Metal surface treatment method for replacing enamel
By using primer and topcoat composed of ceramic resin, spraying and baking to form a metal surface protective layer, the high energy consumption and brittleness problems in traditional enamel technology are solved, and the metal surface treatment with low energy consumption and high pass rate is achieved. It is suitable for Complex structural surface.
Patent Information
- Application Number
- CN202411122087.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The traditional enamel metal surface treatment process has problems such as high firing temperature, large energy consumption, high defect rate, easy to damage coating brittleness, complex composition and easy to react with liquids, making it difficult to adapt to the protection of complex structural parts.
The primer and topcoat composed of ceramic resin, magnesium oxide, alumina powder, boron nitride, etc. are used to form a metal surface protective layer through spraying and baking processes to ensure appropriate viscosity, smooth and durable surface.
It achieves metal surface treatment with low energy consumption, high pass rate and good toughness, is suitable for complex structural surfaces and is easy to produce in large quantities.
Abstract
Description
Technical Field
[0001] The invention relates to the field of metal surface treatment, in particular to a metal surface treatment method replacing enamel. Background Art
[0002] Enamel is used for metal surface treatment because of its wear resistance, heat resistance, corrosion resistance, insulation and beautiful appearance. Its application fields include daily enamel, sanitary enamel, industrial enamel, architectural enamel, medical enamel, artistic enamel and special enamel. However, its high firing temperature, high energy consumption and poor manufacturing environment make it easy to be scrapped due to defects. During use, enameled parts are prone to porcelain peeling and cracking due to the brittleness of the coating when subjected to external forces or rapid heating and cooling temperatures, thus losing their protection of the metal. In addition, its raw material composition is complex and its purity is low. When it is placed in special liquids, the substances in its coating will react with the liquid and dissolve. In addition, the surfaces of some more complex structural parts are difficult to protect with surface enamel because of the changing status quo. Summary of the invention
[0003] The present invention proposes a metal surface treatment method to replace enamel, which solves the defects of the traditional metal surface enamel process, such as high firing temperature, large energy consumption, high defect rate, brittle enamel, easy to be damaged by bumps, complex composition, and easy to react with the liquid.
[0004] The technical solution of the present invention is achieved in this way:
[0005] A metal surface treatment method replacing enamel, including a primer and a topcoat;
[0006] The primer includes the following components in parts by mass:
[0007] Ceramic resin: 40-45 parts;
[0008] Xylene: 10-15 parts;
[0009] Magnesium oxide: 15-20 parts;
[0010] Alumina powder: 6-8 parts;
[0011] Boron nitride: 1-2 parts;
[0012] Fumed silica: 0.5-1 part;
[0013] Dispersant: 18-12 parts;
[0014] Wollastonite: 3-5 parts;
[0015] The topcoat comprises the following components in parts by mass:
[0016] Ceramic resin: 95 parts;
[0017] Wetting agent: 0.5 parts;
[0018] Leveling agent: 0.5 parts;
[0019] Anhydrous ethanol: 8-12 parts;
[0020] The processing method specifically includes the following steps:
[0021] (1) Primer treatment
[0022] Stir the primer thoroughly to prevent precipitation, then check its viscosity to ensure that it is between 12-18 seconds. If the viscosity is too low, open the container to allow the solvent to evaporate and thicken. If the viscosity is too high, add PMA to dilute it. Use a 200-300 mesh filter to filter the paint with appropriate viscosity for later use.
[0023] (2) Metal surface treatment
[0024] Sandblast the metal surface with a sand particle size between 80-120 mesh. After sandblasting, blow dust off the metal surface to ensure that there is no floating dust. Pay attention to protection and do not touch it with your fingers. No dust should fall on it.
