Sorting method for polymetallic ore poor in indium tin antimony

Through multi-stage grinding and flotation technology, combined with particle-grade treatment and agent ratio, the problems of high separation difficulty and low tin recovery in indium-bearing tin antimony polymetallic ore are solved, and efficient tin and antimony recovery is achieved.

CN119016181APending Publication Date: 2024-11-26LIUZHOU HUAXI COLORED DESIGN & RESEARCH INSTITUTE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411402811.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-09
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Indium-bearing tin antimony polymetallic ores, the content of metal elements such as indium, tin, antimony is low and complex and symbiotic, which makes it difficult to sort, cassiter can easily be crushed and dissociated inadequately, and the tin recovery rate is low.

Method used

Multi-stage grinding and flotation technology is adopted, including crushing, screening, rod milling, ball milling, floating shaker sorting and sulfide ore mixed flotation. It is accurately separated by different particle grade treatment and agent ratios, combined with capture The use of collectors, inhibitors and bubble agents is carried out in one coarse selection, secondary selection and secondary scanning.

Benefits of technology

It effectively reduces the over-milling phenomenon of cassiterite, improves the recovery rate of tin, and realizes accurate separation of elements in each stage. The recovery rate of antimony reaches more than 86%, improving the separation recovery rate.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a sorting method of lean indium tin antimony polymetallic ore, which comprises the following steps: (1) crushing the lean indium tin antimony polymetallic ore, carrying out first-stage ore grinding, then screening the lean indium tin antimony polymetallic ore with the screening fraction of 1mm, grading oversize products, carrying out second-stage ore grinding according to different fractions, carrying out rod milling and ball milling on the oversize products with the second-stage ore grinding comprising rod milling and ball milling, carrying out rod milling on the materials with the fraction of more than 2mm, and carrying out ball milling on the materials with the fraction of more than 2mm; carrying out ball milling on the particles with the particle size of 2 mm or below; and (2) grading the discharged ore after rod milling, feeding the discharged ore with the particle size of less than 1.5 mm into a floatation table for separation to obtain coarse-grain tin metal, middlings and tailings, returning the middlings to the rod milling, feeding the tailings into three-section grinding, and grading the discharged ore after three-section grinding. According to the method, the over-crushing phenomenon of cassiterite is effectively reduced, the problem that the grinding granularity of sulfide ore is too coarse is solved, the recovery rate of tin is increased, proper flotation reagents are adopted in all stages, precise separation of all elements in the ore is achieved, and the separation recovery rate is increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ore sorting, and in particular to a method for sorting indium-tin-antimony-poor polymetallic ore. Background Art

[0002] At present, with the continuous exploitation of mineral resources, most of them are left with low-grade, finely dispersed and difficult-to-process ores, and it is becoming increasingly difficult to separate metals from them. Poor indium tin antimony polymetallic ore is an ore containing multiple metal elements such as indium, tin, and antimony. The content of these metal elements is relatively low, so this type of ore is called "poor" ore, usually sulfide ore. Although the content of indium, tin, antimony, etc. in poor indium tin antimony polymetallic ore is relatively low, metals such as indium, tin, and antimony have a wide range of applications in modern industry, such as electronics, chemical industry, metallurgy, etc., and they still have certain recycling value. However, this type of polymetallic ore has many types, complex symbiosis, and large differences in floatability, which makes separation difficult. Cassiterite in the ore is easily over-crushed and insufficiently dissociated, and the tin recovery rate is low. Summary of the invention

[0003] The object of the present invention is to provide a method for separating indium-tin-antimony polymetallic ores poor in indium, tin and antimony, so as to solve the problems existing in the background technology.

