Method for flotation separation of zinc mineral from high-grade lead-zinc sulfide ore
By employing a three-stage flotation separation process of zinc roughing and scavenging in high-grade sulfide lead-zinc ore, and utilizing zinc activators and collectors to separate zinc minerals at natural pH, the problems of large zinc mineral loss and unstable separation indicators were solved, achieving efficient zinc recovery and stable production.
Patent Information
- Application Number
- CN202411212836.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-26
AI Technical Summary
In high-grade sulfide lead-zinc ore, the separation of zinc minerals from tailings is hampered by problems such as large zinc mineral losses, unstable separation parameters, and a wide variety of reagents with poor selectivity, leading to unstable production.
A flotation separation process consisting of three stages of zinc roughing and three stages of zinc scavenging is adopted. Zinc activators and zinc collectors are used under natural pH conditions. The dosage of reagents is controlled and the types of reagents are reduced. The efficient separation of zinc minerals and tailings is achieved through multiple repeated flotation separation processes.
It improves the recovery rate of zinc ore, reduces the loss of zinc metal in tailings, simplifies the production process, avoids the problem of calcium buildup in pipelines under high pH conditions, and ensures the stability and economy of production.
Smart Images

Figure CN119016203A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of zinc mineral flotation separation of lead-zinc sulfide ores, and in particular to a method for flotation separation of zinc minerals from high-grade lead-zinc sulfide ores. Background Art
[0002] In the flotation separation process of zinc ore and tailings in most lead-zinc sulfide mines, lime milk is usually used as a pH adjuster. The pH value of the pulp is adjusted to 11-12 before the pulp enters the flotation process. The pyrite is suppressed by the high alkaline pulp, and then copper sulfate is added as an activator, butyl xanthate and ethyl xanthate are used as collectors, and 2# oil is used as a frother. After roughing, scavenging and concentrating processes, the zinc ore and tailings are separated. In actual production, for the flotation separation process of high-grade lead-zinc sulfide ore containing 3%-5% Pb, 22%-27% Zn, and 50g / t-60g / t of Ag, the lead-silver flotation process indicators are poor, the silver recovery rate is low, and the zinc loss in the tailings is large due to the residual tailings backwater reagents and high pH value. The main reasons for this problem are as follows: First, lime is used as a large amount of inhibitor in the separation process of zinc ore and tailings, usually at a dosage of 6-7 kg / t. During the natural degradation process of tailings backwater, Ca 2+ With CO3 2- The fine particles of calcium carbonate suspension are formed and enter the flotation process with the return water, causing calcium blockage in valves, elbows and other pipeline connection areas. 2+ OH - The lead priority flotation process in the tailings backwater inhibits the floating of lead minerals and associated precious metals such as gold and silver; second, the zinc ore in the original ore is of high grade, the zinc flotation roughing stage has a high yield, the roughing separation effect is not good, the concentrate yield is large, the concentration enrichment effect is poor, the scavenging ore circulation volume is large, and the scavenging is not thorough in the recovery of metals, resulting in a high zinc content in the tailings. Third, there are many types of flotation separation agents with poor selectivity. Collectors such as butyl xanthate and ethyl xanthate have poor selectivity for zinc sulfide minerals. For the separation of high-grade zinc sulfide minerals, a large amount of such collectors need to be added. At the same time, 2# oil needs to be added as a foaming agent, resulting in a large amount of gangue floating with the foam, and returning to the previous level of sorting process as medium ore during the selection, resulting in frequent slot running and slot bubbling at the operation site, resulting in substandard concentrate grade and large loss of zinc metal in the tailings.
[0003] Therefore, how to use economically feasible technology to separate zinc minerals from tailings in high-grade lead-zinc sulfide ores and ensure the stability of separation indicators is the key to ensuring continuous and stable production operation. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a method for flotation separation of zinc minerals from high-grade lead-zinc sulfide ore, aiming to solve the problem of large loss of zinc minerals in tailings in the existing flotation separation process of high-grade lead-zinc sulfide ore.