[0025] (3) Spraying primer layer
[0026] The operation is carried out in a clean workshop of 100,000 grade, with a temperature of 20-26 degrees and a humidity not exceeding 80%. A tank-type spray gun or an automatic spray gun is used, and the primer is loaded. The spray gun caliber is 1.3-1.8 mm, the air pressure is 0.4-0.6 MPa, and the muzzle is 25 cm away from the metal surface. The metal surface is sprayed to form a primer layer. The thickness of the primer layer is 70-300 microns. After spraying, the primer layer should be observed immediately. If the surface is moist and as bright as a mirror, it is qualified. Otherwise, it should be cleaned with PMA, the spraying technique should be readjusted, and spraying should be carried out again. After spraying, let it stand for 5-10 minutes to dry on the surface;
[0027] (4) Primer layer curing
[0028] Put the metal that has been dried on the surface into the oven for curing. The oven is heated from room temperature to 230 degrees within 35-45 minutes, and then kept warm for 15-20 minutes. After that, take it out and cool it down to room temperature. After it cools down to room temperature, check the appearance of the base coating to ensure that there are no stains on the surface. Then polish it with 1000-1500 mesh sponge sandpaper, and then blow dust with an air gun. The whole process must not be touched directly with fingers, and the operator must wear clean gloves that do not fall off.
[0029] (5) Spraying topcoat
[0030] Use a tank spray gun or an automatic spray gun, load the topcoat, the spray gun caliber is 0.8-1.4 mm, the air pressure is 0.4-0.6 MPa, spray the cured metal surface to form a topcoat layer, the thickness of the topcoat layer is 5-8 microns;
[0031] (6) Topcoat curing
[0032] After spraying, put it directly into a 200-degree oven for baking for 10-15 minutes, take it out and let it cool down to room temperature;
[0033] (7) Inspection
[0034] Conduct an appearance inspection. There should be no bubbles or impurities on the surface, and no raised spots when touched.
[0035] Beneficial effects of the present invention: Compared with traditional enamel, the scheme of the present invention has low energy consumption, high pass rate, good toughness, high purity, can process the surface of complex structures, and is easy to mass produce. DETAILED DESCRIPTION
[0036] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0037] A metal surface treatment method replacing enamel, including a primer and a topcoat;
[0038] The primer includes the following components in parts by mass:
[0039] Ceramic resin: 40-45 parts;
[0040] Xylene: 10-15 parts;
[0041] Magnesium oxide: 15-20 parts;
[0042] Alumina powder: 6-8 parts;
[0043] Boron nitride: 1-2 parts;
[0044] Fumed silica: 0.5-1 part;
[0045] Dispersant: 18-12 parts;
[0046] Wollastonite: 3-5 parts;
[0047] The topcoat includes the following components in parts by mass:
[0048] Ceramic resin: 95 parts;
[0049] Wetting agent: 0.5 parts;
[0050] Leveling agent: 0.5 parts;
[0051] Anhydrous ethanol: 8-12 parts;
[0052] The processing method specifically includes the following steps:
[0053] (1) Primer treatment
[0054] Stir the primer thoroughly to prevent precipitation, then check its viscosity to ensure that it is between 12-18 seconds. If the viscosity is too low, open the container to allow the solvent to evaporate and thicken. If the viscosity is too high, add PMA to dilute it. Use a 200-300 mesh filter to filter the paint with appropriate viscosity for later use.
[0055] (2) Metal surface treatment
[0056] Sandblast the metal surface with a sand particle size between 80-120 mesh. After sandblasting, blow dust off the metal surface to ensure that there is no floating dust. Pay attention to protection and do not touch it with your fingers. No dust should fall on it.
[0057] (3) Spraying primer layer
[0058] The operation is carried out in a clean workshop of 100,000 grade, with a temperature of 20-26 degrees and a humidity not exceeding 80%. A tank-type spray gun or an automatic spray gun is used, and the primer is loaded. The spray gun caliber is 1.3-1.8 mm, the air pressure is 0.4-0.6 MPa, and the muzzle is 25 cm away from the metal surface. The metal surface is sprayed to form a primer layer. The thickness of the primer layer is 70-300 microns. After spraying, the primer layer should be observed immediately. If the surface is moist and as bright as a mirror, it is qualified. Otherwise, it should be cleaned with PMA, the spraying technique should be readjusted, and spraying should be carried out again. After spraying, let it stand for 5-10 minutes to dry on the surface;
[0059] (4) Primer layer curing
[0060] Put the metal that has been dried on the surface into the oven for curing. The oven is heated from room temperature to 230 degrees within 35-45 minutes, and then kept warm for 15-20 minutes. After that, take it out and cool it down to room temperature. After it cools down to room temperature, check the appearance of the base coating to ensure that there are no stains on the surface. Then polish it with 1000-1500 mesh sponge sandpaper, and then blow dust with an air gun. The whole process must not be touched directly with fingers, and the operator must wear clean gloves that do not fall off.