[0004] To achieve the above object, the present invention provides the following technical solution: a method for separating indium-tin-antimony-poor polymetallic ore, comprising the following steps:

[0005] (1) crushing the indium-tin-antimony-poor polymetallic ore, performing primary grinding and then screening, the screening particle size is 1 mm, the sieve material is graded and secondary grinding is performed according to different particle sizes, the secondary grinding includes rod milling and ball milling, the rod mill is used for particles above 2 mm, and the ball mill is used for particles below 2 mm;

[0006] (2) The discharge from the rod mill is classified, and the particles below 1.5 mm enter the table flotation shaker for sorting to obtain coarse tin metal, medium ore and tailings. The medium ore returns to the rod mill, and the tailings enter the third-stage grinding, which is ball milling. After the discharge from the third-stage grinding is classified, the particles below 0.5 mm enter the sulfide ore mixed flotation, and the particles above 0.5 mm return to the second-stage grinding;

[0007] (3) After the ball mill discharge of the second stage grinding is classified, the particles below 1.5 mm enter the table flotation shaker for sorting, and the particles below 0.5 mm enter the sulfide ore mixed flotation. The table flotation shaker is added with reagents, which include collectors and inhibitors. The collector is a mixture of benzohydroxamic acid and cyclohexane acid, and the inhibitor is zinc sulfate. Based on the weight of the ore pulp, the collector dosage is 100-120g / t, and the inhibitor dosage is 50-70g / t.

[0008] (4) The mixed flotation of sulfide ore adopts primary roughing, secondary cleaning and secondary scavenging. The flotation reagents for roughing include collectors, depressants and bubbling agents. The collectors are xanthate mixture and ethylthiocyanate, the depressants are zinc sulfate and the bubbling agent is No. 2 oil. In roughing, the amount of collector is 300-400g / t, the amount of depressants is 1000-1500g / t and the amount of frother is 30-50g / t based on the weight of ore pulp. The flotation reagents for cleaning include depressants, the depressants are zinc sulfate, During the first concentration, the amount of inhibitor is 500-600g / t based on the weight of the ore pulp; during the second concentration, the amount of inhibitor is 300-400g / t based on the weight of the ore pulp; the flotation reagents for scavenging include collectors. During the first scavenging, the collectors are a mixture of xanthate and ethylthiocyanate, and the amount of collector is 50-70g / t based on the weight of the ore pulp. During the second scavenging, the collectors are a mixture of butyl ammonium black medicine and aniline black medicine, and the amount of collector is 30-40g / t based on the weight of the ore pulp.

[0009] As a preferred embodiment of the present technical solution, the material on the screen is classified by a jig, and the discharge after rod milling and ball milling is classified by a spiral classifier, and the balls of the ball mill are forged balls.

[0010] As a preferred embodiment of the present technical solution, the mass ratio of benzohydroxamic acid to cyclohexaneic acid in the collector of step (3) is 2:1.

[0011] As a preferred embodiment of the present technical solution, the slurry concentration of the mixed flotation of sulfide ore is 40-60%.

[0012] As a preferred embodiment of the present technical solution, the mass ratio of the xanthate mixture to ethyl thiocyanate is 3:(1-1.5).

[0013] As a preferred embodiment of the present technical solution, the xanthate mixture is a mixture of ethyl xanthate, isobutyl xanthate and amyl xanthate.

[0014] Compared with the prior art, the present invention has the following beneficial effects:

[0015] 1. The present invention performs multi-stage grinding according to the particle size, effectively reduces the over-crushing of cassiterite, solves the problem of too coarse grinding particle size of sulfide ore, and improves the recovery rate of tin.

[0016] 2. The present invention uses primary roughing, secondary cleaning and secondary scavenging to sort the indium-tin-antimony polymetallic ore, and sorts indium and antimony on the basis of selecting tin. The recovery rate of antimony reaches more than 86%.