[0005] The technical solution of the present invention is as follows:
[0006] The present invention provides a method for flotation separation of zinc minerals from high-grade lead-zinc sulfide ore, which comprises:
[0007] Step 1, grinding the high-grade lead-zinc sulfide ore until the ore fineness is -200 mesh accounting for 65-72%, and then adjusting the mass concentration of the ore in the slurry to 30-35% to obtain a grinding slurry;
[0008] Step 2: subjecting the grinding pulp obtained in step 1 to lead and silver preferential flotation to obtain re-selected tailings pulp, and then subjecting the re-selected tailings pulp to three-stage zinc roughing operations under natural pH conditions; in the first stage of zinc roughing operation, 280-320 g / t of zinc activator and 25-30 g / t of zinc collector are added, the flotation time is 3-5 min, and the aeration volume is 2.10-2.60 m 3 / (m 2 ·min), to obtain the first roughing concentrate and the first tailings; the first tailings are subjected to the second stage zinc roughing operation, in which 200-240g / t of zinc activator and 10-20g / t of zinc collector are added, the flotation time is 3-4min, and the aeration volume is 1.10-1.40m 3 / (m 2 ·min), to obtain the second roughing concentrate and the second tailings; the second tailings are subjected to the third stage of zinc roughing operation, in which 200-240g / t of zinc activator and 10-20g / t of zinc collector are added, the flotation time is 3-4min, and the aeration volume is 1.10-1.40m 3 / (m 2 ·min), to obtain the third rougher concentrate and the third tailings; the first rougher concentrate, the second rougher concentrate and the third rougher concentrate are zinc concentrate;
[0009] Step 3: The third tailings obtained in step 2 are subjected to three-stage zinc scavenging operations under natural pH conditions to obtain three zinc scavenging mid-ranges and final tailings, and the three zinc scavenging mid-ranges are returned to the previous layer in sequence; wherein, 60-100 g / t of zinc activator and 10-15 g / t of zinc collector are added to the first stage of zinc scavenging operation, the flotation time is 3-4 min, and the aeration volume is 1.10-1.40 m 3 / (m 2 ·min); No reagent is added in the second stage of zinc scavenging operation, the flotation time is 3-4min, and the aeration volume is 1.10-1.40m 3 / (m 2 ·min); No reagent is added in the third zinc scavenging operation, the flotation time is 3-4min, and the aeration volume is 1.10-1.40m 3 / (m 2 ·min).
[0010] Optionally, the high-grade lead-zinc sulfide ore has a lead grade of 3%-5%, a zinc grade of 22%-27%, and a silver grade of 50-60 g / t.
[0011] Optionally, the zinc activator is copper sulfate, and the zinc collector is one or more of P2 and A2.
[0012] Optionally, the final tailings have a lead grade of 0.15%-0.18%, a zinc grade of 0.30%-0.40%, and a silver grade of 3-4 g / t.
[0013] Optionally, when the zinc grade of the final tailings is higher than 0.5%, 20-30 g / t of butyl xanthate or ethyl xanthate is added in the third zinc roughing operation in step 2.
[0014] Optionally, the lead and silver preferential flotation in step 2 adopts a flotation separation process of one roughing, three fines and three sweeps.
[0015] Optionally, in the one rough three fine three sweep flotation separation process, the lead collector used is Pa, the zinc depressants are ZnSO4 and Na2SO3, and the pyrite depressants are EMY101 and Na2SO3.
[0016] The present invention has the following beneficial effects:
[0017] (1) The present invention controls the concentrate yield in the roughing stage by controlling the dosage of the reagents and reducing the types of flotation reagents under the joint action of the zinc activator and the zinc collector, thereby improving the quality of the roughing concentrate. The roughing concentrate can be used as the product zinc concentrate without the need for fine separation, thereby shortening the production process. In addition, during the flotation separation process, as the zinc concentrate is continuously produced, the roughing operation is naturally divided into different grade gradients, and the flotation separation process is repeated to achieve the separation of zinc ore and tailings. The zinc recovery rate can reach more than 96%, greatly reducing the loss of zinc ore in the tailings.
[0018] (2) The present invention can separate zinc ore from tailings under natural pH conditions, eliminating the commonly used lime milk addition process and reducing the Ca content in tailings return water. 2+ The content of Ca 2+ Solubility decreases, Ca 2+ Crystallization and precipitation lead to calcium deposition in the return water pipeline, which requires frequent shutdowns for maintenance, thus ensuring the continuous and stable production of the concentrator.
