High-dispersion and high-load type Mo2N catalyst as well as preparation method and application thereof
Through the combination coordination of amine carbon sources and copper molybdate and silicon sphere support, a high-load carbon-coated molybdenum nitride catalyst was prepared, which solved the problem of inactivation of non-precious metal catalysts under high temperature conditions and achieved efficient ammonia decomposition The reaction improves the stability and activity of the catalyst.
Patent Information
- Application Number
- CN202411124129.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-15
AI Technical Summary
Existing non-precious metal catalysts are prone to inactivate under high temperature conditions and the loading of active components is low, resulting in low ammonia decomposition reaction efficiency, which cannot effectively solve the need for low-temperature and efficient ammonia decomposition.
The combination coordination effect of amine carbon sources and ammonium molybdate is used to perform in situ nitriding of high-temperature inert gas to prepare a high-load carbon-coated molybdenum nitride catalyst, and the addition of silicon spheres as support dispersants is used to inhibit carbon etching. and sintering to improve the anti-sintering performance of the catalyst.
The preparation of high-dispersion and high-loaded Mo2N catalyst was achieved, with the molybdenum nitride load reaching 46.6%, the initial conversion rate of NH3 reached 99% at 550℃, and the conversion rate of 90% at 600℃ was maintained, which significantly improved ammonia. Stability and specific surface area of the decomposition reaction.
Smart Images

Figure CN119016083A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of ammonia decomposition, and in particular to a highly dispersed and highly loaded Mo2N catalyst and a preparation method and application thereof. Background Art
[0002] The greenhouse gases and solid particulate pollutants produced by fossil energy have far exceeded nature's self-purification capacity, so the development and utilization of clean energy is the key to solving environmental and energy problems.
[0003] Hydrogen energy is recognized as the most promising clean energy due to its cleanliness and high calorific value. Hydrogen fuel cells are the most effective form of utilizing hydrogen energy, which can increase the utilization rate by 40% to 50% compared with other methods. However, hydrogen has a low volume energy density and is difficult to store. With current hydrogen storage technology, whether it is stored in the form of liquid or gas, there are problems such as too large volume, too high pressure, and low safety factor. If hydrogen is stored in liquid fuel (ammonia, methanol, formic acid) in chemical form, and then released in situ through a certain catalytic reaction for use in fuel cells, the hydrogen storage problem of fuel cells can be effectively solved, allowing hydrogen fuel cells to be further developed.
[0004] In recent years, ammonia has been considered as a promising long-term large-scale energy storage carrier. First of all, industrial ammonia synthesis has a long history and mature technology, and has the conditions for large-scale industrial synthesis of ammonia. At the same time, ammonia molecules have a high H / N ratio and strong hydrogen storage capacity. In addition, ammonia molecules do not contain carbon, are easy to release hydrogen and have zero carbon emissions. Using ammonia as a hydrogen storage carrier has high hydrogen content (17.6wt%), high energy density (3000Whkg -1 ), easy liquefaction (normal temperature, 8atm), convenient storage and transportation, zero carbon emissions, non-flammability, etc., combined with the ammonia decomposition reaction to produce hydrogen, is expected to promote the development of the hydrogen energy industry and has great economic value and practical significance. Since the ammonia decomposition reaction is an endothermic reaction with an increase in the number of reaction molecules, increasing the reaction temperature is conducive to improving the reaction conversion rate, which also leads to higher energy consumption for ammonia decomposition at low temperatures. Therefore, low-temperature and high-efficiency ammonia decomposition catalysts are the key to solving the problem of high energy consumption.