[0017] 3. The present invention adopts suitable flotation reagents at each stage to achieve accurate separation of elements in the ore and improve separation recovery rate. DETAILED DESCRIPTION

[0018] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0019] Example 1

[0020] In the indium-tin-antimony polymetallic ore poor in indium, tin and antimony, the analysis results of the content of each element are: Sn 0.23%, Pb 0.31%, Sb 0.19%, Zn 2.37%, S 9.14%, As 0.72%, Fe 9.04%, Cu 0.085%, SiO2 72.35%, Al2O3 1.19%, CaO 2.08%, Cd 0.083%, In 0.016%, Ag 2.19%.

[0021] The separation method of the indium-tin-antimony-poor polymetallic ore comprises the following steps:

[0022] (1) crushing the indium-tin-antimony polymetallic ore, performing primary grinding and then screening, the screening particle size is 1 mm, the screened material is classified by a jig and secondary grinding is performed according to different particle sizes, the secondary grinding includes rod milling and ball milling, the rod mill is used for particles above 2 mm, and the ball mill is used for particles below 2 mm;

[0023] (2) The discharge from the rod mill is classified by a spiral classifier, and the particles below 1.5 mm enter the table flotation shaker for sorting to obtain coarse tin metal, medium ore and tailings. The medium ore returns to the rod mill, and the tailings enter the third-stage grinding, which is a ball mill. The discharge from the third-stage grinding is classified by a spiral classifier, and the particles below 0.5 mm enter the sulfide ore mixed flotation, and the particles above 0.5 mm return to the second-stage grinding;

[0024] (3) After the ball mill discharge of the second stage grinding is classified, the ore with a particle size below 1.5 mm enters the table flotation shaker for sorting, and the ore with a particle size below 0.5 mm enters the sulfide ore mixed flotation. The table flotation shaker is added with reagents, which include collectors and inhibitors. The amount of collector is 100 g / t based on the weight of the ore pulp. The collector is a mixture of benzohydroxamic acid and cyclohexanecarboxylic acid, with a mass ratio of benzohydroxamic acid to cyclohexanecarboxylic acid of 2:1. The inhibitor is zinc sulfate, and the inhibitor dosage is 70 g / t. The balls used in the ball mill are forged balls.

[0025] (4) The mixed flotation of sulfide ore adopts primary roughing, secondary cleaning and secondary scavenging, and the slurry concentration of the mixed flotation of sulfide ore is 60%. The flotation reagents of the roughing include collectors, depressants and bubble agents. The collectors are xanthate mixture and ethylthiocyanate, and the mass ratio of xanthate mixture to ethylthiocyanate is 3:1. The xanthate mixture is a mixture of ethyl xanthate, isobutyl xanthate and amyl xanthate, and the mass ratio of ethyl xanthate, isobutyl xanthate and amyl xanthate is 1:1:1.5. The inhibitor is zinc sulfate, and the bubbling agent is No. 2 oil. During roughing, the amount of collector is 300g / t, the amount of inhibitor is 1500g / t, and the amount of frother is 50g / t, calculated on the weight of the ore pulp; the flotation reagent for fine selection includes an inhibitor, and the inhibitor is zinc sulfate. During the first fine selection, the amount of inhibitor is 600g / t, calculated on the weight of the ore pulp; during the second fine selection, the amount of inhibitor is 400g / t, calculated on the weight of the ore pulp; the flotation reagent for scavenging selection includes a collector. During the first scavenging selection, the collector is a mixture of xanthate and ethylthiocyanate, and the amount of collector is 70g / t, calculated on the weight of the ore pulp; during the second scavenging selection, the collector is a mixture of butyl ammonium black medicine and aniline black medicine, and the amount of collector is 40g / t, calculated on the weight of the ore pulp, and the mass ratio of butyl ammonium black medicine to aniline black medicine is 1:0.8.

[0026] After the implementation of this embodiment, the tin grade is 18.34%, the tin recovery rate is 82.39%, the antimony grade is 16.32%, the antimony recovery rate is 87.49%, and the indium grade is 17.28%, and the indium recovery rate is 83.37%.