[0019] (3) The present invention solves the problems of multiple types of zinc mineral flotation reagents, large dosage, high zinc metal content in tailings, long process, and high pH tailings backwater affecting the recovery of precious metals such as gold and silver in the production of medium- and high-grade lead-zinc sulfide ores. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 The present invention provides a process flow chart of the method for flotation separation of zinc minerals from high-grade lead-zinc sulfide ore. DETAILED DESCRIPTION
[0021] The present invention provides a method for flotation separation of zinc minerals from high-grade lead-zinc sulfide ore. In order to make the purpose, technical scheme and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0022] It should also be noted that, in order to avoid obscuring the present invention due to unnecessary details, only structures and / or processing steps closely related to the scheme of the present invention are shown in the drawings, while other details that are not closely related to the present invention are omitted.
[0023] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.
[0024] The embodiment of the present invention provides a method for flotation separation of zinc minerals from high-grade lead-zinc sulfide ore, which comprises:
[0025] Step 1, grinding the high-grade lead-zinc sulfide ore until the ore fineness is -200 mesh accounting for 65-72%, and then adding water to adjust the mass concentration of the ore in the slurry to 30-35%, to obtain a grinding slurry;
[0026] Step 2: subjecting the grinding pulp obtained in step 1 to lead and silver preferential flotation to obtain re-selected tailings pulp, and then subjecting the re-selected tailings pulp to three-stage zinc roughing operations under natural pH conditions; in the first stage of zinc roughing operation, 280-320 g / t of zinc activator and 25-30 g / t of zinc collector are added, the flotation time is 3-5 min, and the aeration volume is 2.10-2.60 m 3 / (m 2·min), to obtain the first roughing concentrate and the first tailings; the first tailings are subjected to the second stage zinc roughing operation, in which 200-240g / t of zinc activator and 10-20g / t of zinc collector are added, the flotation time is 3-4min, and the aeration volume is 1.10-1.40m 3 / (m 2 ·min), to obtain the second roughing concentrate and the second tailings; the second tailings are subjected to the third stage of zinc roughing operation, in which 200-240g / t of zinc activator and 10-20g / t of zinc collector are added, the flotation time is 3-4min, and the aeration volume is 1.10-1.40m 3 / (m 2 ·min), to obtain the third rougher concentrate and the third tailings; the first rougher concentrate, the second rougher concentrate and the third rougher concentrate are zinc concentrate;
[0027] Step 3: The third tailings obtained in step 2 are subjected to three-stage zinc scavenging operations under natural pH conditions to obtain three zinc scavenging mid-ranges and final tailings, and the three zinc scavenging mid-ranges are returned to the previous layer in sequence; wherein, 60-100 g / t of zinc activator and 10-15 g / t of zinc collector are added to the first stage of zinc scavenging operation, the flotation time is 3-4 min, and the aeration volume is 1.10-1.40 m 3 / (m 2 ·min); No reagent is added in the second stage of zinc scavenging operation, the flotation time is 3-4min, and the aeration volume is 1.10-1.40m 3 / (m 2 ·min); No reagent is added in the third zinc scavenging operation, the flotation time is 3-4min, and the aeration volume is 1.10-1.40m 3 / (m 2 ·min).
[0028] The method provided by the embodiment of the present invention is a method for flotation separation of zinc minerals from high-grade sulfide lead-zinc ore under natural pH value and no concentration operation conditions. The lead concentrate and silver metal are first separated and recovered by lead-silver priority flotation operation. The zinc flotation adopts a simple process flow of three-stage zinc roughing operation and three-stage zinc scavenging operation to achieve the separation of zinc concentrate and tailings. By controlling the dosage of reagents and reducing the types of flotation reagents (only zinc activators and zinc collectors) under the joint action of zinc activators and zinc collectors, the concentrate yield in the roughing stage is controlled, the quality of the roughing concentrate is improved, and the roughing concentrate can be used as a product zinc concentrate without the need for concentration operation, shortening the production process, reducing the difficulty of operation on the operation site, and reducing the production cost. In addition, in the process of flotation separation, as the zinc concentrate is continuously produced, the roughing operation is naturally divided into different grade gradients, and the flotation separation process is repeated to achieve the separation of zinc minerals and tailings. The method of the invention realizes efficient separation of zinc ore and tailings, reduces the content of zinc metal in tailings, and improves the recovery rate of zinc metal. The zinc recovery rate can reach more than 96%, which greatly reduces the loss of zinc ore in tailings.