[0005] At present, metal carbon / nitrides and iron, cobalt, nickel, and ruthenium-based catalysts are often used in ammonia decomposition reactions. Among them, the temperature at which non-precious metal-based catalysts such as Fe, Co, and Ni reach equilibrium conversion is generally 600 degrees or above, and the low-temperature ammonia decomposition activity is poor; precious metal ruthenium-based catalysts exhibit the best catalytic activity, but their high price limits their promotion and application. In contrast, transition metal carbon / nitrides have low cost, good thermal stability, and precious metal-like properties. They are more active in activating small molecules (CH4, NH3, CH3OH, etc.) to produce hydrogen. Among them, carbon / molybdenum nitride has excellent ammonia decomposition activity and has received widespread attention and research. CN114100661A discloses a sol-gel method for preparing Mo2N. After the reaction generates a Mo2N-MoO2 composite structure, it is heated for 30,000 hours. -1 , the ammonia decomposition conversion rate at 600℃ was 94.3%. Zheng et al. (Zheng, W., et al. (2013). Journal of the American Chemical Society, 135 (9), 3458.) studied the changes of β-Mo2C during the long-term ammonia decomposition reaction. The main reason for its deactivation was the formation of a MoN phase with a smaller surface area. Combined with the calculation results, it can be seen that the defect sites on the catalyst surface are the active centers of ammonia decomposition. Zhai et al. (Zhai, L., et al. Applied Catalysis B: Environmental, 294.) used SBA-15 to limit the dispersed Mo2N and added graphene to adjust the electronic structure to obtain a Mo2N / SBA-15 / rGO catalyst with high ammonia decomposition activity. Although the inert carrier SBA-15 is conducive to maintaining the high specific surface area of the catalyst, the problem of its transformation to the less active molybdenum phase has not yet been solved. Summary of the invention
[0006] The purpose of the present invention is to provide a highly dispersed and highly loaded Mo2N catalyst and a preparation method and application thereof. The highly dispersed and highly loaded Mo2N catalyst has the characteristics of high activity and high stability, which makes up for the shortcomings of low loading of active components on existing non-precious metal catalysts and deactivation of the catalyst due to sintering and phase transition under high temperature conditions.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The invention provides a highly dispersed and highly loaded Mo2N catalyst, which comprises raw materials in the following mass molar ratio: silicon source: amine organic matter: molybdenum source = 0-20 g: 10 mmol: 1-20 mmol.
[0009] Preferably, the silicon source includes one of silica sol, silica balls, and amorphous silica; the amine-containing organic matter includes one of p-phenylenediamine and hexamethylenetetramine; and the molybdenum source includes one of ammonium paramolybdate, phosphomolybdic acid, and sodium molybdate.
[0010] The present invention also provides a method for preparing a highly dispersed and highly loaded Mo2N catalyst, comprising the following steps:
[0011] (1) dissolving a silicon source in deionized water, adding hydrochloric acid for pre-acidification treatment, and sequentially adding an amine-containing organic solution and a molybdenum source solution, and mixing them uniformly to obtain a mixed system;
[0012] (2) adjusting the pH value of the mixed system, stirring and aging, separating and precipitating, washing, and drying to obtain a precursor;
[0013] (3) The precursor is placed in flowing argon gas and heated for nitridation to obtain a highly dispersed and highly loaded Mo2N catalyst.
[0014] Preferably, in step (1), the concentration of the hydrochloric acid is 1 mol / L, and the mass volume ratio of the silicon source to the hydrochloric acid is 0-10 g:0-2 mL.
[0015] Preferably, in step (2), the pH value is 1 to 5, and the stirring aging time is 2 to 5 hours.
[0016] Preferably, the method of heating nitriding in step (3) is:
[0017] The temperature was raised to 600-800°C at a rate of 5-20°C / min and kept at that temperature for 1-4h, then cooled to room temperature and passivated in 1% O2 / Ar for 10-12h.
[0018] The present invention also provides an application of a highly dispersed and highly loaded Mo2N catalyst in an ammonia decomposition reaction.
[0019] Preferably, the highly dispersed and highly loaded Mo2N catalyst needs to be pretreated before ammonia decomposition to produce hydrogen; the pretreatment temperature is 350-550°C; the heating rate during pretreatment is 5-15°C / min; the pretreatment time is 30-60min; and the pretreatment is carried out under a H2 / N2 atmosphere.
[0020] The beneficial effects of the present invention compared with the prior art are:
[0021] (1) On the one hand, the present invention utilizes the binding and coordination effect of amine carbon sources on ammonium molybdate, and uses high-temperature inert gas in-situ nitridation to prepare a high-load carbon-coated molybdenum nitride catalyst, wherein the molybdenum nitride loading is as high as 46.6%. The obtained highly dispersed and highly loaded Mo2N catalyst has an initial conversion rate of about 99% for NH3 at 550°C.