[0027] Example 2

[0028] In the indium-tin-antimony polymetallic ore poor in indium, tin and antimony in this embodiment, the analysis results of the content of each element are: Sn 0.18%, Pb 0.25%, Sb 0.21%, Zn 2.15%, S 8.23%, As 0.64%, Fe 9.24%, Cu 0.063%, SiO2 70.14%, Al2O3 1.03%, CaO 1.98%, Cd 0.096%, In 0.036%, Ag 5.75%.

[0029] The separation method of the indium-tin-antimony-poor polymetallic ore comprises the following steps:

[0030] (1) crushing the indium-tin-antimony polymetallic ore, performing primary grinding and then screening, the screening particle size is 1 mm, the screened material is classified by a jig and secondary grinding is performed according to different particle sizes, the secondary grinding includes rod milling and ball milling, the rod mill is used for particles above 2 mm, and the ball mill is used for particles below 2 mm;

[0031] (2) The discharge from the rod mill is classified by a spiral classifier, and the particles below 1.5 mm enter the table flotation shaker for sorting to obtain coarse tin metal, medium ore and tailings. The medium ore returns to the rod mill, and the tailings enter the third-stage grinding, which is a ball mill. The discharge from the third-stage grinding is classified by a spiral classifier, and the particles below 0.5 mm enter the sulfide ore mixed flotation, and the particles above 0.5 mm return to the second-stage grinding;

[0032] (3) After the ball mill discharge of the second stage grinding is classified, the ore with a particle size below 1.5 mm enters the table flotation shaker for sorting, and the ore with a particle size below 0.5 mm enters the sulfide ore mixed flotation. The table flotation shaker is added with reagents, which include collectors and inhibitors. The amount of collector is 120 g / t based on the weight of the ore pulp. The collector is a mixture of benzohydroxamic acid and cyclohexanecarboxylic acid, with a mass ratio of benzohydroxamic acid to cyclohexanecarboxylic acid of 2:1. The inhibitor is zinc sulfate, and the inhibitor dosage is 50 g / t. The balls used in the ball mill are forged balls.

[0033] (4) The mixed flotation of sulfide ore adopts primary roughing, secondary cleaning and secondary scavenging, and the slurry concentration of the mixed flotation of sulfide ore is 40%. The flotation reagents of the roughing include collectors, depressants and bubble agents. The collectors are xanthate mixture and ethylthiocyanate, and the mass ratio of xanthate mixture to ethylthiocyanate is 3:1.5. The xanthate mixture is a mixture of ethyl xanthate, isobutyl xanthate and amyl xanthate, and the mass ratio of ethyl xanthate, isobutyl xanthate and amyl xanthate is 1:1:1.5. The inhibitor is zinc sulfate, and the bubbling agent is No. 2 oil. During roughing, the amount of collector is 400g / t, the amount of inhibitor is 1000g / t, and the amount of frother is 30g / t, calculated on the weight of the ore pulp; the flotation reagent for fine selection includes an inhibitor, and the inhibitor is zinc sulfate. During the first fine selection, the amount of inhibitor is 500g / t, calculated on the weight of the ore pulp; during the second fine selection, the amount of inhibitor is 300g / t, calculated on the weight of the ore pulp; the flotation reagent for scavenging selection includes a collector. During the first scavenging selection, the collector is a mixture of xanthate and ethylthiocyanate, and the amount of collector is 50g / t, calculated on the weight of the ore pulp; during the second scavenging selection, the collector is a mixture of butyl ammonium black medicine and aniline black medicine, and the amount of collector is 30g / t, calculated on the weight of the ore pulp, and the mass ratio of butyl ammonium black medicine to aniline black medicine is 1:0.8.

[0034] After the implementation of this embodiment, the tin grade is 16.87%, the tin recovery rate is 85.81%, the antimony grade is 17.15%, the antimony recovery rate is 85.32%, and the indium grade is 16.71%, and the indium recovery rate is 81.35%.

