TaO8Cl photocatalyst.
[0054] Comparative Example 2
[0055] A method for preparing a Bi-Bi4TaO8Cl catalyst comprises the following steps:
[0056] (1) Dissolve 10 mmol of bismuth nitrate (Bi(NO3)3·5H2O) in 25 mL of ethylene glycol to obtain solution A; dissolve 10 mmol of potassium chloride (KCl) in 25 mL of deionized water to obtain solution B; pour solution B into solution A, stir at room temperature for 1 hour, and then stand to separate the layers. Pour out the supernatant, wash the obtained suspension thoroughly with distilled water and anhydrous ethanol three times, filter and separate to remove other ions, and then dry at 80°C overnight to collect BiOCl.
[0057] (2) 0.5 mmol BiOCl, 0.75 mmol Bi2O3, 0.25 mmol Ta2O5, 40 mmol KCl and 50 mmol NaCl were ground and mixed, and then calcined in a muffle furnace at 700°C for 14 h. After the product was cooled, it was added into 60-100 mL deionized water, stirred at room temperature for 1 h, and then allowed to stand for stratification. The supernatant was poured off, and the obtained suspension was thoroughly washed three times with distilled water and anhydrous ethanol respectively, filtered and separated, and then dried at 80°C overnight to obtain Bi4TaO8Cl nanosheets.
[0058] (3) 0.10 g Bi4TaO8Cl and 0.20 g polyvinyl pyrrolidone were dissolved in 40 mL deionized water, and then 0.025 g NaBH4 was added and stirred at a rate of 350 r / min for 0.5 h. The mixture was washed three times with 60-80 °C deionized water and ethanol respectively, filtered and separated, and then dried at 80 °C overnight to obtain the Bi-Bi4TaO8Cl single metal site photocatalyst.
[0059] Figure 1 The X-ray diffraction diagrams of the photocatalysts prepared in Example 1, Comparative Example 1 and Comparative Example 2 show the successful preparation of Bi4TaO8Cl, Bi-Bi4TaO8Cl and Pd-Bi-Bi4TaO8Cl. As the materials are modified, the peak intensity changes, indicating the change of the material properties. However, due to the low crystallinity of the Pd element, no obvious diffraction peaks appear.
[0060] Figure 4 It is the UV-vis DRS diagram of the photocatalysts prepared in Example 1, Comparative Example 1 and Comparative Example 2. It can be seen from the figure that the absorption edge of Pd-Bi-Bi4TaO8Cl prepared in Example 1 is significantly red-shifted relative to that in Comparative Example 1 and Comparative Example 2, indicating that the Pd-Bi bimetallic site significantly improves the light capture ability of the material.
[0061] Effect example
[0062] The catalysts prepared in the examples and comparative examples were used for the photocatalytic oxidation of benzyl alcohol, and the specific steps were as follows:
[0063] (1) Take 20 mg of the catalyst and place it in a 50 mL photoreaction tube. Use condensed water to control the reaction temperature at room temperature.
[0064] (2) Pipette 21 μL of benzyl alcohol (BA) and 2 mL of benzene trifluoride (BTF) into a test tube, ultrasonicate them in an ultrasonic cleaner for about 5 min to make them evenly mixed, and finally stir them for 30 min in a dark environment to allow the catalyst and BA to reach an adsorption-desorption equilibrium state.
[0065] (3) Before the reaction started, O2 was blown into the solution for 20 min to saturate the O2 concentration. A 300 W xenon lamp equipped with a 400 nm cutoff filter was used as the simulated solar light source. After continuous irradiation for 4 h, the suspension was collected and filtered through a 0.45 μm filter to remove the catalyst.
[0066] (4) The filtrate was analyzed by high performance liquid chromatography (HPLC) to calculate the conversion rate of BA and the selectivity of benzaldehyde (BD). The results are shown in Table 1.