[0022] (2) On the other hand, since the amorphous carbon formed by the pyrolysis of organic matter is easily etched and sintered in the ammonia decomposition reaction, which reduces the activity of the ammonia decomposition reaction, the present invention adds silicon balls with supporting and dispersing functions to the molybdenum nitride-carbon structure, which effectively inhibits the aggregation of molybdenum caused by carbon etching and improves the overall anti-sintering performance of the catalyst, so that the catalyst has excellent ammonia decomposition stability, which makes up for the shortcomings of the existing non-precious metal catalysts, such as low active component loading and catalyst deactivation caused by sintering and phase transition under high temperature conditions.
[0023] In the process of preparing Mo2N catalyst, Mo was successfully coated and dispersed by carbon source and in-situ nitrided to Mo2N. When the catalyst was used in the ammonia decomposition hydrogen production reaction, the added carrier silica beads significantly improved the stability, making the conversion rate at 600℃, WHSV = 90,000mL / g / h about 90%, and basically remained unchanged within 200h. In addition, the specific surface area of Mo2N catalyst with added SiO2 beads reached 178.7m 2 / g, compared with the sample without silicon balls (132.9m 2 / g) has been significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0025] Figure 1 XRD spectra of Mo2N catalysts prepared in Example 1, Example 5, Example 6 and Comparative Example 1;
[0026] Figure 2 N2 adsorption and desorption curves of Mo2N catalysts prepared in Example 1, Example 5, Example 6, and Comparative Example 1;
[0027] Figure 3 The pore size distribution diagram of the Mo2N catalyst prepared in Example 1, Example 5, Example 6, and Comparative Example 1;
[0028] Figure 4 The transmission electron microscope image and particle size statistics of the catalyst Mo2N@C(HM) prepared in Example 1;
[0029] Figure 5 This is a high-magnification transmission electron microscopy image of the catalyst Mo2N@C (HM) prepared in Example 1;
[0030] Figure 6Transmission electron microscope image and particle size statistics of the catalyst Mo2N@C(pP) prepared in Example 5;
[0031] Figure 7 This is a high-magnification transmission electron microscopy image of the catalyst Mo2N@C(pP) prepared in Example 5;
[0032] Figure 8 Transmission electron microscope image and particle size statistics of the catalyst Mo2N@C / SiO2 prepared in Example 6;
[0033] Fig. 9 This is a high-magnification transmission electron microscopy image of the catalyst Mo2N@C / SiO2 prepared in Example 6;
[0034] Fig.10 The transmission electron microscope image and particle size statistics of the catalyst Mo2N@C(oP) prepared in Comparative Example 1;
[0035] Fig.11 This is a high-magnification transmission electron microscopy image of the catalyst Mo2N@C(oP) prepared in Comparative Example 1;
[0036] Fig.12 The catalytic performance results of the Mo2N catalysts prepared in Example 1, Example 5, Example 6, and Comparative Example 1 in Test Example 1 are shown in FIG.
[0037] Fig.13 The catalytic performance results of the Mo2N catalysts prepared in Example 2, Example 3, Example 4, and Example 7 in Test Example 1 are shown;
[0038] Fig.14 This is a graph showing the stability evaluation results of the Mo2N catalysts prepared in Example 1, Example 6, and Example 7 in Experimental Example 2. DETAILED DESCRIPTION
[0039] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0040] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0041] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0042] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0043] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0044] The present invention provides a method for preparing a highly dispersed and highly loaded Mo2N catalyst, comprising the following steps:
[0045] (1) dissolving a silicon source in deionized water, adding hydrochloric acid for pre-acidification treatment, and sequentially adding an amine-containing organic solution and a molybdenum source solution, and mixing them uniformly to obtain a mixed system;
[0046] Preferably, the silicon source includes one of silica sol, silica spheres, and amorphous silica, more preferably silica sol;
[0047] Preferably, the amine-containing organic compound includes one of p-phenylenediamine and hexamethylenetetramine, more preferably hexamethylenetetramine;
[0048] Preferably, the molybdenum source includes one of ammonium paramolybdate, phosphomolybdic acid, and sodium molybdate, more preferably ammonium paramolybdate;
[0049] Preferably, the silicon source: amine organic matter: molybdenum source = 0-20 g: 10 mmol: 1-4 mmol, more preferably 10 g: 10 mmol: 3-4 mmol;
[0050] The concentration of the hydrochloric acid is 1 mol / L, and the mass volume ratio of the silicon source to the hydrochloric acid is 0-10 g:0-2 mL.