[0035] Example 3

[0036] In the indium-tin-antimony polymetallic ore poor in indium, tin and antimony in this embodiment, the analysis results of the content of each element are: Sn 0.28%, Pb 0.75%, Sb 0.21%, Zn 2.07%, S 9.34%, As 0.82%, Fe 8.74%, Cu 0.085%, SiO2 71.25%, Al2O3 1.45%, CaO 2.63%, Cd 0.073%, In 0.103%, Ag 2.20%.

[0037] The separation method of the indium-tin-antimony-poor polymetallic ore comprises the following steps:

[0038] (1) crushing the indium-tin-antimony polymetallic ore, performing primary grinding and then screening, the screening particle size is 1 mm, the screened material is classified by a jig and secondary grinding is performed according to different particle sizes, the secondary grinding includes rod milling and ball milling, the rod mill is used for particles above 2 mm, and the ball mill is used for particles below 2 mm;

[0039] (2) The discharge from the rod mill is classified by a spiral classifier, and the particles below 1.5 mm enter the table flotation shaker for sorting to obtain coarse tin metal, medium ore and tailings. The medium ore returns to the rod mill, and the tailings enter the third-stage grinding, which is a ball mill. The discharge from the third-stage grinding is classified by a spiral classifier, and the particles below 0.5 mm enter the sulfide ore mixed flotation, and the particles above 0.5 mm return to the second-stage grinding;

[0040] (3) After the ball mill discharge of the second stage grinding is classified, the ore with a particle size below 1.5 mm enters the table flotation shaker for sorting, and the ore with a particle size below 0.5 mm enters the sulfide ore mixed flotation. The table flotation shaker is added with reagents, which include collectors and inhibitors. The amount of collector is 110 g / t based on the weight of the ore pulp. The collector is a mixture of benzohydroxamic acid and cyclohexanecarboxylic acid, with a mass ratio of benzohydroxamic acid to cyclohexanecarboxylic acid of 2:1. The inhibitor is zinc sulfate, and the inhibitor dosage is 60 g / t. The balls used in the ball mill are forged balls.

[0041] (4) The mixed flotation of sulfide ore adopts primary roughing, secondary cleaning and secondary scavenging, and the slurry concentration of the mixed flotation of sulfide ore is 50%. The flotation reagents of the roughing include collectors, depressants and bubble agents. The collectors are xanthate mixture and ethylthiocyanate, and the mass ratio of xanthate mixture to ethylthiocyanate is 3:1.2. The xanthate mixture is a mixture of ethyl xanthate, isobutyl xanthate and amyl xanthate, and the mass ratio of ethyl xanthate, isobutyl xanthate and amyl xanthate is 1:1:1.5. The inhibitor is zinc sulfate, and the bubbling agent is No. 2 oil. During roughing, the amount of collector is 350g / t, the amount of inhibitor is 1200g / t, and the amount of frother is 40g / t, calculated on the weight of the ore pulp; the flotation reagent for fine selection includes an inhibitor, and the inhibitor is zinc sulfate. During the first fine selection, the amount of inhibitor is 550g / t, calculated on the weight of the ore pulp; during the second fine selection, the amount of inhibitor is 350g / t, calculated on the weight of the ore pulp; the flotation reagent for scavenging selection includes a collector. During the first scavenging selection, the collector is a mixture of xanthate and ethylthiocyanate. Calculated on the weight of the ore pulp, the collector is 60g / t. During the second scavenging selection, the collector is a mixture of butylammonium black medicine and aniline black medicine. The mass ratio of butylammonium black medicine to aniline black medicine is 1:0.8, and the collector is 35g / t, calculated on the weight of the ore pulp.

[0042] After the implementation of this embodiment, the tin grade is 15.32%, the tin recovery rate is 83.29%, the antimony grade is 18.32%, the antimony recovery rate is 84.27%, and the indium grade is 13.82%, and the indium recovery rate is 80.35%.

