Silver-based catalyst and preparation method and application thereof

By using a zeolite molecular sieve support with high specific surface area and calcination reduction treatment, the high dispersion of silver-based catalysts is achieved, and the problems of low dispersion and selectivity of catalysts in the prior art are solved, and the preparation of 1,3-butadiene oxidation is significantly improved 3,4-epoxy-1-butene efficiency.

CN119016091APending Publication Date: 2024-11-26SHIMING (SUZHOU) NEW MATERIAL RES INST CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411120676.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The specific surface area of ​​the existing α-Al2O3 support is small, resulting in the conversion of 1,3-butadiene and 3 in the silver-based catalysts when catalyzing the oxidation of 1,3-butadiene, 3,4-epoxy-1-butene. ,4-epoxy-1-butene has a low selectivity.

Method used

A zeolite molecular sieve containing α-Al2O3 and metal cations with a high specific surface area was used as a support, and the silver was highly dispersed by calcining and reducing treatment, and a silver-based catalyst was prepared with a zeolite molecular sieve containing α-Al2O3 and metal cations as a support.

Benefits of technology

The conversion rate of 1,3-butadiene and the selectivity of 3,4-epoxy-1-butene were significantly improved, reaching more than 95%, achieving efficient synthesis of 3,4-epoxy-1-butene.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a silver-based catalyst. The preparation method comprises the following steps: roasting a silicon-aluminum zeolite molecular sieve containing metal cations to obtain a zeolite molecular sieve containing alpha-Al2O3 and the metal cations; the method comprises the following steps: mixing a zeolite molecular sieve containing alpha-Al2O3 and metal cations, an organic amine aqueous solution and a silver source to prepare a reaction solution; and reacting the reaction liquid at a certain temperature, and carrying out suction filtration, drying and reduction on the reacted product to obtain the silver-based catalyst taking the zeolite molecular sieve containing alpha-Al2O3 and metal cations as the carrier. According to the prepared silver-based catalyst, the zeolite molecular sieve which is high in specific surface area and contains alpha-Al2O3 and metal cations is used as the carrier, high dispersion of silver on the carrier is achieved, the silver-based catalyst is applied to preparation of 3, 4-epoxy-1-butene through oxidation of 1, 3-butadiene, and the conversion rate of the 1, 3-butadiene and the selectivity of the 3, 4-epoxy-1-butene can both reach 95% or above.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of industrial catalysis, and in particular to a silver-based catalyst, a preparation method thereof and application of the silver-based catalyst in the preparation of 3,4-epoxy-1-butene by oxidation of 1,3-butadiene. Background Art

[0002] 3,4-Epoxy-1-butene is a rare fine chemical that contains both epoxy bonds and double bonds. It has a relatively active reaction activity. It is used as a raw material for the synthesis of pharmaceutical intermediates, chiral compounds, new flame retardants and functional polymer materials. It is a fine chemical that is in short supply both at home and abroad.

[0003] The preparation of 3,4-epoxy-1-butene from 1,3-butadiene by gas phase oxidation is considered to be an economical and feasible process route, and has triggered a wave of research in industry and academia. In addition, the process route uses silver supported on α-Al2O3 as the active component, and improves the conversion rate of 1,3-butadiene and the selectivity of 3,4-epoxy-1-butene by adding additives such as alkali metal cations and alkaline earth metal cations (US5081096, US6011163). However, the specific surface area of ​​α-Al2O3 is small (1-5 m 2 / g), silver cannot be highly dispersed on the carrier, resulting in low 1,3-butadiene conversion (14-18%) and 3,4-epoxy-1-butene selectivity (87-90%). Summary of the invention

[0004] In order to solve the above technical problems, the purpose of the present invention is to provide a silver-based catalyst and its preparation method and application. The silver-based catalyst uses a high-specific-surface-area zeolite molecular sieve containing α-Al2O3 and metal cations as a carrier, and achieves a high dispersion of silver on the carrier. It is applied to the oxidation of 1,3-butadiene to prepare 3,4-epoxy-1-butene, and can make the conversion rate of 1,3-butadiene and the selectivity of 3,4-epoxy-1-butene both reach more than 95%.

