Catalyst as well as preparation method and application thereof

By combining amorphous silicon aluminum oxide and zeolite molecular sieve modification in the catalyst, the problem of low methanol conversion and monomethylamine selectivity is solved, the efficiency and economicality of the catalyst are improved, and it is suitable for industrial methylamine production.

CN119016096APending Publication Date: 2024-11-26HUALU ENG & TECH
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411194089.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing problems of low methanol conversion and low monomethylamine selectivity lead to the fact that the product composition of industrial methylamine catalysts is mostly trimethylamine under high temperature and high pressure conditions, and excessive recycle is required, which increases energy consumption and economic costs.

Method used

The methanol conversion rate is improved by using amorphous silicon aluminum oxide and a supported metal oxide as the first active ingredient and a second metal ion exchange zeolite molecular sieve as the second active ingredient through specific modification and modification. Methylamine selectivity.

Benefits of technology

It achieves the increase in monomethylamine selectivity while high methanol conversion, reduces energy consumption and economic costs, and is suitable for industrial-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005015863770000111
    Figure BDA0005015863770000111
  • Figure BDA0005015863770000112
    Figure BDA0005015863770000112
Patent Text Reader

Abstract

The invention provides a catalyst as well as a preparation method and application thereof. The catalyst comprises a first active component and a second active component, wherein the first active component comprises an amorphous silicon aluminum oxide and an oxide of a first metal, the oxide of the first metal is loaded on at least part of the surface of the amorphous silicon aluminum oxide, and the first metal comprises a transition metal and / or an alkaline earth metal; the specific surface area of the first active component is not less than 350m < 2 > / g, and the surface acidity is 0.02-0.5 mmol / g; the second active component comprises a zeolite molecular sieve subjected to ion exchange of a second metal, and the second metal comprises at least one of potassium, calcium, sodium and magnesium; and the pore diameter of the second active component is 2-50nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalyst preparation, and specifically relates to a catalyst and a preparation method and application thereof. Background Art

[0002] Organic amines are an important class of chemical raw materials. They are widely used in various aspects of the national economy and are the basic raw materials for many industrial chemicals. Among them, monomethylamine is an important organic amine, which can react with γ-butyrolactone and then dehydrate to form N-methylpyrrolidone (NMP). NMP is widely used in the supporting solvents of lithium battery positive electrode binders (PVDF). In recent years, the booming lithium battery market has led to a surge in demand for the upstream raw material monomethylamine. Monomethylamine accounts for more than 60% of the NMP preparation industry. In addition, it also involves other industries such as electronic chemicals, additives, chemical intermediates, and pharmaceuticals.

[0003] At present, the synthesis of methylamine in industry is based on methanol and liquid ammonia as raw materials. Under high temperature and high pressure, a methylamine mixture is first obtained through gas-solid catalysis in the presence of a catalyst, and then a certain separation process is used to obtain pure monomethylamine, dimethylamine, and trimethylamine. However, traditional methylamine catalysts are limited by thermodynamic equilibrium, and the composition of the reactor outlet product is mostly trimethylamine. In order to produce more monomethylamine, the industry often recycles excess trimethylamine, which causes a large amount of material to "idle" in the entire system, resulting in excessive energy consumption for subsequent separation and poor economic efficiency. For this reason, many researchers have focused on shape-selective catalysts based on zeolite molecular sieves, attempting to use the confinement effect of molecular sieves to break the thermodynamic equilibrium of the methanol amination reaction, thereby achieving the purpose of producing more monomethylamine. However, the low conversion rate of zeolite molecular sieves limits their large-scale application in actual industrial scenarios.

[0004] Therefore, it is of great significance to develop a catalyst with high conversion rate and improved selectivity for monomethylamine. Summary of the invention

[0005] The invention provides a catalyst for solving the problems of low methanol conversion rate and low monomethylamine selectivity in the prior art.

[0006] The invention provides a method for preparing a catalyst. The method is simple and easy to implement, has high operability, and can prepare a catalyst with high methanol conversion rate and monomethylamine selectivity.

[0007] The present invention also provides an application of a catalyst for improving the methanol conversion rate and monomethylamine selectivity when monomethylamine is produced using methanol and liquid ammonia as raw materials.

