Production process for Hazelite continuous casting and rolling thin production
By adjusting the three-pass hot rolling process parameters of the Hazlett continuous casting and rolling production line and optimizing the structure of the three-pass hot rolling mill, stable production of 1.6mm thick aluminum alloy plates was achieved, solving the problems of production efficiency and cost in the existing technology, improving production efficiency and reducing the number of passes in the cold rolling process.
Patent Information
- Application Number
- CN202411032075.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-26
AI Technical Summary
The existing Hazlett production line is unable to stably produce 1.6mm thick aluminum alloy sheets, which requires additional processing passes in the cold rolling process, reducing production efficiency and increasing costs.
By adjusting the three-pass hot rolling process parameters of the Hazlete continuous casting and rolling production line, including the reduction, unit tension, bending roll angle and emulsion temperature settings, the work roll and bending roll structure of the three-pass hot rolling mill was optimized, enabling stable production of 1.6mm thick products.
While maintaining the original production efficiency, the number of cold rolling processes was reduced, which improved production efficiency and reduced production costs.
Smart Images

Figure CN119016498A_ABST
Abstract
Description
Technical Field
[0001] This article belongs to the technical field of Hazlet continuous rolling production, and specifically relates to a production process for producing 1.6mm thick products through Hazlet continuous casting and rolling. Background Art
[0002] With the development of my country's construction, packaging and home appliance industries, the demand for aluminum foil is also increasing year by year. At present, the production methods of aluminum sheet and strip in the world mainly include iron mold casting-hot rolling, semi-continuous casting-hot rolling, continuous casting and rolling, and continuous casting and rolling. The iron mold casting-hot rolling method has simple equipment, low investment, flexible production, and good deep drawing performance of the product, but the yield is low and the product surface quality is poor.
[0003] The Hazlet production process is currently the most advanced aluminum alloy casting process in the world. Compared with the traditional ingot hot rolling process, the Hazlet continuous casting and rolling process has a series of advantages such as low investment, energy saving, low production cost, and good product performance. It is widely used in the production of various metal (aluminum, copper, zinc, etc.) strips. After the casting machine, the ingot is hot rolled online at the billet temperature. The casting output is high, averaging 45 tons / hour / mm (1950mm casting width). That is to say, the ingot will enter the rolling mill at a speed of nearly 7.6 meters per minute. The pass reduction is 60% or more, and excellent hot rolled metal structure can be obtained.
[0004] At present, most of the existing Hazlet production lines produce products with a thickness of 3.5mm and above, and a few companies can produce products with a thickness of 2.3mm. Since most Hazlet products are semi-finished products, they will still undergo cold rolling, foil rolling and other deep processing rolling. Therefore, if thinner plates are needed, it is necessary to directly ask the Hazlet equipment manufacturer to design the production equipment according to the needs.
[0005] There is still much room for reducing the thickness of the products currently produced. The production process can be improved and optimized based on the existing 2.3mm thick product production line to reduce the thickness, which can further reduce the number of cold foil rolling passes and improve production efficiency. Summary of the invention
[0006] In order to solve the above problems, this paper proposes a production process for thinning Hazelet continuous casting and rolling. The Hazelet continuous casting and rolling thinning process is three-pass continuous hot rolling, and the three-pass continuous hot rolling is rolled by a three-pass hot rolling mill. The three-pass hot rolling mill is a 2.3 mm thick plate rolling mill. The three-pass hot rolling mill includes the first hot rolling, the second hot rolling and the third hot rolling. The three-pass hot rolling mill is equipped with unit tension adjustment, bending roll angle adjustment and emulsion temperature adjustment. By modifying the existing 2.3 mm Hazelet production process parameter setting, after multiple attempts on site, the Hazelet production line can stably produce 1.6 mm thick products. While maintaining the original production efficiency of Hazelet, one processing pass is reduced for the rolling of the cold rolling process, which greatly improves the production efficiency and reduces the production cost. The specific production process of the 1.6 mm thin plate of the three-pass hot rolling mill is as follows;
[0007] a. The thickness reduction of the first hot rolling is set to 19mm-7.2±0.3mm, the unit tension is set to 1.0±0.3 (Kg / mm2), the bending roll angle is set to (-30,30)%, and the emulsion temperature is set to 45-50℃;
[0008] b. The thickness reduction of the second hot rolling is set to 7.2±0.3mm-3.2±0.3mm, the unit tension is set to 1.3±0.3 (Kg / mm2), the bending roll angle is set to (-30,30)%, and the emulsion temperature is set to 47-50℃;
[0009] c. The thickness reduction of the first hot rolling is set to 3.2±0.3mm-1.6mm, the unit tension is set to 2.0±0.4 (Kg / mm2), the bending roll angle is set to (-30,30)%, and the emulsion temperature is set to 50-53℃.