[0005] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0006] A method for preparing a silver-based catalyst comprises the following steps:

[0007] (1) calcining a silica-alumina zeolite molecular sieve containing metal cations to obtain a zeolite molecular sieve containing α-Al2O3 and metal cations;

[0008] (2) mixing a zeolite molecular sieve containing α-Al2O3 and metal cations, an organic amine aqueous solution and a silver source to prepare a reaction solution;

[0009] (3) reacting the reaction solution at a certain temperature, filtering, drying and reducing the product after the reaction to obtain a silver-based catalyst with a zeolite molecular sieve containing α-Al2O3 and metal cations as a carrier.

[0010] Preferably, the metal cation in step (1) is at least one of an alkali metal cation and an alkaline earth metal cation; and the content of the metal cation in the silica-alumina zeolite molecular sieve containing the metal cation is 1 to 5 wt.%.

[0011] Preferably, the silica-alumina molecular sieve in step (1) is one of FAU and LTA type silica-alumina zeolite molecular sieves, and the aluminum content is 10 to 25 wt.%.

[0012] Preferably, the calcination conditions in step (1) are 700-1000° C. in an air atmosphere for 6-12 hours.

[0013] Preferably, in step (2), the weight ratio of the zeolite molecular sieve containing α-Al2O3 and metal cations, the organic amine aqueous solution and the silver source is 1:(5-30):(0.01-0.1).

[0014] Preferably, the organic amine aqueous solution in step (2) is an aqueous solution of piperidine, pyridine or hexamethyleneimine, and its concentration is 0.1-1M.

[0015] Preferably, the silver source in step (2) is one of silver acetate and silver oxalate.

[0016] Preferably, in step (3), the reaction conditions of the reaction solution are 40-80° C. for 8-24 hours; and the reduction conditions in step (3) are 400-600° C. for 4-12 hours in a hydrogen atmosphere.

[0017] The silver-based catalyst prepared by the above preparation method uses a zeolite molecular sieve containing α-Al2O3 and metal cations as a carrier. The silver-based catalyst can be used in the process reaction of catalyzing the oxidation of 1,3-butadiene to prepare 3,4-epoxy-1-butene.

[0018] The beneficial effects of the present invention are:

[0019] The present invention firstly calcines the alumina-silica zeolite molecular sieve containing metal cations at a certain temperature, so that the aluminum in the zeolite molecular sieve is highly dispersed in the pores of the zeolite molecular sieve in the form of α-Al2O3, thereby obtaining a zeolite molecular sieve having a high specific surface area (~400m 2 / g) of zeolite molecular sieve containing α-Al2O3 and metal cations, the zeolite molecular sieve is mixed with an organic amine aqueous solution and a silver source for reaction, and then subjected to high-temperature reduction treatment to prepare a catalyst in which silver is highly dispersed on a zeolite molecular sieve carrier containing α-Al2O3 and metal cations.

[0020] The preparation method of the present invention realizes high dispersion of silver on the carrier, and is applied to the oxidation of 1,3-butadiene to prepare 3,4-epoxy-1-butene, which can increase the conversion rate of 1,3-butadiene and the selectivity of 3,4-epoxy-1-butene to more than 95%, thereby realizing efficient synthesis of 3,4-epoxy-1-butene. The metal cation in the silver-based catalyst can play a role in regulating the catalytic selectivity. DETAILED DESCRIPTION

[0021] The technical solutions in the present invention will be described clearly and completely below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] The present invention provides a method for preparing a silver-based catalyst, which comprises the following steps:

[0023] (1) calcining a silica-alumina zeolite molecular sieve containing metal cations to obtain a zeolite molecular sieve containing α-Al2O3 and metal cations; wherein the silica-alumina zeolite molecular sieve is preferably one of FAU and LTA type silica-alumina zeolite molecular sieves, and the aluminum content is 10 to 25 wt.%; the calcination conditions in step (1) are calcination at 700 to 1000° C. in an air atmosphere for 6 to 12 hours;

[0024] (2) mixing a zeolite molecular sieve containing α-Al2O3 and metal cations, an organic amine aqueous solution and a silver source to prepare a reaction solution; the weight ratio of the zeolite molecular sieve containing α-Al2O3 and metal cations, the organic amine aqueous solution and the silver source is 1:(5-30):(0.01-0.1); the organic amine aqueous solution is preferably an aqueous solution of piperidine, pyridine or hexamethyleneimine, and its concentration is 0.1-1M; wherein the silver source is one of silver acetate and silver oxalate;

[0025] (3) reacting the reaction solution at a certain temperature, the reaction conditions are 40-80° C. for 8-24 hours, filtering, drying and reducing the product after the reaction to obtain a silver-based catalyst with a zeolite molecular sieve containing α-Al2O3 and metal cations as a carrier; wherein the reduction conditions are 400-600° C. in a hydrogen atmosphere for 4-12 hours.

[0026] The silver-based catalyst prepared by the above preparation method uses a zeolite molecular sieve containing α-Al2O3 and metal cations as a carrier, and zero-valent silver is highly dispersed on the carrier.

[0027] The silver-based catalyst can be used in the process reaction of catalyzing the oxidation of 1,3-butadiene to prepare 3,4-epoxy-1-butene.

[0028] The present invention is further described in detail below through specific examples.

[0029] Unless otherwise specified, the reagents involved in the embodiments of the present invention are all commercially available products and can be purchased through commercial channels.

[0030] Example 1

[0031] (1) calcining a silica-alumina zeolite molecular sieve containing metal cations to obtain a zeolite molecular sieve containing α-Al2O3 and metal cations, wherein the silica-alumina zeolite molecular sieve containing metal cations is a FAU type silica-alumina molecular sieve containing sodium ions, wherein the sodium ion and aluminum contents are 2.5 wt.% and 10 wt.%, respectively, and the calcination condition is 700° C. in an air atmosphere for 12 hours;

[0032] (2) mixing the raw materials with a zeolite molecular sieve containing α-Al2O3 and metal cations, an organic amine aqueous solution and a silver source in a weight ratio of 1:5:0.01 to prepare a reaction solution, wherein the organic amine aqueous solution is an aqueous solution of piperidine with a concentration of 0.1 M, and the silver source is silver acetate;

[0033] (3) reacting the reaction solution at 40° C. for 24 hours, and filtering, drying and reducing the product obtained after the reaction to obtain a silver-based catalyst with a zeolite molecular sieve containing α-Al2O3 and metal cations as a carrier, wherein the reduction condition is 500° C. in a hydrogen atmosphere for 6 hours.

[0034] Example 2

[0035] (1) calcining a silica-alumina zeolite molecular sieve containing metal cations to obtain a zeolite molecular sieve containing α-Al2O3 and metal cations, wherein the silica-alumina zeolite molecular sieve containing metal cations is an LTA type silica-alumina molecular sieve containing calcium ions, the calcium ion and aluminum contents are 5 wt.% and 25 wt.%, respectively, and the calcination conditions are 1000° C. in an air atmosphere for 6 hours;

[0036] (2) mixing the raw materials with a zeolite molecular sieve containing α-Al2O3 and metal cations, an organic amine aqueous solution and a silver source in a weight ratio of 1:30:0.1 to prepare a reaction solution, wherein the organic amine aqueous solution is an aqueous solution of pyridine with a concentration of 1M, and the silver source is silver oxalate;

[0037] (3) reacting the reaction solution at 80° C. for 8 hours, and filtering, drying and reducing the product obtained after the reaction to obtain a silver-based catalyst with a zeolite molecular sieve containing α-Al2O3 and metal cations as a carrier, wherein the reduction condition is 600° C. in a hydrogen atmosphere for 4 hours.