[0061] (5) Spraying topcoat
[0062] Use a tank spray gun or an automatic spray gun, load the topcoat, the spray gun caliber is 0.8-1.4 mm, the air pressure is 0.4-0.6 MPa, spray the cured metal surface to form a topcoat layer, the thickness of the topcoat layer is 5-8 microns;
[0063] (6) Topcoat curing
[0064] After spraying, put it directly into a 200-degree oven for baking for 10-15 minutes, take it out and let it cool down to room temperature;
[0065] (7) Inspection
[0066] Conduct an appearance inspection. There should be no bubbles or impurities on the surface, and no raised spots when touched.
[0067] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A metal surface treatment method to replace enamel, Features: Includes primer and topcoat; The primer includes the following components in parts by mass: Ceramic resin: 40-45 parts; Xylene: 10-15 parts; Magnesium oxide: 15-20 parts; Alumina powder: 6-8 parts; Boron nitride: 1-2 parts; Fumed silica: 0.5-1 part; Dispersant: 18-12 parts; Wollastonite: 3-5 parts; The topcoat comprises the following components in parts by mass: Ceramic resin: 95 parts; Wetting agent: 0.5 parts; Leveling agent: 0.5 parts; Anhydrous ethanol: 8-12 parts; The processing method specifically includes the following steps: (1) Primer treatment Stir the primer thoroughly to prevent precipitation, then check its viscosity to ensure that it is between 12-18 seconds. Use a 200-300 mesh filter to filter the paint with appropriate viscosity for later use; (2) Metal surface treatment Sandblast the metal surface. After sandblasting, blow the dust off the metal surface to ensure that there is no floating dust. (3) Spraying primer layer The operation is carried out in a clean workshop of 100,000 grade, with a temperature of 20-26 degrees and a humidity not exceeding 80%. Use a tank spray gun or an automatic spray gun, load the primer, and spray the metal surface to form a primer layer. The thickness of the primer layer is 70-300 microns. After spraying, the primer layer should be observed immediately. If the surface is moist and as bright as a mirror, it is qualified. Otherwise, it should be cleaned with PMA, the spraying technique should be readjusted, and spraying should be carried out again. After spraying, let it stand for 5-10 minutes to dry on the surface; (4) Primer curing Put the surface-dried metal into the oven for curing. The oven is heated from room temperature to 230 degrees in 35-45 minutes, and then kept warm for 15-20 minutes. After that, it is taken out and cooled to room temperature. After cooling to room temperature, the base coating is inspected for appearance to ensure that there are no stains on the surface. Then, it is polished with 1000-1500 mesh sponge sandpaper, and then dusted with an air gun. (5) Spraying topcoat Use a tank spray gun or an automatic spray gun to load the topcoat and spray the cured metal surface to form a topcoat layer with a thickness of 5-8 microns; (6) Curing of topcoat layer After spraying the topcoat layer, put it directly into a 200-degree oven for baking for 10-15 minutes, take it out and let it cool to room temperature.
2. The metal surface treatment method as claimed in claim 1, Features: The step (7) includes inspection: performing an appearance inspection to ensure that there are no bubbles or impurities on the surface and no convex spots when touched.
3. The metal surface treatment method as claimed in claim 1, Features: In step (1), if the viscosity is too low, the container is opened to allow the solvent to evaporate and thicken. If the viscosity is too high, PMA is added to dilute it.
4. The metal surface treatment method as claimed in claim 1, Features: In step (2), the particle size of the sand blasting is between 80-120 meshes. During the dust blowing process, the metal surface cannot be touched with fingers and dust must not fall on it.
5. The metal surface treatment method as claimed in claim 1, Features: In step (3), the caliber of the spray gun of the upper tank spray gun or the automatic spray gun is 1.3-1.8 mm, the air pressure used is 0.4-0.6 MPa, and the distance between the muzzle and the metal surface is 25 cm.
6. The metal surface treatment method as claimed in claim 1, Features: In step (4), during the entire process of blowing dust with the air gun, the operator must not touch the dust directly with fingers, and must wear clean gloves that do not fall off.
7. The metal surface treatment method as claimed in claim 1, Features: In step (5), the caliber of the spray gun of the upper tank type spray gun or the automatic spray gun is 0.8-1.4 mm, and the air pressure used is 0.4-0.6 MPa.