[0051] (2) adjusting the pH value of the mixed system, stirring and aging, separating and precipitating, washing, and drying to obtain a precursor;
[0052] Preferably, the pH value is 1 to 5, more preferably 2.3 to 2.8;
[0053] Preferably, the stirring aging time is 2 to 5 hours, more preferably 2 to 4 hours; the heating stirring temperature is 20 to 70°C.
[0054] (3) placing the precursor in flowing argon gas and heating it for nitridation to obtain a highly dispersed and highly loaded Mo2N catalyst;
[0055] Preferably, the method of heating nitriding is:
[0056] The temperature is raised to 600-800°C at a rate of 5-20°C / min and kept at this temperature for 1-4h, then cooled to room temperature and passivated in 1% O2 / Ar for 10-12h; more preferably, the temperature is raised at a rate of 10-15°C / min and the holding time is 2-3h.
[0057] Example 1
[0058] Example 1 of the present invention provides a method for preparing a highly dispersed and highly loaded Mo2N catalyst Mo2N@C(HM), which specifically comprises the following steps:
[0059] (1) 1.40 g of hexamethylenetetramine (HM) was dissolved in 50 ml of deionized water to obtain a hexamethylenetetramine solution after complete dissolution, and 3.69 g of ammonium paramolybdate was dissolved in 50 ml of deionized water to obtain an ammonium paramolybdate solution after complete dissolution.
[0060] (2) In 50 ml of deionized water, add 1 ml of 1 M hydrochloric acid, then add the hexamethylenetetramine solution, mix well, and then slowly drop the ammonium paramolybdate solution, mix well to obtain a mixed system.
[0061] (3) The pH value of the mixed system was adjusted to 2.5 with 1 M hydrochloric acid, and the mixture was stirred for 2.5 h for aging. After aging, the precipitate was separated by centrifugation. The precipitate was washed three times with water and ethanol, and then dried under vacuum at 60° C. for 10 h to obtain a precursor.
[0062] (4) The precursor was placed in a tube furnace, heated to 650°C at a heating rate of 5°C / min under a flowing argon atmosphere, and maintained at 650°C for 2 h for nitridation to obtain a highly dispersed and highly loaded Mo2N catalyst Mo2N@C (HM) with hexamethylenetetramine as the dispersed carbon source.
[0063] The Mo2N@C(HM) prepared in Example 1 was subjected to XRD test, and its N2 adsorption and desorption effect, pore size, particle size, and transmission electron microscopy were tested. The results are as follows: Figures 1 to 5 shown.
[0064] Example 2
[0065] Example 2 of the present invention provides a method for preparing a highly dispersed and highly loaded Mo2N catalyst Mo2N-1@C(HM), which specifically comprises the following steps:
[0066] (1) 1.40 g of hexamethylenetetramine (HM) was dissolved in 50 ml of deionized water to obtain a hexamethylenetetramine solution after complete dissolution, and 1.23 g of ammonium paramolybdate was dissolved in 50 ml of deionized water to obtain an ammonium paramolybdate solution after complete dissolution.
[0067] (2) In 50 ml of deionized water, add 1 ml of 1 M hydrochloric acid, then add the hexamethylenetetramine solution, mix well, and then slowly drop the ammonium paramolybdate solution, mix well to obtain a mixed system.
[0068] (3) The pH value of the mixed system was adjusted to 2.5 with 1 M hydrochloric acid, and the mixture was stirred for 2.5 h for aging. After aging, the precipitate was separated by centrifugation. The precipitate was washed three times with water and ethanol, and then dried under vacuum at 60° C. for 10 h to obtain a precursor.