[0038] Example 3

[0039] (1) calcining a silica-alumina zeolite molecular sieve containing metal cations to obtain a zeolite molecular sieve containing α-Al2O3 and metal cations, wherein the silica-alumina zeolite molecular sieve containing metal cations is a FAU type silica-alumina molecular sieve containing magnesium ions, and the magnesium ion and aluminum contents are 1 wt.% and 15 wt.%, respectively, and the calcination conditions are 850° C. in an air atmosphere for 8 hours;

[0040] (2) mixing the raw materials with a zeolite molecular sieve containing α-Al2O3 and metal cations, an organic amine aqueous solution and a silver source in a weight ratio of 1:15:0.05 to prepare a reaction solution, wherein the organic amine aqueous solution is an aqueous solution of hexamethyleneimine with a concentration of 0.5 M, and the silver source is silver acetate;

[0041] (3) reacting the reaction solution at 60° C. for 12 hours, and filtering, drying and reducing the product obtained after the reaction to obtain a silver-based catalyst with a zeolite molecular sieve containing α-Al2O3 and metal cations as a carrier, wherein the reduction condition is reduction at 400° C. in a hydrogen atmosphere for 12 hours.

[0042] Example 4

[0043] (1) calcining a silica-alumina zeolite molecular sieve containing metal cations to obtain a zeolite molecular sieve containing α-Al2O3 and metal cations, wherein the silica-alumina zeolite molecular sieve containing metal cations is an LTA type silica-alumina molecular sieve containing potassium ions, the potassium ion and aluminum contents are 2.5 wt.% and 10 wt.%, respectively, and the calcination conditions are 700° C. in an air atmosphere for 12 hours;

[0044] (2) mixing the raw materials with a zeolite molecular sieve containing α-Al2O3 and metal cations, an organic amine aqueous solution and a silver source in a weight ratio of 1:5:0.01 to prepare a reaction solution, wherein the organic amine aqueous solution is an aqueous solution of piperidine with a concentration of 0.1 M, and the silver source is silver oxalate;

[0045] (3) reacting the reaction solution at 60° C. for 12 hours, and filtering, drying and reducing the product obtained after the reaction to obtain a silver-based catalyst with a zeolite molecular sieve containing α-Al2O3 and metal cations as a carrier, wherein the reduction condition is reduction at 600° C. in a hydrogen atmosphere for 6 hours.

[0046] Comparative Example 1

[0047] (1) mixing 2.5 wt.% of α-Al2O3 with an organic amine aqueous solution and a silver source in a weight ratio of 1:5:0.01 to prepare a reaction solution, wherein the organic amine aqueous solution is an aqueous solution of piperidine with a concentration of 0.1 M, and the silver source is silver acetate;

[0048] (2) reacting the reaction solution at 40° C. for 24 hours, and filtering, drying and reducing the product obtained after the reaction to obtain a silver-based catalyst with α-Al2O3 containing metal cations as a carrier, wherein the reduction condition is 500° C. in a hydrogen atmosphere for 6 hours.

[0049] Comparative Example 2

[0050] (1) α-Al2O3 containing 5 wt.% calcium ions is mixed with an organic amine aqueous solution and a silver source in a weight ratio of 1:5:0.01 to prepare a reaction solution, wherein the organic amine aqueous solution is an aqueous solution of piperidine with a concentration of 0.1 M, and the silver source is silver oxalate.

[0051] (2) reacting the reaction solution at 60° C. for 12 hours, and filtering, drying and reducing the product obtained after the reaction to obtain a silver-based catalyst with α-Al2O3 containing metal cations as a carrier, wherein the reduction condition is 600° C. in a hydrogen atmosphere for 6 hours.