[0029] The embodiment of the present invention can separate zinc ore from tailings under natural pH conditions, eliminates the commonly used lime milk addition step, and does not require a concentration operation. By controlling the dosage of reagents and reducing the types of flotation reagents, the concentrate yield in the roughing stage is controlled, the quality of the roughing concentrate is improved, the content of zinc metal in the tailings is reduced, and the recovery rate of zinc metal is improved. The problem of many types of reagents, large dosage, high zinc content in tailings, and long process in the zinc flotation operation of high-grade lead-zinc sulfide ore in production is solved, and the problem of frequent shutdown and maintenance in winter due to calcium deposition in the return water pipeline in high pH zinc concentration operations in high-cold areas is solved. The invention has a very high industrial application prospect.
[0030] The natural pH value of the embodiment of the present invention refers to a pH of 7.0-7.5.
[0031] In one embodiment, the zinc grade of the high-grade lead-zinc sulfide ore is 22%-27%.
[0032] In one embodiment, the high-grade lead-zinc sulfide ore has a lead grade of 3%-5%, a zinc grade of 22%-27%, and a silver grade of 50-60 g / t.
[0033] In one embodiment, the zinc activator is copper sulfate, and the zinc collector is one or more of P2 and A2. The collector P2 is a mineral processing agent containing thiocyanate, hydroxy fatty alcohol, etc., and the content of mineral processing active substances is ≥ 98%, and the collector A2 is a mineral processing agent containing thiocyanate, thiocyanate, hydrocarbon oil, and the content of mineral processing active substances is ≥ 98%.
[0034] In one embodiment, the final tailings have a lead grade of 0.15%-0.18%, a zinc grade of 0.30%-0.40%, and a silver grade of 3-4 g / t.
[0035] In one embodiment, when the zinc grade of the final tailings is higher than 0.5%, 20-30 g / t of butyl xanthate or ethyl xanthate is added in the third stage zinc roughing operation in step 2.
[0036] In one embodiment, the lead-silver preferential flotation operation in step 2 can reduce the pH value and calcium ion content of the tailings return water, and can improve the recovery rate of lead metal and silver metal, thereby achieving the separation and recovery of zinc concentrate, lead concentrate and silver metal in high-grade sulfide lead-zinc ore, and reducing the loss of metals such as zinc, lead and silver in the tailings.
[0037] In one embodiment, the lead-silver preferential flotation adopts a flotation separation process of one roughing, three fines and three sweeps, wherein the lead collector used is Pa, the zinc inhibitors are ZnSO4 and Na2SO3, and the pyrite inhibitors are EMY101 and Na2SO3. The collector Pa is a mineral processing agent containing dialkyl dithiophosphate, thiocyanate, etc., and the content of mineral processing active substances is ≥60%, and the inhibitor EMY101 is a mineral processing agent containing modified starch, sodium hydroxide, water and other substances.
[0038] In this embodiment, the one coarse three fine three sweep flotation separation process is a commonly used process in the art and is not particularly limited herein.
[0039] The present invention will be further described below by means of specific examples.
[0040] In the following examples, the reagents used are all commercially available products. The dosage of the reagents is based on the mass of the high-grade lead-zinc sulfide ore. For example, the dosage of the zinc activator copper sulfate is 240 g / t, that is, 240 g of copper sulfate is added per ton of high-grade lead-zinc sulfide ore.