[0010] The three-pass hot rolling mill is an integrated plate thinning hot rolling device, and working rolls, bending rolls and emulsion pipes are arranged inside the three-pass hot rolling mill. The emulsion pipes are arranged above the working rolls and the bending rolls. The reduction amounts of the first hot rolling, the second hot rolling and the third hot rolling are increased step by step in sequence, the unit tensions of the first hot rolling, the second hot rolling and the third hot rolling are increased step by step in sequence, and the emulsion temperatures of the first hot rolling, the second hot rolling and the third hot rolling are increased step by step in sequence.
[0011] The first hot rolling: Compared with the rolling pass of 2.3mm products, the first pass reduction of 1.6mm products is increased by 6.8%, and is set to 19-7.2±0.3mm, in order to reduce the final pass reduction for thinning of finished products; the unit tension is set to 1.0±0.3 (Kg / mm2), and the bending roll is set to (-30,30)%, which can keep the plate surface taut, avoid scratches on the plate surface, and ensure that the plate shape is convex; the emulsion temperature is set to 45-50℃, mainly to reduce the temperature of the working roll surface during the hot rolling process, which can avoid the problem of aluminum sticking, and at the same time play the role of lubrication and cleaning aluminum powder when the working roll surface contacts the plate surface;
[0012] The second hot rolling: compared with the rolling pass of 2.3mm products, the second pass reduction of 1.6mm products is increased by 5.0%, set to 7.2±0.3mm-3.2±0.3mm, and continue to reduce the final pass reduction for thinning the finished product; the unit tension is set to 1.3±0.3 (Kg / mm2), the bending roll is set to (-30,30)%, increase the tension, continue to keep the plate surface taut, avoid scratches on the plate surface, and ensure that the plate shape is convex; the emulsion temperature is set to 47-50℃, which can play a role in lubrication and cleaning aluminum powder when the working roll surface contacts the plate surface;
[0013] The third hot rolling pass: compared with the rolling pass of 2.3mm products, the reduction of the third pass of 1.6mm products is increased by 4.8%, set to 3.2±0.3mm-1.6mm, and the reduction of the final pass is relatively small, which can ensure that the plate shape is parabolic to a certain extent; the unit tension is set to 2.0±0.4 (Kg / mm2), the bending roll is set to (-30,30)%, and the plate surface is kept taut to avoid scratches on the plate surface, and ensure that the final plate shape is a convex plate; the emulsion temperature of the final pass of this process is set to 47-50℃, which is higher than the emulsion temperature of the first two passes. It is mainly to ensure lubrication and cleaning of aluminum powder while avoiding the problem of emulsion residue and corrosion on the plate surface caused by too low plate temperature.
[0014] Beneficial effects:
[0015] By modifying the existing 2.3mm Hazlet production process parameter settings and after multiple on-site adjustments, the Hazlet production line can stably produce 1.6mm thick products. While maintaining the original production efficiency of Hazlet, one processing pass is reduced for the cold rolling process, which greatly improves production efficiency and reduces production costs.