[0008] In one aspect, the present invention provides a catalyst comprising a first active component and a second active component;

[0009] The first active component includes amorphous silicon aluminum oxide and an oxide of a first metal supported on at least a portion of the surface of the amorphous silicon aluminum oxide, wherein the first metal includes a transition metal and / or an alkaline earth metal; and the specific surface area of ​​the first active component is not less than 350 m 2 / g, surface acidity is 0.02-0.5mmol / g;

[0010] The second active component includes a zeolite molecular sieve exchanged with a second metal ion, wherein the second metal includes at least one of potassium, calcium, sodium and magnesium; and the pore size of the second active component is 2-50 nm.

[0011] Furthermore, the mass ratio of the first active ingredient to the second active ingredient is (70-99):(1-30).

[0012] Furthermore, the chemical formula of the amorphous silicon aluminum oxide is xAl2O3·ySiO2, wherein 0.49≤x≤0.99, 0.001≤y≤0.67.

[0013] Furthermore, the mass ratio of the amorphous silicon aluminum oxide to the first metal is 100:(1-20).

[0014] Furthermore, the molar ratio of the zeolite molecular sieve to the second metal is (0.01-10):1.

[0015] Furthermore, the particle size of the catalyst is 10-40 meshes.

[0016] Furthermore, the first metal includes at least one of magnesium, calcium, barium, potassium, cerium, zirconium and zinc.

[0017] Further, the zeolite molecular sieve is an ammonium type and / or a hydrogen type zeolite molecular sieve; and / or,

[0018] The zeolite molecular sieve includes at least one of mordenite, SPAO-11, SPAO-14, SAPO-34, ZSM-5, SSZ-13, and β molecular sieve.

[0019] In another aspect, the present invention provides a method for preparing the above catalyst, comprising the following steps:

[0020] (1) Add the silicon source solution dropwise to the aluminum source solution and adjust the pH value to 7-10, perform an aging treatment, wash to neutrality, perform a first drying treatment and a first calcination treatment in sequence, and obtain a specific surface area of ​​not less than 350m 2 / g amorphous silicon aluminum oxide;

[0021] (2) adding a first metal salt solution to the amorphous silicon aluminum oxide, stirring while dripping, and then sequentially performing an aging treatment and a second calcination treatment to obtain a first active ingredient with a surface acidity of 0.02-0.5 mmol / g; the first metal salt comprises at least one of a transition metal and / or an alkaline earth metal salt;

[0022] (3) adding the zeolite molecular sieve to a second metal salt solution, and sequentially performing an ion exchange treatment, a second drying treatment, and a third calcination treatment to obtain a second active ingredient with a pore size of 2-50 nm; the second metal salt comprises at least one of a potassium salt, a sodium salt, a calcium salt, and a magnesium salt;

[0023] (4) The first active ingredient and the second active ingredient are mixed uniformly and crushed to obtain a catalyst.

[0024] In another aspect, the present invention provides an application of the above catalyst and the catalyst prepared by the above preparation method in producing monomethylamine using methanol and liquid ammonia as raw materials.

[0025] The present invention provides a catalyst comprising a first active component and a second active component, wherein the first active component comprises amorphous silicon aluminum oxide and an oxide of a first metal supported on at least a portion of the surface of the amorphous silicon aluminum oxide, wherein the first metal comprises a transition metal and / or an alkaline earth metal; and the specific surface area of ​​the first active component is not less than 350 m 2 / g, and the surface acidity is 0.02-0.5mmol / g; the second active ingredient includes a zeolite molecular sieve exchanged with a second metal ion, and the second metal includes at least one of potassium, calcium, sodium and magnesium; the pore size of the second active ingredient is 2-50nm; the two active ingredients are specifically modified and modified by the above-mentioned specific metals, so that the first active ingredient improves the methanol conversion rate and the second active ingredient improves the monomethylamine selectivity, so that the prepared catalyst can have a good monomethylamine selectivity while maintaining a high methanol conversion rate. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] In one aspect, the present invention provides a catalyst comprising a first active component and a second active component;

[0028] The first active component includes amorphous silicon aluminum oxide and an oxide of a first metal supported on at least a portion of the surface of the amorphous silicon aluminum oxide, wherein the first metal includes a transition metal and / or an alkaline earth metal; the specific surface area of ​​the first active component is not less than 350 m 2 / g, surface acidity is 0.02-0.5mmol / g;

[0029] The second active component includes a zeolite molecular sieve exchanged with a second metal ion, wherein the second metal includes at least one of potassium, calcium, sodium and magnesium; and the pore size of the second active component is 2-50 nm.