[0069] (4) The precursor was placed in a tube furnace, heated to 650°C at a heating rate of 5°C / min under a flowing argon atmosphere, and maintained at 650°C for 2 h for nitridation to obtain a highly dispersed and highly loaded Mo2N catalyst Mo2N-1@C (HM) with hexamethylenetetramine as the dispersed carbon source.
[0070] Example 3
[0071] Example 3 of the present invention provides a method for preparing a highly dispersed and highly loaded Mo2N catalyst Mo2N-2@C (HM), which specifically comprises the following steps:
[0072] (1) 1.40 g of hexamethylenetetramine (HM) was dissolved in 50 ml of deionized water to obtain a hexamethylenetetramine solution after complete dissolution, and 2.46 g of ammonium paramolybdate was dissolved in 50 ml of deionized water to obtain an ammonium paramolybdate solution after complete dissolution.
[0073] (2) In 50 ml of deionized water, add 1 ml of 1 M hydrochloric acid, then add the hexamethylenetetramine solution, mix well, and then slowly dropwise add the ammonium paramolybdate solution, mix well to obtain a mixed system.
[0074] (3) The pH value of the mixed system was adjusted to 2.5 with 1 M hydrochloric acid, and the mixture was stirred for 2.5 h for aging. After aging, the precipitate was separated by centrifugation. The precipitate was washed three times with water and ethanol, and then dried under vacuum at 60° C. for 10 h to obtain a precursor.
[0075] (4) The precursor was placed in a tube furnace, heated to 650°C at a heating rate of 5°C / min under a flowing argon atmosphere, and maintained at 650°C for 2 h for nitridation to obtain a highly dispersed and highly loaded Mo2N catalyst Mo2N-2@C (HM) with hexamethylenetetramine as the dispersed carbon source.
[0076] Example 4
[0077] Example 4 of the present invention provides a method for preparing a highly dispersed and highly loaded Mo2N catalyst Mo2N-4@C (HM), which specifically comprises the following steps:
[0078] (1) 1.40 g of hexamethylenetetramine (HM) was dissolved in 50 ml of deionized water to obtain a hexamethylenetetramine solution after complete dissolution, and 4.92 g of ammonium paramolybdate was dissolved in 50 ml of deionized water to obtain an ammonium paramolybdate solution after complete dissolution.
[0079] (2) In 50 ml of deionized water, add 1 ml of 1 M hydrochloric acid, then add the hexamethylenetetramine solution, mix well, and then slowly drop the ammonium paramolybdate solution, mix well to obtain a mixed system.
[0080] (3) The pH value of the mixed system was adjusted to 2.5 with 1 M hydrochloric acid, and the mixture was stirred for 2.5 h for aging. After aging, the precipitate was separated by centrifugation. The precipitate was washed three times with water and ethanol, and then dried under vacuum at 60° C. for 10 h to obtain a precursor.
[0081] (4) The precursor was placed in a tube furnace, heated to 650°C at a heating rate of 5°C / min under a flowing argon atmosphere, and maintained at 650°C for 2 h for nitridation to obtain a highly dispersed and highly loaded Mo2N catalyst Mo2N-4@C (HM) with hexamethylenetetramine as the dispersed carbon source.
[0082] Example 5
[0083] Example 5 of the present invention provides a method for preparing a highly dispersed and highly loaded Mo2N catalyst Mo2N@C(pP), which specifically comprises the following steps:
[0084] (1) 1.08 g of p-phenylenediamine (pP) was dissolved in 50 ml of deionized water to obtain a p-phenylenediamine solution after complete dissolution, and 3.69 g of ammonium paramolybdate was dissolved in 50 ml of deionized water to obtain an ammonium paramolybdate solution after complete dissolution.
[0085] (2) In 50 ml of deionized water, add 1 ml of 1 M hydrochloric acid, then add the p-phenylenediamine solution, mix well, and then slowly drop the ammonium paramolybdate solution, mix well to obtain a mixed system.
[0086] (3) The pH value of the mixed system was adjusted to 2.5 with 1 M hydrochloric acid, and the mixture was stirred for 2.5 h for aging. After aging, the precipitate was separated by centrifugation. The precipitate was washed three times with water and ethanol, and then dried under vacuum at 60° C. for 10 h to obtain a precursor.