[0067] Table 1
[0068] Selectivity of benzaldehyde / % Conversion rate of benzyl alcohol / % Example 1 98.78 86.88 Example 2 97.36 56.88 Example 3 97.72 76.88 Example 4 98.01 81.88 Example 5 98.84 69.88 Comparative Example 1 97.70 24.12 Comparative Example 2 98.10 39.37
[0069] according to Figure 3 , Figure 5 As shown in Table 1, the selective oxidation ability of the bimetallic site photocatalyst prepared in Example 1 is significantly enhanced. After four hours of illumination, its conversion rate is the highest, which is 86.88%, and the selectivity reaches 98.78%. Examples 2 to 5 show that the selectivity of Pd-Bi-BTC photocatalysts with different Pd contents has decreased. The selective oxidation ability of the Bi4TaO8Cl catalyst prepared in Comparative Example 1 and the Bi-Bi4TaO8Cl single metal site photocatalyst prepared in Comparative Example 2 has greatly decreased, indicating that the introduction of bimetallic sites has a greater promoting effect on performance improvement.
[0070] The stability test of the photocatalytic selective oxidation of benzyl alcohol by the bimetallic site photocatalyst prepared in Example 1 is as follows Figure 6 As shown, multiple cycle experiments were carried out under the same conditions, and it can be seen that the Pd-Bi-BTC photocatalyst has good stability. After four cycles of photocatalytic selective oxidation of benzyl alcohol experiments, the Pd-Bi-BTC photocatalyst still maintained considerable performance. Its good stability makes it have certain potential for large-scale application, mainly because the addition of Pb enhances the structural stability and catalytic performance stability of the Bi-BTC photocatalyst.
[0071] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a catalyst for enhancing the oxidation of benzyl alcohol, characterized in that: The steps include: (1) dissolving bismuth nitrate in ethylene glycol to obtain solution A; dissolving potassium chloride in water to obtain solution B; pouring solution B into solution A and stirring at room temperature, washing, drying and collecting the precipitate to obtain BiOCl; (2) Grind and mix BiOCl, Bi2O3, Ta2O5, KCl and NaCl, then calcine, cool the obtained product, add it into water, stir at room temperature, wash and dry the precipitate to obtain Bi4TaO8Cl; (3) Dissolve Bi4TaO8Cl and polyvinyl pyrrolidone in water, then add NaBH4 and PdCl2, stir, wash and dry to obtain Pd-Bi-Bi4TaO8Cl.
2. The method for preparing a catalyst for enhancing the oxidation of benzyl alcohol as claimed in claim 1, characterized in that: The concentration of bismuth nitrate in the A solution is 0.2-0.6 mol / L, the concentration of KCl in the B solution is 0.2-0.6 mol / L; the volume ratio of the A solution to the B solution is 1:
1.
3. The method for preparing a catalyst for enhancing benzyl alcohol oxidation according to claim 1, characterized in that: The molar ratio of BiOCl, Bi2O3, Ta2O5, KCl and NaCl is (2-5):(3-8):(1-3):(150-180):(180-220).
4. The method for preparing a catalyst for enhancing benzyl alcohol oxidation according to claim 1, characterized in that: The calcination temperature is 600-800°C and the calcination time is 8-14h.
5. The method for preparing a catalyst for enhancing benzyl alcohol oxidation according to claim 1, characterized in that: The Bi4TaO8Cl and polyvinyl pyrrolidone are dissolved in water, the concentration of Bi4TaO8Cl is 1-4 g / L, and the concentration of polyvinyl pyrrolidone is 3-10 g / L.
6. The method for preparing a catalyst for enhancing benzyl alcohol oxidation according to claim 1, characterized in that: The mass ratio of the Bi4TaO8Cl, NaBH4 and PdCl2 is (0.05-0.15):(0.01-0.05):(0.001-0.005).
7. The catalyst for enhancing the oxidation of benzyl alcohol prepared by the method for preparing the catalyst for enhancing the oxidation of benzyl alcohol according to any one of claims 1 to 6.
8. Use of the catalyst for enhancing benzyl alcohol oxidation as claimed in claim 7 in photocatalytic benzyl alcohol oxidation.
Citation Information
Patent Citations
Method for catalyzing benzyl alcohol to generate benzaldehyde at room temperature
CN109134228A
Silene-Aurivillius layered structure material Bi4SbO8Cl and synthesis method thereof
CN114014360A
Bi elementary substance and oxygen deficiency synergistically modified bismuth tantalum oxyhalide as well as preparation method and application thereof
CN116966919A
Water splitting apparatus using photocatalyst, and water splitting system provided with same
WO2023182282A1