[0030] The catalyst provided by the present invention comprises a first active component and a second active component; wherein the first active component comprises amorphous silicon aluminum oxide and an oxide of a first metal supported on at least a portion of the surface of the amorphous silicon aluminum oxide, wherein the first metal comprises a transition metal and / or an alkaline earth metal; and the specific surface area of ​​the first active component is not less than 350 m 2 / g, surface acidity is 0.02-0.5mmol / g;

[0031] Among them, amorphous silicon aluminum oxide has the characteristics of high specific surface area, and there are a large number of active sites required for methanol amination reaction on its surface, which can promote the rapid reaction of methanol and ammonia, and the oxide of transition metal and / or alkaline earth metal is loaded on at least part of the surface of amorphous silicon aluminum oxide, and its surface can be modified by transition metal and / or alkaline earth metal ions to weaken its surface acidity, and the transition metal and / or alkaline earth metal may form a unique electronic interaction with at least part of the surface of amorphous silicon aluminum oxide, thereby inhibiting the generation of by-products such as dimethyl ether in the methanol amination reaction;

[0032] The second active component includes a zeolite molecular sieve exchanged with a second metal ion, wherein the second metal includes at least one of potassium, calcium, sodium and magnesium, and the pore size of the second active component is 2-50nm; the zeolite molecular sieve structure contains a large number of silicon-oxygen tetrahedrons and aluminum-oxygen tetrahedrons, which form a complex pore network. By exchanging ions between the second metal including at least one of potassium, calcium, sodium and magnesium and the zeolite molecular sieve, the metal ions of the second metal enter the pores of the zeolite molecular sieve and replace part of the original ion positions in the zeolite molecular sieve, thereby modifying the pore openings and greatly improving the shape selectivity of the zeolite molecular sieve, making it difficult for products with larger molecular sizes such as dimethylamine and trimethylamine to escape from the cage of the zeolite molecular sieve, thereby improving the selectivity of monomethylamine in the product distribution to a certain extent.

[0033] The present invention provides a catalyst comprising a first active component and a second active component, wherein the first active component comprises amorphous silicon aluminum oxide and an oxide of a first metal supported on at least a portion of the surface of the amorphous silicon aluminum oxide, wherein the first metal comprises a transition metal and / or an alkaline earth metal; and the specific surface area of ​​the first active component is not less than 350 m 2 / g, and the surface acidity is 0.02-0.5mmol / g; the second active ingredient includes a zeolite molecular sieve exchanged with a second metal ion, and the second metal includes at least one of potassium, calcium, sodium and magnesium; the pore size of the second active ingredient is 2-50nm; the two active ingredients are specifically modified and modified by the above-mentioned specific metals, so that the first active ingredient improves the methanol conversion rate and the second active ingredient improves the monomethylamine selectivity, so that the prepared catalyst can have a good monomethylamine selectivity while maintaining a high methanol conversion rate.

[0034] Furthermore, the mass ratio of the first active ingredient to the second active ingredient is (70-99):(1-30).

[0035] It can be understood that the catalyst provided by the present invention has two active ingredients, and the ratio of the two active ingredients is crucial to the catalytic effect. When the mass ratio of the first active ingredient to the second active ingredient is (70-99): (1-30), the methanol conversion rate can be further improved while improving the selectivity of monomethylamine.

[0036] In one specific embodiment, the chemical formula of amorphous silicon aluminum oxide is xAl2O3·ySiO2, wherein 0.49≤x≤0.99, 0.001≤y≤0.67.

[0037] Amorphous silicon aluminum oxide is composed of aluminum oxide and silicon oxide. When the chemical formula of amorphous silicon aluminum oxide can be expressed as xAl2O3·ySiO2, wherein 0.49≤x≤0.99 and 0.001≤y≤0.67, the ratio of silicon dioxide to aluminum oxide in the amorphous silicon aluminum oxide can be further limited. At this time, the raw material conversion rate and product selectivity of the catalyst in catalyzing methanol to produce monomethylamine can be further improved, and the life of the catalyst can be extended.

[0038] Furthermore, the mass ratio of amorphous silicon aluminum oxide to the first metal is 100:(1-20).