[0041] Example 1
[0042] This embodiment provides a method for flotation separation of zinc minerals from a high-grade lead-zinc sulfide ore. In terms of mass percentage, the high-grade lead-zinc sulfide ore in this embodiment contains 3.95% Pb, 24.17% Zn, and 56.61 g / t Ag. Figure 1 As shown, the specific steps include:
[0043] S1. The flotation separation process of "lead and silver priority flotation - tailings selection for zinc" is adopted to grind the high-grade sulfide lead-zinc ore to a fineness of -200 mesh, accounting for 71.44%, and then water is added to adjust the mass concentration of the ore in the slurry to 33.5% to obtain the grinding slurry. The obtained grinding slurry is then subjected to a lead-silver priority flotation operation. The lead-silver priority flotation operation adopts a flotation separation process of "one roughing, three finishing and three sweeping", specifically, the grinding slurry is first subjected to a lead roughing operation; in the lead roughing operation, 60g / t of lead collector Pa, 80g / t of zinc depressant ZnSO4, 80g / t of pyrite depressant Na2SO3, and 20g / t of pyrite depressant EMY101 are added to obtain a lead roughing concentrate, and the lead roughing concentrate enters the lead concentrating operation. The concentrates obtained from the three lead concentrating operations enter the next level of concentrating operation in turn until the three concentrations are completed to obtain lead concentrate 1, and the intermediate ore is returned to the upper level operation step by step; the tailings obtained from the lead roughing operation are subjected to three-stage lead sweeping operations to obtain three lead sweeping middlings and re-selected tailings, and the three lead sweeping middlings are returned to the upper level operation step by step; among them, 30g / t of lead collector Pa and 40g / t of zinc depressant ZnSO4 are added to the first stage of lead sweeping operation. After the lead and silver preferential flotation operation, the re-selected tailings slurry is obtained, and then the zinc flotation operation is performed on the re-selected tailings slurry.
[0044] S2, the tailings pulp is subjected to three-stage zinc roughing operation under natural pH conditions. In the first stage of zinc roughing operation, 320g / t of zinc activator copper sulfate and 30g / t of zinc collector P2 are added and stirred in a stirring barrel for 8-10 minutes. The pulp is fed into a flotation machine for separation and roughing I. The flotation time is 4min and the aeration volume is 2.46m 3 / (m 2 ·min), the roughing concentrate is zinc concentrate 1, and the roughing tailings I are separated and fed to the next roughing stage.
[0045] S3, in the second zinc roughing operation, 240g / t of zinc activator copper sulfate and 20g / t of zinc collector P2 were added, the flotation time was 3min, and the aeration volume was 1.36m 3 / (m 2 ·min), the roughing concentrate is zinc concentrate 2, and the roughing II tailings are separated and fed to the next roughing stage.
[0046] S4, in the third zinc roughing operation, 200g / t of zinc activator copper sulfate and 20g / t of zinc collector P2 were added, the flotation time was 3min, and the aeration volume was 1.13m 3 / (m 2 ·min), the roughing concentrate is zinc concentrate 3, and the roughing III tailings are separated and fed to the next stage of separation and scavenging.
[0047] S5, separation of roughing III tailings under natural pH conditions for three-stage zinc scavenging operations, three zinc scavenging middlings and final tailings are obtained, and the three zinc scavenging middlings are returned to the previous layer in turn; in the first stage of zinc scavenging operation, 80g / t of zinc activator copper sulfate and 15g / t of zinc collector P2 are added, the flotation time is 3min, and the aeration volume is 1.36m 3 / (m 2 ·min); No reagent was added in the second zinc scavenging operation, the flotation time was 3min, and the aeration volume was 1.29m 3 / (m 2 ·min); No reagent was added in the third zinc scavenging operation, the flotation time was 3min, and the aeration volume was 1.19m 3 / (m 2 ·min).
[0048] The concentrate grade, recovery rate, yield and other index data obtained in this example are shown in Table 1.
[0049] Comparative Example 1
[0050] Comparative Example 1 uses the same ore sample as Example 1, and adopts the flotation process of "lead and silver priority flotation-reselection of tailings for zinc selection". The lead and silver priority flotation process adopts the same "one coarse, three fine, and three sweeping" flotation separation process as in Example 1, but the lead mineral collector used therein is 25# black medicine, and the zinc mineral inhibitor is ZnSO4.
[0051] Then, the flotation process of reselected tailings for zinc selection was carried out, the pH value of the tailings slurry was adjusted to 11-12 with lime, the dosage was 6kg / t, the collector was xanthate (butyl xanthate: ethyl xanthate = 1:1), the dosage was 160g / t, the activator was copper sulfate, the dosage was 440g / t, the frother was 2# oil, the dosage was 50g / t. Then the operation was carried out according to the same flotation process of "reselected tailings for zinc selection" as in Example 1.