[0043] Finally, it should be noted that the above-described embodiments are only specific implementations of the present invention, which are used to illustrate the technical solutions of the present invention, rather than to limit them. The protection scope of the present invention is not limited thereto. Although the present invention is described in detail with reference to the above-described embodiments, ordinary technicians in the field should understand that any technician familiar with the technical field can still modify the technical solutions recorded in the above-described embodiments within the technical scope disclosed by the present invention, or can easily think of changes, or make equivalent replacements for some of the technical features therein; and these modifications, changes or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention, and should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the protection scope of the claims.

Claims

1. A method for separating indium-tin-antimony-poor polymetallic ores, It is characterized in that The following steps are involved: (1) crushing the indium-tin-antimony-poor polymetallic ore, performing primary grinding and then screening, the screening particle size is 1 mm, the sieve material is graded and secondary grinding is performed according to different particle sizes, the secondary grinding includes rod milling and ball milling, the rod mill is used for particles above 2 mm, and the ball mill is used for particles below 2 mm; (2) The discharge from the rod mill is classified, and the particles below 1.5 mm enter the table flotation shaker for sorting to obtain coarse tin metal, medium ore and tailings. The medium ore returns to the rod mill, and the tailings enter the third-stage grinding, which is ball milling. After the discharge from the third-stage grinding is classified, the particles below 0.5 mm enter the sulfide ore mixed flotation, and the particles above 0.5 mm return to the second-stage grinding; (3) After the ball mill discharge of the second stage grinding is classified, the particles below 1.5 mm enter the table flotation shaker for sorting, and the particles below 0.5 mm enter the sulfide ore mixed flotation. The table flotation shaker is added with reagents, which include collectors and inhibitors. The collector is a mixture of benzohydroxamic acid and cyclohexane acid, and the inhibitor is zinc sulfate. The amount of collector is 100-120 g / t, and the amount of inhibitor is 50-70 g / t, based on the weight of the ore pulp; (4) The mixed flotation of sulfide ore adopts primary roughing, secondary cleaning and secondary scavenging. The flotation reagents for roughing include collectors, depressants and bubbling agents. The collectors are xanthate mixture and ethylthiocyanate, the depressants are zinc sulfate and the bubbling agent is No. 2 oil. In roughing, the amount of collector is 300-400g / t, the amount of depressants is 1000-1500g / t and the amount of frother is 30-50g / t based on the weight of ore pulp. The flotation reagents for cleaning include depressants, the depressants are zinc sulfate, During the first concentration, the amount of inhibitor is 500-600g / t based on the weight of the ore pulp; during the second concentration, the amount of inhibitor is 300-400g / t based on the weight of the ore pulp; the flotation reagents for scavenging include collectors. During the first scavenging, the collectors are a mixture of xanthate and ethylthiocyanate, and the amount of collector is 50-70g / t based on the weight of the ore pulp. During the second scavenging, the collectors are a mixture of butyl ammonium black medicine and aniline black medicine, and the amount of collector is 30-40g / t based on the weight of the ore pulp.

2. The method for separating indium-tin-antimony-poor polymetallic ores according to claim 1, Features: The material on the screen is classified by a jig, and the discharge after rod milling and ball milling is classified by a spiral classifier. The balls used in ball milling are forged balls.

3. The method for separating indium-tin-antimony-poor polymetallic ore according to claim 1, Features: The mass ratio of benzohydroxamic acid to cyclohexaneic acid in the collector of step (3) is 2:

1.

4. The method for separating indium-tin-antimony-poor polymetallic ore according to claim 1, Features: The slurry concentration of sulfide ore mixed flotation is 40-60%.

5. The method for separating indium-tin-antimony-poor polymetallic ore according to claim 1, Features: The mass ratio of the xanthate mixture to ethylthiocyanate is 3:(1-1.5).

6. The method for separating indium-tin-antimony-poor polymetallic ore according to claim 1, Features: The xanthate mixture is a mixture of ethyl xanthate, isobutyl xanthate and amyl xanthate.