[0039] The inventors have discovered through research that surface acidity of amorphous silicon aluminum oxide can be weakened by modifying the surface of the amorphous silicon aluminum oxide with a first metal including a transition metal and / or an alkaline earth metal. When the mass ratio of the amorphous silicon aluminum oxide to the first metal is 100:(1-20), the conversion rate of methanol and the selectivity of monomethylamine can be further improved, and the production of side reactions such as dimethyl ether can be further reduced.

[0040] In one specific embodiment, the molar ratio of the zeolite molecular sieve to the second metal is (0.01-10):1.

[0041] The pore size of the zeolite molecular sieve can be modified by ion exchange between a second metal including at least one of potassium, calcium, sodium and magnesium and the zeolite molecular sieve. When the molar ratio of the zeolite molecular sieve to the second metal is (0.01-10):1, the pore size of the zeolite molecular sieve can be made more favorable for the selective production of monomethylamine, and the coking phenomenon that may be caused by too small pores can be balanced.

[0042] Optionally, the particle size of the catalyst is 10-40 mesh.

[0043] It can be understood that the particle size of the catalyst is related to the activity and selectivity of the catalyst. When the particle size of the catalyst is 10-40 mesh, the selectivity of the raw materials and the selectivity of the products can be further improved, and the stability of the catalyst can be improved.

[0044] Specifically, the first metal includes at least one of magnesium, calcium, barium, potassium, cerium, zirconium, and zinc.

[0045] The first metal includes a transition metal and / or an alkaline earth metal. In a specific embodiment, the inventors have found that when the first metal includes at least one of magnesium, calcium, barium, potassium, cerium, zirconium and zinc, the activity of the catalyst can be further improved, and the methanol conversion rate and monomethylamine selectivity can be further improved.

[0046] In a specific embodiment, the zeolite molecular sieve is an ammonium type and / or hydrogen type zeolite molecular sieve. The zeolite molecular sieve is an ammonium type and / or hydrogen type zeolite molecular sieve, which can improve the modification effect of the second metal on the zeolite molecular sieve, and further improve the shape selectivity of the second active ingredient on monomethylamine; further, the zeolite molecular sieve can include at least one of mordenite, SPAO-11, SPAO-14, SAPO-34, ZSM-5, SSZ-13, and β molecular sieve.

[0047] On the other hand, the present invention also provides a method for preparing the above-mentioned catalyst, comprising the following steps:

[0048] (1) Add the silicon source solution dropwise to the aluminum source solution and adjust the pH value to 7-10, perform an aging treatment, wash to neutrality, perform a first drying treatment and a first calcination treatment in sequence, and obtain a specific surface area of ​​not less than 350m 2 / g amorphous silicon aluminum oxide;

[0049] (2) adding a first metal salt solution to amorphous silicon aluminum oxide, dripping and stirring, and then sequentially performing an aging treatment and a second calcination treatment to obtain a first active ingredient with a surface acidity of 0.02-0.5 mmol / g; the first metal salt includes at least one of a transition metal and / or an alkaline earth metal salt;

[0050] (3) adding the zeolite molecular sieve to a second metal salt solution, and sequentially performing an ion exchange treatment, a second drying treatment, and a third calcination treatment to obtain a second active ingredient with a pore size of 2-50 nm; the second metal salt comprises at least one of a potassium salt, a sodium salt, a calcium salt, and a magnesium salt;

[0051] (4) The first active ingredient and the second active ingredient are mixed uniformly and crushed to obtain a catalyst.

[0052] Specifically, in step (1), a silicon source and an aluminum source are respectively dissolved in deionized water and stirred until completely dissolved to obtain a silicon source solution and an aluminum source solution, respectively; the silicon source solution is added dropwise to the aluminum source solution, and then ammonia water is added to the aluminum source solution to adjust the pH value to 7-10, and then an aging treatment is performed to obtain a silica-alumina gel; the silica-alumina gel is then washed with deionized water until neutral, and a first drying treatment and a first calcination treatment are performed in sequence to obtain a silica-alumina gel having a specific surface area of ​​not less than 350 m 2 / g amorphous silicon aluminum oxide;