[0087] (4) The precursor was placed in a tube furnace, heated to 650°C at a heating rate of 5°C / min under a flowing argon atmosphere, and maintained at 650°C for 2 h for nitridation to obtain a highly dispersed and highly loaded Mo2N catalyst Mo2N@C(pP) with p-phenylenediamine as the dispersed carbon source.
[0088] The Mo2N@C(pP) prepared in Example 5 was subjected to XRD test, and its N2 adsorption and desorption effect, pore size, particle size, and transmission electron microscopy were tested. The results are as follows: Figures 1 to 3 , 6, and 7.
[0089] Example 6
[0090] Example 6 of the present invention provides a method for preparing a highly dispersed and highly loaded Mo2N catalyst Mo2N@C / SiO2, which specifically comprises the following steps:
[0091] (1) 1.40 g of hexamethylenetetramine (HM) was dissolved in 50 ml of deionized water to obtain a hexamethylenetetramine solution after complete dissolution, and 3.69 g of ammonium paramolybdate was dissolved in 50 ml of deionized water to obtain an ammonium paramolybdate solution after complete dissolution.
[0092] (2) 1 mL of 1M hydrochloric acid was added to 10 g of AS-40 silica sol, and then 50 ml of deionized water was added, and then the hexamethylenetetramine solution was added. After mixing evenly, the ammonium paramolybdate solution was slowly added dropwise, and mixed evenly to obtain a mixed system.
[0093] (3) The pH value of the mixed system was adjusted to 2.5 with 1 M hydrochloric acid, and the mixture was stirred for 2.5 h for aging. After aging, the precipitate was separated by centrifugation. The precipitate was washed three times with water and ethanol, and then dried under vacuum at 60° C. for 10 h to obtain a precursor.
[0094] (4) The precursor was placed in a tube furnace, heated to 650°C at a heating rate of 5°C / min under a flowing argon atmosphere, and maintained at 650°C for 2 h for nitridation to obtain a carbon-coated highly dispersed and highly loaded Mo2N catalyst Mo2N@C / SiO2 with 22 nm silicon spheres as the dispersed carrier.
[0095] The Mo2N@C / SiO2 prepared in Example 6 was subjected to XRD test, and its N2 adsorption and desorption effect, pore size, particle size, and transmission electron microscopy were tested. The results are as follows: Figures 1 to 3 , 8, and 9.
[0096] Example 7
[0097] Example 7 of the present invention provides a method for preparing a highly dispersed and highly loaded Mo2N catalyst Mo2N@C / SiO2-2, which specifically comprises the following steps:
[0098] (1) 1.40 g of hexamethylenetetramine (HM) was dissolved in 50 ml of deionized water to obtain a hexamethylenetetramine solution after complete dissolution, and 3.69 g of ammonium paramolybdate was dissolved in 50 ml of deionized water to obtain an ammonium paramolybdate solution after complete dissolution.
[0099] (2) 1 mL of 1 M hydrochloric acid was added to 4 g of AS-40 silica sol, and then 50 ml of deionized water was added, and then the hexamethylenetetramine solution was added. After mixing evenly, the ammonium paramolybdate solution was slowly added dropwise, and mixed evenly to obtain a mixed system.
[0100] (3) The pH value of the mixed system was adjusted to 2.5 with 1 M hydrochloric acid, and the mixture was stirred for 2.5 h for aging. After aging, the precipitate was separated by centrifugation. The precipitate was washed three times with water and ethanol, and then dried under vacuum at 60° C. for 10 h to obtain a precursor.
[0101] (4) The precursor was placed in a tube furnace, heated to 650°C at a heating rate of 5°C / min under a flowing argon atmosphere, and maintained at 650°C for 2 h for nitridation to obtain a carbon-coated highly dispersed and highly loaded Mo2N catalyst Mo2N@C / SiO2-2 with 22 nm silicon spheres as the dispersed carrier.
[0102] Comparative Example 1
[0103] Example 6 of the present invention provides a method for preparing a highly dispersed and highly loaded Mo2N catalyst Mo2N@C(oP), which specifically comprises the following steps:
[0104] (1) 1.08 g of o-phenylenediamine (oP) was dissolved in 50 ml of deionized water to obtain an o-phenylenediamine solution after complete dissolution, and 3.69 g of ammonium paramolybdate was dissolved in 50 ml of deionized water to obtain an ammonium paramolybdate solution after complete dissolution.