[0052] Application Examples

[0053] The silver-based catalysts obtained in the embodiment and the comparative example were respectively used to catalyze the oxidation of 1,3-butadiene to prepare 3,4-epoxy-1-butene; the reaction was carried out in a fixed bed reaction apparatus, and the mass space velocity of 1,3-butadiene was 3h -1 , the molar ratio of 1,3-butadiene to oxygen is 1:0.5, the reaction temperature is 250°C, and the reaction pressure is 0.1MPa.

[0054] The conversion rate of 1,3-butadiene and the selectivity of 3,4-epoxy-1-butene in each embodiment and comparative example are shown in Table 1.

[0055] Table 1

[0056] Serial number 1,3-Butadiene conversion rate (%) 3,4-Epoxy-1-butene selectivity (%) Example 1 98 95 Example 2 96 96 Example 3 98 98 Example 4 97 96 Comparative Example 1 15 90 Comparative Example 2 18 87

[0057] It can be seen from Table 1 that compared with Comparative Examples 1 and 2, the reaction of 1,3-butadiene oxidation to prepare 3,4-epoxy-1-butene using the silver-based catalyst of Examples 1-4 of the present invention has a higher 1,3-butadiene conversion rate and 3,4-epoxy-1-butene selectivity.

[0058] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.

[0059] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A method for preparing a silver-based catalyst, characterized in that: The steps include: (1) calcining a silica-alumina zeolite molecular sieve containing metal cations to obtain a zeolite molecular sieve containing α-Al2O3 and metal cations; (2) mixing a zeolite molecular sieve containing α-Al2O3 and metal cations, an organic amine aqueous solution and a silver source to prepare a reaction solution; (3) reacting the reaction solution at a certain temperature, filtering, drying and reducing the product after the reaction to obtain a silver-based catalyst with a zeolite molecular sieve containing α-Al2O3 and metal cations as a carrier.

2. The method for preparing a silver-based catalyst according to claim 1, characterized in that: The metal cation in step (1) is at least one of an alkali metal cation and an alkaline earth metal cation; and the content of the metal cation in the silica-alumina zeolite molecular sieve containing the metal cation is 1 to 5 wt.%.

3. The method for preparing a silver-based catalyst according to claim 1, characterized in that: The silica-alumina molecular sieve in step (1) is one of FAU and LTA type silica-alumina zeolite molecular sieves, and the aluminum content is 10-25wt.%.

4. The method for preparing a silver-based catalyst according to claim 1, characterized in that: The calcination conditions in step (1) are 700-1000° C. in an air atmosphere for 6-12 hours.

5. The method for preparing a silver-based catalyst according to claim 1, characterized in that: In step (2), the weight ratio of the zeolite molecular sieve containing α-Al2O3 and metal cations, the organic amine aqueous solution and the silver source is 1:(5-30):(0.01-0.1).

6. The method for preparing a silver-based catalyst according to claim 1 or 5, characterized in that: The organic amine aqueous solution in step (2) is an aqueous solution of piperidine, pyridine or hexamethyleneimine, and its concentration is 0.1-1M.

7. The method for preparing a silver-based catalyst according to claim 1 or 5, characterized in that: The silver source in step (2) is one of silver acetate and silver oxalate.

8. The method for preparing a silver-based catalyst according to claim 1 or 5, characterized in that: In step (3), the reaction conditions of the reaction solution are 40-80° C. for 8-24 hours; and the reduction conditions in step (3) are 400-600° C. for 4-12 hours in a hydrogen atmosphere.

9. A silver-based catalyst prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The silver-based catalyst uses a zeolite molecular sieve containing α-Al2O3 and metal cations as a carrier.

10. Use of the silver-based catalyst according to claim 9, characterized in that: The silver-based catalyst is used in the oxidation of 1,3-butadiene to prepare 3,4-epoxy-1-butene.