[0053] The present invention is not limited to obtaining a specific surface area of ​​not less than 350m 2 / g of amorphous silicon aluminum oxide; in a specific embodiment, the silicon source includes at least one of silicic acid, silica sol, sodium silicate, tetraethyl orthosilicate, and tetramethyl orthosilicate; the concentration of the silicon source in the silicon source solution is 0.1-5mol / L; the aluminum source includes at least one of aluminum nitrate, aluminum chloride, aluminum sulfate, sodium aluminate, and aluminum isopropoxide; the concentration of the aluminum source in the aluminum source solution is 0.5-6mol / L; the molar ratio of silicon element in the silicon source to aluminum element in the aluminum source is (0.001-10): 1; the temperature for preparing the silicon source solution and the aluminum source solution is 30-80℃; the mass percentage of ammonia in ammonia water is 15-30%; the temperature of the aging treatment is 50-70℃, and the time is 1-5h; the temperature of the first drying treatment is 80-120℃, and the time is 10-15h; optionally, grinding treatment is required after the first drying treatment until a fine powder is formed; the temperature of the first roasting treatment is 450-700℃, and the time is 3-7h.

[0054] In step (2), a first metal salt solution including at least one of a transition metal and / or an alkaline earth metal salt is added to the amorphous silicon aluminum oxide, and the solution is stirred while dripping, and then an aging treatment and a second calcination treatment are sequentially performed to obtain a first active ingredient with a surface acidity of 0.02-0.5 mmol / g;

[0055] The present invention does not specifically limit the specific method of obtaining the first active ingredient with a surface acidity of 0.02-0.5mmol / g; in a specific embodiment, the mass ratio of amorphous silicon aluminum oxide and the first metal is 100:(1-20); the first metal salt solution includes at least one of sulfates or nitrates of magnesium, calcium, barium, potassium, cerium, zirconium, and zinc; the concentration of the first metal salt in the first metal salt solution is 0.001-10mol / L; the temperature of the aging treatment is room temperature, and the time is 12-24h; the temperature of the second calcination treatment is 450-700°C, and the time is 3-7h.

[0056] In step (3), the zeolite molecular sieve is added to a second metal salt solution comprising at least one of potassium salt, sodium salt, calcium salt, and magnesium salt, and ion exchange treatment, a second drying treatment, and a third calcination treatment are performed in sequence to obtain a second active ingredient with a pore size of 2-50 nm;

[0057] The present invention does not specifically limit the specific method for obtaining the second active ingredient with a pore size of 2-50nm; in a specific embodiment, the molar ratio of the zeolite molecular sieve to the second metal is 0.01-10; the concentration of the second metal salt in the second metal salt solution is 1.0-2.0mol / L; the zeolite molecular sieve includes at least one of mordenite, SPAO-11, SPAO-14, SAPO-34, ZSM-5, SSZ-13, and β molecular sieve; the temperature of the ion exchange treatment is 40-100°C and the time is 1-8h; the temperature of the second drying treatment is 80-120°C and the time is 6-14h; the temperature of the third calcination treatment is 450-700°C and the time is 3-7h.

[0058] In step (4), the first active ingredient and the second active ingredient are mixed evenly and crushed to obtain a catalyst;

[0059] The present invention provides a method for preparing the above-mentioned catalyst, and prepares catalysts with a specific surface area of ​​not less than 350m 2 / g of amorphous silicon aluminum oxide, a first active ingredient with a surface acidity of 0.02-0.5mmol / g and a second active ingredient with a pore size of 2-50nm, and a catalyst is obtained by physically mixing the first active ingredient and the second active ingredient. The method is simple and easy, and the prepared catalyst can have good monomethylamine selectivity while maintaining a high methanol conversion rate.

[0060] Furthermore, in step (4), the mass ratio of the first active ingredient to the second active ingredient is (70-99):(1-30); and the catalyst is crushed to a particle size of 10-40 mesh.

[0061] In another aspect, the present invention also provides an application of the above catalyst and the catalyst prepared by the above preparation method in producing monomethylamine using methanol and liquid ammonia as raw materials.

[0062] The present invention also provides an application of a catalyst for improving the methanol conversion rate and monomethylamine selectivity when monomethylamine is produced using methanol and liquid ammonia as raw materials.

[0063] Hereinafter, a catalyst provided by the present invention is described in detail through specific examples.