[0105] (2) In 50 ml of deionized water, add 1 ml of 1 M hydrochloric acid, then add the o-phenylenediamine solution, mix well, and then slowly drop the ammonium paramolybdate solution, mix well to obtain a mixed system.
[0106] (3) The pH value of the mixed system was adjusted to 2.5 with 1 M hydrochloric acid, and the mixture was stirred for 2.5 h for aging. After aging, the precipitate was separated by centrifugation. The precipitate was washed three times with water and ethanol, and then dried under vacuum at 60° C. for 10 h to obtain a precursor.
[0107] (4) The precursor was placed in a tube furnace, heated to 650°C at a heating rate of 5°C / min under a flowing argon atmosphere, and maintained at 650°C for 2 h for nitridation to obtain a highly dispersed and highly loaded Mo2N catalyst Mo2N@C(oP) with o-phenylenediamine as the dispersed carbon source.
[0108] The Mo2N@C(oP) prepared in Example 6 was subjected to XRD test, and its N2 adsorption and desorption effect, pore size, particle size, and transmission electron microscopy were tested. The results are as follows: Figures 1 to 3 , 10, and 11.
[0109] Test Example 1
[0110] Test Example 1 of the present invention evaluated the catalytic activity of the highly dispersed and highly loaded Mo2N catalyst prepared in Examples 1 to 8, and the specific method is as follows:
[0111] Ammonia decomposition and hydrogen production reaction was carried out in a laboratory micro fixed bed reactor consisting of three parts: a reaction gas distribution system, a fixed bed reaction system, and a detection system to evaluate the catalyst activity. The flow rate of the reaction gas in the gas distribution system is controlled by a mass flow meter; the fixed bed reactor in the reaction system is a quartz tube with an inner diameter of 6mm and a length of 40cm; the detection system uses gas chromatography to quantitatively analyze the gas components at the reactor outlet. The flow rates of each gas required for the experiment are controlled by a mass flow meter and introduced into the reactor after being mixed evenly.
[0112] Weigh 50 mg of the catalysts of Examples 1 to 8 with a particle size of 50 mesh and place them in a quartz tube reactor respectively, and conduct the following experiment: introduce H2 / N2 (60 ml / min, H2 / N2=3:1) to replace the air in the reaction tube, and pretreat the catalyst at a rate of 10°C / min to 500°C for 50 minutes. After the pretreatment, switch the introduced gas to pure ammonia gas and cool it to 400°C, then raise the temperature from 400°C to 600°C, stay at 50°C for 50 minutes at each interval, and conduct performance evaluation under the condition of an air velocity of 30000 mL / g / h. The results are as follows: Fig.12 , 13 shown.
[0113] The initial conversion rate of NH3 for the catalyst Mo2N@C(HM) of Example 1 at 550°C is 99%.
[0114] The initial conversion rate of NH3 for the catalyst Mo2N-1@C(HM) of Example 2 at 550°C is 91%.
[0115] The initial conversion rate of NH3 for the catalyst Mo2N-2@C(HM) of Example 3 at 550°C is 97%.
[0116] The initial conversion rate of NH3 for the catalyst Mo2N-4@C(HM) of Example 4 at 550°C is 99%.
[0117] The initial conversion rate of NH3 for the catalyst Mo2N@C(pP) of Example 5 at 550°C is 76%.
[0118] The initial conversion rate of NH3 for the catalyst Mo2N@C / SiO2 of Example 6 at 550°C is 100%.
[0119] The initial conversion rate of NH3 for the catalyst Mo2N@C / SiO2-2 of Example 7 at 550°C is 99%.
[0120] The initial conversion rate of NH3 for the catalyst Mo2N@C(oP) of Comparative Example 1 at 550°C is 57%.