[0052] The concentrate grade, recovery rate, yield and other index data obtained in Comparative Example 1 are shown in Table 2.
[0053] Comparative Example 2
[0054] Comparative Example 2 uses the same ore sample as Example 1, and adopts the flotation process of "lead-silver priority flotation-reselection tailings zinc selection". The lead-silver priority flotation adopts the same process as in Example 1. In the reselection tailings zinc selection flotation process, a concentration process is added after the separation roughing process I of Example 1, and flotation separation is performed according to "one roughing, one fine and three sweeping", specifically, the reselection tailings slurry is subjected to three stages of zinc roughing operations under natural pH conditions; 320g / t of zinc activator copper sulfate and 30g / t of zinc collector P2 are added to the first stage of zinc roughing operation, the flotation time is 4min, and the inflation volume is 2.46m3 / (m 2 ·min), to obtain a first roughing concentrate and a first tailings; the first roughing concentrate enters a first concentration operation to obtain a zinc concentrate and a middling, the zinc concentrate is output as a product, and the middling returns to the first zinc roughing operation; subsequently, the second zinc roughing operation, the third zinc roughing operation and the three-stage zinc scavenging operation in Example 1 are continued.
[0055] The concentrate grade, recovery rate, yield and other index data obtained in Comparative Example 2 are shown in Table 3.
[0056] Table 1
[0057]
[0058] Table 2
[0059]
[0060] Table 3
[0061]
[0062] Among them, 1-PbK in Table 1, Table 2 and Table 3 represents the lead concentrate 1 obtained by the lead-silver priority flotation process, 1-ZnK1 represents the zinc concentrate 1 obtained by the first stage zinc roughing operation, 2-ZnK1 represents the zinc concentrate obtained by the first stage zinc roughing operation after the first stage zinc roughing operation, 1-ZnK2 represents the zinc concentrate 2 obtained by the second stage zinc roughing operation, 1-ZnK3 represents the zinc concentrate 3 obtained by the third stage zinc roughing operation, and 1-X represents the final tailings obtained after three stages of zinc scavenging operations.
[0063] According to the data in Table 1, it can be seen that in Example 1, the flotation separation process is carried out under natural pH value and no concentration operation conditions. The raw ore contains 3.95% Pb, 24.17% Zn, and 56.61 g / t Ag. The final tailings contain 0.16% Pb, 0.34% Zn, and 3 g / t Ag. The metal recovery rates are 94.90% Pb, 96.49% Zn, and 81.03% Ag.
[0064] According to the data in Table 2, the raw ore of Example 1 was subjected to the flotation process of "lead and silver priority flotation-reselection of tailings for zinc selection" under a high alkaline environment, and the tailings obtained contained 0.22% Pb, 1.32% Zn, and 4 g / t Ag, and the metal recovery rates were Pb 93.16%, Zn 94.60%, and Ag 79.24%. It can be seen that due to the high alkaline environment and Ca in the return water of Comparative Example 1, 2+The metal grade of the final tailings increased by 0.06% Pb, 0.98% Zn, and 1 g / t Ag relative to that in Example 1, and the metal recovery rate decreased by 1.74% Pb, 1.89% Zn, and 1.79% Ag relative to that in Example 1.
[0065] According to the data in Table 3, it can be seen that in Comparative Example 2, a concentration operation is added on the basis of Example 1 for separation, and the zinc grade of zinc concentrate 1 is increased by 2.34%, but the metal content in the final tailings is increased. The final tailings contain Pb 0.18%, Zn 0.93%, Ag 4g / t, and the metal recovery rates are Pb 94.79%, Zn 95.32%, and Ag 79.20%. It can be seen that Comparative Example 2 is affected by the concentration process and the circulating middlings, and the final tailings zinc grade increases by 0.59%, and the zinc metal recovery rate decreases by 1.17%.