[0064] Example 1

[0065] (1) 2.5 ml of a 0.5 mol / L silicon source solution (tetraethyl orthosilicate) is added dropwise to 150 ml of a 2 mol / L aluminum source solution (aluminum nitrate), wherein the molar ratio of the silicon source to the aluminum source is 0.0042:1, the pH value is adjusted to 8 with 27% ammonia water, the mixture is aged at 50-70° C. for 1-5 h, washed to neutrality, dried at 80-120° C. for 10-15 h, ground to fine powder, and calcined at 450-700° C. for 3-7 h to obtain an amorphous silicon aluminum oxide having a chemical formula of 0.5Al2O3·0.0042SiO2;

[0066] (2) adding 0.1 mol / L, specifically 5 ml, of a first metal salt solution (zirconium nitrate) to amorphous silicon aluminum oxide, dripping and stirring, wherein the mass ratio of amorphous silicon aluminum oxide to the first metal is 100:17; then aging treatment at room temperature for 12 h, and second calcination treatment at 550° C. for 5 h, to obtain a first active ingredient;

[0067] (3) adding 3 g of hydrogen-type zeolite molecular sieve to 1.5 mol / L 30 ml of a second metal salt solution (potassium nitrate), wherein the molar ratio of the zeolite molecular sieve to the second metal is 0.15; sequentially subjecting the mixture to an ion exchange treatment at 60° C. for 3 h, a second drying treatment at 110° C. for 10 h, and a third calcination treatment at 550° C. for 5 h to obtain a second active ingredient;

[0068] (4) The first active ingredient and the second active ingredient are mixed uniformly in a mass ratio of 4:1, and crushed into 40 meshes to obtain a catalyst.

[0069] Example 2

[0070] The difference between this embodiment and embodiment 1 is that in step (4), the mass ratio of the first active ingredient to the second active ingredient is 3:1.

[0071] Example 3

[0072] The difference between this embodiment and embodiment 1 is that in step (1), the molar ratio or mass ratio of the silicon source to the aluminum source is 4.02:1, and an amorphous silicon aluminum oxide with a chemical formula of 0.22Al2O3·0.78SiO2 is obtained.

[0073] Example 4

[0074] The difference between this embodiment and embodiment 1 is that in step (2), the mass ratio of amorphous silicon aluminum oxide to the first metal is 4:1.

[0075] Example 5

[0076] The difference between this embodiment and embodiment 1 is that in step (3), the molar ratio of the zeolite molecular sieve to the second metal is 0.05:1.

[0077] Example 6

[0078] The difference between this embodiment and embodiment 1 is that in step (4), the particles are crushed to 60 mesh.

[0079] Example 7

[0080] The difference between this embodiment and embodiment 1 is that in step (2), the first metal salt solution is indium nitrate.

[0081] Example 8

[0082] The difference between this embodiment and embodiment 1 is that in step (3), the zeolite molecular sieve is a sodium-type molecular sieve.

[0083] Comparative Example 1

[0084] The difference between this comparative example and Example 1 is that it only includes steps (1) and (2), and the first active component obtained in step (2) is used as a catalyst.

[0085] Comparative Example 2

[0086] The difference between this comparative example and Example 1 is that it only includes step (3), and the second active component obtained in step (3) is used as a catalyst.

[0087] Comparative Example 3

[0088] The difference between this comparative example and Example 1 is that step (1) is not included, and the amorphous silicon aluminum oxide in step (2) is replaced by SAPO-18 common zeolite.

[0089] Comparative Example 4

[0090] The difference between this comparative example and Example 1 is that step (2) is not performed, and the amorphous silicon aluminum oxide obtained in step (1) is used as the first active ingredient.

[0091] Comparative Example 5

[0092] The difference between this comparative example and Example 1 is that in step (2), the first metal salt solution is lithium nitrate.

[0093] Comparative Example 6

[0094] The difference between this comparative example and Example 1 is that in step (3), the second metal salt solution is zinc nitrate.

[0095] Comparative Example 7

[0096] The difference between this comparative example and Example 1 is that in step (3), the pH value is adjusted to 11.

[0097] Test Example 1

[0098] The catalysts obtained in the above examples and comparative examples were tested. The specific surface area and pore size of the catalysts were tested using a physical adsorption instrument; the acidity of the catalysts was tested using a chemical adsorption instrument; and methanol and liquid ammonia were used as raw materials at 425°C and normal pressure with a space velocity of 12000 ml / h / g cat , analyzing the product by gas chromatography instrument;

[0099] The calculation formula for methanol conversion is: The formula for calculating the selectivity of monomethylamine is:

[0100] The above results are shown in Table 1.