[0121] Test Example 2
[0122] Test Example 2 of the present invention evaluated the catalyst activity of the highly dispersed and highly loaded Mo2N catalyst prepared in Examples 1 to 8, and the specific method is as follows:
[0123] The same pretreatment method as in Experimental Example 1 was adopted. After the pretreatment, the gas introduced was switched to Ar and the temperature was raised to 600°C. The reaction stability performance was evaluated at 600°C and NH3 space velocity of 90,000 mL / g / h. The results are as follows: Fig.14 shown.
[0124] Depend on Fig.14 It can be seen that no obvious deactivation was observed for the catalyst Mo2N@C / SiO2 of Example 6 after 200 hours of stability evaluation, the catalyst Mo2N@C / SiO2-2 of Example 7 was deactivated from 87% ammonia conversion rate to 76% after 40 hours of reaction, and the catalyst Mo2N@C(HM) of Example 1 was deactivated from 80% ammonia conversion rate to 36% after 40 hours of reaction.
[0125] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A highly dispersed and highly loaded Mo2N catalyst, characterized in that: The highly dispersed and highly loaded Mo2N catalyst comprises raw materials in the following mass molar ratio: silicon source: amino organic matter: molybdenum source = 0-20 g: 10 mmol: 1-20 mmol.
2. The highly dispersed and highly loaded Mo2N catalyst according to claim 1, characterized in that: The silicon source includes one of silica sol, silica balls, and amorphous silica; the amine-containing organic matter includes one of p-phenylenediamine and hexamethylenetetramine; and the molybdenum source includes one of ammonium paramolybdate, phosphomolybdic acid, and sodium molybdate.
3. A method for preparing the highly dispersed and highly loaded Mo2N catalyst according to any one of claims 1 to 2, characterized in that: The steps include: (1) dissolving a silicon source in deionized water, adding hydrochloric acid for pre-acidification treatment, and sequentially adding an amine-containing organic solution and a molybdenum source solution, and mixing them uniformly to obtain a mixed system; (2) adjusting the pH value of the mixed system, heating and stirring for aging, separating and precipitating, washing, and drying to obtain a precursor; (3) The precursor is placed in flowing argon gas and heated for nitridation to obtain a highly dispersed and highly loaded Mo2N catalyst.
4. The method for preparing the highly dispersed and highly loaded Mo2N catalyst according to claim 3, characterized in that: In step (1), the concentration of the hydrochloric acid is 1 mol / L, and the mass volume ratio of the silicon source to the hydrochloric acid is 0-10 g:0-2 mL.
5. The method for preparing the highly dispersed and highly loaded Mo2N catalyst according to claim 3, characterized in that: In step (2), the pH value is 1 to 5, and the stirring aging time is 2 to 5 hours.
6. The method for preparing the highly dispersed and highly loaded Mo2N catalyst according to claim 3, characterized in that: The method of heating nitriding in step (3) is: The temperature was raised to 600-800°C at a rate of 5-20°C / min and kept at that temperature for 1-4h, then cooled to room temperature and passivated in 1% O2 / Ar for 10-12h.
7. Use of a highly dispersed and highly loaded Mo2N catalyst prepared by the highly dispersed and highly loaded Mo2N catalyst according to any one of claims 1 to 2 or the method for preparing a highly dispersed and highly loaded Mo2N catalyst according to any one of claims 3 to 6 in an ammonia decomposition reaction.
8. The use of the highly dispersed and highly supported Mo2N catalyst in ammonia decomposition hydrogen production reaction according to claim 7, characterized in that: The highly dispersed and highly loaded Mo2N catalyst needs to be pretreated before decomposing ammonia to produce hydrogen; the pretreatment temperature is 350-550°C; the heating rate during pretreatment is 5-15°C / min; the pretreatment time is 30-60min; and the pretreatment is carried out under a H2 / N2 atmosphere.
Citation Information
Patent Citations
Preparation method of molybdenum nitride
CN102161478A
Molybdenum-based ammonia decomposition hydrogen production catalyst and preparation method thereof
CN114100661A
Supported hydrodechlorination catalyst, preparation method and application thereof, and method for preparing chlorotrifluoroethylene by using catalyst
CN115364888A
Supported molybdenum carbide catalyst and preparation method and application thereof
CN116571260A
Catalyst using TiO2 as carrier to load metal nitride Mo2N
CN1262969A