[0066] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for flotation separation of zinc minerals from high-grade lead-zinc sulfide ore, characterized in that: include: Step 1, grinding the high-grade lead-zinc sulfide ore until the ore fineness is -200 mesh accounting for 65-72%, and then adjusting the mass concentration of the ore in the slurry to 30-35% to obtain a grinding slurry; Step 2: subjecting the grinding pulp obtained in step 1 to lead and silver preferential flotation to obtain re-selected tailings pulp, and then subjecting the re-selected tailings pulp to three-stage zinc roughing operations under natural pH conditions; in the first stage of zinc roughing operation, 280-320 g / t of zinc activator and 25-30 g / t of zinc collector are added, the flotation time is 3-5 min, and the aeration volume is 2.10-2.60 m 3 / (m 2 ·min), to obtain the first roughing concentrate and the first tailings; the first tailings are subjected to the second stage zinc roughing operation, in which 200-240g / t of zinc activator and 10-20g / t of zinc collector are added, the flotation time is 3-4min, and the aeration volume is 1.10-1.40m 3 / (m 2 ·min), to obtain the second roughing concentrate and the second tailings; the second tailings are subjected to the third stage of zinc roughing operation, in which 200-240g / t of zinc activator and 10-20g / t of zinc collector are added, the flotation time is 3-4min, and the aeration volume is 1.10-1.40m 3 / (m 2 ·min), to obtain the third rougher concentrate and the third tailings; the first rougher concentrate, the second rougher concentrate and the third rougher concentrate are zinc concentrate; Step 3: The third tailings obtained in step 2 are subjected to three-stage zinc scavenging operations under natural pH conditions to obtain three zinc scavenging mid-ranges and final tailings, and the three zinc scavenging mid-ranges are returned to the previous layer in sequence; wherein, 60-100 g / t of zinc activator and 10-15 g / t of zinc collector are added to the first stage of zinc scavenging operation, the flotation time is 3-4 min, and the aeration volume is 1.10-1.40 m 3 / (m 2 ·min); No reagent is added in the second stage of zinc scavenging operation, the flotation time is 3-4min, and the aeration volume is 1.10-1.40m 3 / (m 2 ·min); No reagent is added in the third zinc scavenging operation, the flotation time is 3-4min, and the aeration volume is 1.10-1.40m 3 / (m 2 ·min).
2. The method for flotation separation of zinc minerals from high-grade lead-zinc sulfide ore according to claim 1, characterized in that: The high-grade lead-zinc sulfide ore has a lead grade of 3%-5%, a zinc grade of 22%-27%, and a silver grade of 50-60 g / t.
3. The method for flotation separation of zinc minerals from high-grade lead-zinc sulfide ore according to claim 1, characterized in that: The zinc activator is copper sulfate, and the zinc collector is one or more of P2 and A2.
4. The method for flotation separation of zinc minerals from high-grade lead-zinc sulfide ore according to claim 1, characterized in that: The lead grade of the final tailings is 0.15%-0.18%, the zinc grade is 0.30%-0.40%, and the silver grade is 3-4g / t.
5. The method for flotation separation of zinc minerals from high-grade lead-zinc sulfide ore according to claim 1, characterized in that: When the zinc grade of the final tailings is higher than 0.5%, 20-30 g / t of butyl xanthate and / or ethyl xanthate is added in the third zinc roughing operation in step 2.
6. The method for flotation separation of zinc minerals from high-grade lead-zinc sulfide ore according to claim 1, characterized in that: The lead and silver preferential flotation in step 2 adopts a flotation separation process of one roughing, three fines and three sweeps.
7. The method for flotation separation of zinc minerals from high-grade lead-zinc sulfide ore according to claim 6, characterized in that: In the one rough three fine three sweep flotation separation process, the lead collector used is Pa, the zinc depressants are ZnSO4 and Na2SO3, and the pyrite depressants are EMY101 and Na2SO3.
Citation Information
Patent Citations
Lead-zinc sulfide ore zinc separation reagent composition and zinc-sulfur separation beneficiation method
CN113262881A
Efficient collecting agent for zinc separation of lead-zinc sulfide ore and zinc separation method of efficient collecting agent
CN114042539A
Zinc sulfide ore flotation process
CN116393259A
Beneficiation method for lead zinc ore containing marmatite and pyrrhotite
CN117443585A
Beneficiation method for asynchronous flotation and efficient recovery of high-sulfur copper-lead-zinc-silver-iron polymetallic ore
CN117753550A