[0101] Table 1

[0102]

[0103] The present invention provides a catalyst comprising a first active component and a second active component, wherein the first active component comprises amorphous silicon aluminum oxide and an oxide of a first metal supported on at least a portion of the surface of the amorphous silicon aluminum oxide, wherein the first metal comprises a transition metal and / or an alkaline earth metal; and the specific surface area of ​​the first active component is not less than 350 m 2 / g, and the surface acidity is 0.02-0.5mmol / g; the second active ingredient includes a zeolite molecular sieve exchanged with a second metal ion, and the second metal includes at least one of potassium, calcium, sodium and magnesium; the pore size of the second active ingredient is 2-50nm; the two active ingredients are specifically modified and modified by the above-mentioned specific metals, so that the first active ingredient improves the methanol conversion rate and the second active ingredient improves the monomethylamine selectivity, so that the prepared catalyst can have a good monomethylamine selectivity while maintaining a high methanol conversion rate.

[0104] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A catalyst, characterized in that including a first active ingredient and a second active ingredient; The first active component includes amorphous silicon aluminum oxide and an oxide of a first metal supported on at least a portion of the surface of the amorphous silicon aluminum oxide, wherein the first metal includes a transition metal and / or an alkaline earth metal; and the specific surface area of ​​the first active component is not less than 350 m 2 / g, surface acidity is 0.02-0.5mmol / g; The second active component includes a zeolite molecular sieve exchanged with a second metal ion, wherein the second metal includes at least one of potassium, calcium, sodium and magnesium; and the pore size of the second active component is 2-50 nm.

2. The catalyst according to claim 1, characterized in that The mass ratio of the first active ingredient to the second active ingredient is (70-99):(1-30).

3. The catalyst according to claim 1 or 2, characterized in that The chemical formula of the amorphous silicon aluminum oxide is xAl2O3·ySiO2, wherein 0.49≤x≤0.99, 0.001≤y≤0.

67.

4. The catalyst according to any one of claims 1 to 3, characterized in that The mass ratio of the amorphous silicon aluminum oxide to the first metal is 100:(1-20).

5. The catalyst according to any one of claims 1 to 4, characterized in that The molar ratio of the zeolite molecular sieve to the second metal is (0.01-10):

1.

6. The catalyst according to any one of claims 1 to 5, characterized in that The particle size of the catalyst is 10-40 meshes.

7. The catalyst according to any one of claims 1 to 6, characterized in that The first metal includes at least one of magnesium, calcium, barium, potassium, cerium, zirconium and zinc.

8. The catalyst according to any one of claims 1 to 4, characterized in that The zeolite molecular sieve is an ammonium type and / or a hydrogen type zeolite molecular sieve; and / or, The zeolite molecular sieve includes at least one of mordenite, SPAO-11, SPAO-14, SAPO-34, ZSM-5, SSZ-13, and β molecular sieve.

9. A method for preparing the catalyst according to any one of claims 1 to 8, characterized in that: The following steps are involved: (1) Add the silicon source solution dropwise to the aluminum source solution and adjust the pH value to 7-10, perform an aging treatment, wash to neutrality, perform a first drying treatment and a first calcination treatment in sequence, and obtain a specific surface area of ​​not less than 350m 2 / g amorphous silicon aluminum oxide; (2) adding a first metal salt solution to the amorphous silicon aluminum oxide, stirring while dripping, and then sequentially performing an aging treatment and a second calcination treatment to obtain a first active ingredient with a surface acidity of 0.02-0.5 mmol / g; the first metal salt comprises at least one of a transition metal and / or an alkaline earth metal salt; (3) adding the zeolite molecular sieve to a second metal salt solution, and sequentially performing an ion exchange treatment, a second drying treatment, and a third calcination treatment to obtain a second active ingredient with a pore size of 2-50 nm; the second metal salt comprises at least one of a potassium salt, a sodium salt, a calcium salt, and a magnesium salt; (4) The first active ingredient and the second active ingredient are mixed uniformly and crushed to obtain a catalyst.

10. Use of the catalyst according to any one of claims 1 to 8 or the catalyst prepared by the preparation method according to claim 9 in producing monomethylamine using methanol and liquid ammonia as raw materials.

Citation Information

Cited By

  • Methane-to-methylamine hydrochloride green synthesis method based on continuous flow technology

    CN122079788A

  • Composite modified adsorption material, preparation method and application thereof

    CN122806452A