[0016] The first hot rolling: Compared with the rolling pass of 2.3mm products, the first pass reduction of 1.6mm products is increased by 6.8%, and is set at 19-7.2±0.3mm to reduce the final pass reduction for thinning of finished products; the unit tension is 1.0±0.3 (Kg / mm2), and the bending roll is (-30,30)%, which can keep the plate surface taut, avoid scratches on the plate surface, and ensure that the plate shape is convex; the emulsion temperature is set at 45-50℃, mainly to reduce the temperature of the working roll surface during the hot rolling process, which can avoid the problem of aluminum sticking, and at the same time play the role of lubrication and cleaning aluminum powder when the working roll surface contacts the plate surface;
[0017] The second hot rolling: compared with the rolling pass of 2.3mm products, the second pass reduction of 1.6mm products increased by 5.0%, set to 7.2±0.3mm-3.2±0.3mm, and continued to reduce the final pass reduction for thinning of finished products; unit tension 1.3±0.3 (Kg / mm2), bending roll (-30,30)%, increase tension, continue to keep the plate surface taut, avoid scratches on the plate surface, and ensure that the plate shape is convex; the emulsion temperature is set to 47-50℃, which can play a role in lubrication and cleaning aluminum powder when the working roll surface contacts the plate surface;
[0018] The third hot rolling pass: compared with the rolling pass of 2.3mm products, the third pass reduction of 1.6mm products is increased by 4.8%, set to 3.2±0.3mm-1.6mm, and the final pass reduction is relatively small, which can ensure that the plate shape is parabolic to a certain extent; the unit tension is 2.0±0.4 (Kg / mm2), the bending roll is (-30,30)%, and the plate surface is kept taut to avoid scratches on the plate surface, and the final plate shape is a convex plate; the emulsion temperature of the final pass of this process is set to 47-50℃, which is higher than the emulsion temperature of the first two passes. It is mainly to ensure lubrication and cleaning of aluminum powder while avoiding the problem of emulsion residue and corrosion on the plate surface caused by too low plate temperature. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The present invention is a process flow chart of the production process of Hazelt continuous casting and rolling thin production. DETAILED DESCRIPTION
[0020] In order to deepen the understanding of the present invention, the present invention will be further described in detail below with reference to embodiments and drawings. The embodiments are only used to explain the present invention and do not constitute a limitation on the protection scope of the present invention.
[0021] like Figure 1 As shown;
[0022] A production process for thinning Hazelet continuous casting and rolling. The Hazelet continuous casting and rolling thinning process is three-pass continuous hot rolling. The three-pass continuous hot rolling is performed by a three-pass hot rolling mill. The three-pass hot rolling mill is a 2.3 mm thick plate rolling mill. The three-pass hot rolling mill includes a first hot rolling, a second hot rolling and a third hot rolling. The three-pass hot rolling mill is provided with a unit tension adjustment, a bending roll angle adjustment and an emulsion temperature adjustment. The three-pass hot rolling mill is an integrated plate thinning hot rolling device. The three-pass hot rolling mill is provided with a working roll, a bending roll and an emulsion pipeline. The emulsion pipeline is arranged above the working roll and the bending roll. The reduction amount of the first hot rolling, the second hot rolling and the third hot rolling is increased in sequence in a step-by-step variable manner. The unit tension of the first hot rolling, the second hot rolling and the third hot rolling is increased in sequence in a step-by-step variable manner. The emulsion temperature of the first hot rolling, the second hot rolling and the third hot rolling is increased in sequence in a step-by-step variable manner.
[0023] The first hot rolling: Compared with the rolling pass of 2.3mm products, the first pass reduction of 1.6mm products is increased by 6.8%, and is set at 19-7.2±0.3mm to reduce the final pass reduction for thinning of finished products; the unit tension is 1.0±0.3 (Kg / mm2), and the bending roll is (-30,30)%, which can keep the plate surface taut, avoid scratches on the plate surface, and ensure that the plate shape is convex; the emulsion temperature is set at 45-50℃, mainly to reduce the temperature of the working roll surface during the hot rolling process, which can avoid the problem of aluminum sticking, and at the same time play the role of lubrication and cleaning aluminum powder when the working roll surface contacts the plate surface;
[0024] The second hot rolling: compared with the rolling pass of 2.3mm products, the second pass reduction of 1.6mm products increased by 5.0%, set to 7.2±0.3mm-3.2±0.3mm, and continued to reduce the final pass reduction for thinning of finished products; unit tension 1.3±0.3 (Kg / mm2), bending roll (-30,30)%, increase tension, continue to keep the plate surface taut, avoid scratches on the plate surface, and ensure that the plate shape is convex; the emulsion temperature is set to 47-50℃, which can play a role in lubrication and cleaning aluminum powder when the working roll surface contacts the plate surface;
[0025] The third hot rolling pass: compared with the rolling pass of 2.3mm products, the third pass reduction of 1.6mm products is increased by 4.8%, set to 3.2±0.3mm-1.6mm, and the final pass reduction is relatively small, which can ensure that the plate shape is parabolic to a certain extent; the unit tension is 2.0±0.4 (Kg / mm2), the bending roll is (-30,30)%, and the plate surface is kept taut to avoid scratches on the plate surface, and the final plate shape is a convex plate; the emulsion temperature of the final pass of this process is set to 47-50℃, which is higher than the emulsion temperature of the first two passes. It is mainly to ensure lubrication and cleaning of aluminum powder while avoiding the problem of emulsion residue and corrosion on the plate surface caused by too low plate temperature.
[0026] Implementation examples;
[0027] a. The thickness reduction of the first hot rolling is set to 19mm-7.2±0.3mm, the unit tension is set to 1.0±0.3 (Kg / mm2), the bending roll angle is set to (-30,30)%, and the emulsion temperature is set to 45-50℃;
[0028] b. The thickness reduction of the second hot rolling is set to 7.2±0.3mm-3.2±0.3mm, the unit tension is set to 1.3±0.3 (Kg / mm2), the bending roll angle is set to (-30,30)%, and the emulsion temperature is set to 47-50℃;
[0029] c. The thickness reduction of the first hot rolling is set to 3.2±0.3mm-1.6mm, the unit tension is set to 2.0±0.4 (Kg / mm2), the bending roll angle is set to (-30,30)%, and the emulsion temperature is set to 50-53℃.
[0030] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A production process for thinning by continuous casting and rolling of Hazelett, wherein the process of continuous casting and rolling of Hazelett is three-pass continuous hot rolling, and the three-pass continuous hot rolling is carried out by a three-pass hot rolling mill, and the three-pass hot rolling mill is a 2.3 mm thick plate rolling mill, characterized in that: The three-pass hot rolling mill includes a first hot rolling, a second hot rolling and a third hot rolling. The three-pass hot rolling mill is provided with unit tension adjustment, bending roll angle adjustment and emulsion temperature adjustment. The specific production process of the 1.6 mm thin plate of the three-pass hot rolling mill is as follows; a. The thickness reduction of the first hot rolling is set to 19mm-7.2±0.3mm, the unit tension is set to 1.0±0.3 (Kg / mm2), the bending roll angle is set to (-30,30)%, and the emulsion temperature is set to 45-50℃; b. The thickness reduction of the second hot rolling is set to 7.2±0.3mm-3.2±0.3mm, the unit tension is set to 1.3±0.3 (Kg / mm2), the bending roll angle is set to (-30,30)%, and the emulsion temperature is set to 47-50℃; c. The thickness reduction of the first hot rolling is set to 3.2±0.3mm-1.6mm, the unit tension is set to 2.0±0.4 (Kg / mm2), the bending roll angle is set to (-30,30)%, and the emulsion temperature is set to 50-53℃.
2. The production process of Hazeltite continuous casting and rolling thin production according to claim 1, characterized in that: The three-continuous hot rolling mill is an integrated plate thinning hot rolling device, and working rolls, bending rolls and emulsion pipelines are arranged inside the three-continuous hot rolling mill, and the emulsion pipelines are all arranged above the working rolls and the bending rolls.
3. The production process of Hazeltite continuous casting and rolling thin production according to claim 1, characterized in that: The reduction amounts of the first hot rolling, the second hot rolling and the third hot rolling are increased in sequence in a step-by-step variable manner.
4. The production process of Hazeltite continuous casting and rolling thin production according to claim 1, characterized in that: The unit tensions of the first hot rolling pass, the second hot rolling pass and the third hot rolling pass are increased step by step in sequence.
5. The production process of Hazeltite continuous casting and rolling thin production according to claim 1, characterized in that: The emulsion temperatures of the first hot rolling pass, the second hot rolling pass and the third hot rolling pass are increased in sequence in a step-by-step manner.
Citation Information
Patent Citations
Continuous casting and rolling production method for aluminium and aluminium alloy by using double racks
CN102489509A
Method for producing high-strength thin strip steel in short process
CN103658178A
Method for improving bottom plate type edge waves of Hazitride air conditioner foil finished product
CN116000086A
Technological method for producing deep-drawing aluminum plate strip for kitchen ware from secondary aluminum
CN116219210A
Method and installation for the continuous production of hot-rolled, thin flat products
US6527882B1