Production method of vanadium-containing hot-rolled H-shaped steel with low compression ratio
By adopting low compression ratio vanadium-containing technology in hot-rolled H-shaped steel production, and controlling the cooling water flow rate and casting billet loading system, the problem of uneven steel performance under extremely low compression ratio is solved, and low temperature, high strength, and high Tough H-shaped steel meets the needs of high-rise buildings and large-span bridges.
Patent Information
- Application Number
- CN202411089226.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-26
AI Technical Summary
The existing technology is difficult to effectively produce low-temperature high-performance hot-rolled H-shaped steel with extremely low compression ratios, and cannot meet the application needs of high-rise buildings and large-span bridges.
The production method of low-compression ratio vanadium-containing hot-rolled H-shaped steel is adopted. The internal and external arc cooling water flow of the crystallizer is controlled through the full protection continuous casting process of the special-form blank, which promotes the growth of fine isometric grains, and combines the unique cast blank charging system and heating furnace. Time regulation to achieve the improvement of the microstructure uniformity and macromechanical performance of steel.
Low temperature, high strength, high toughness, and high toughness hot-rolled H-shaped steel were prepared under extremely low compression ratio to meet the application requirements of high-rise buildings and large-span bridges, and improve the stability and application prospects of product performance.
Smart Images

Figure BDA0004986034190000131
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hot-rolled H-shaped steel production, and in particular to a production method of low-reduction-ratio vanadium-containing hot-rolled H-shaped steel. Background Art
[0002] Hot-rolled H-beams are mainly used in the construction and manufacturing industries. The construction industry involves industrial and civil buildings, large bridges, high-speed projects, engineering support, etc. The manufacturing industry involves steel structure processing, industrial and civil machinery, shipbuilding, etc. In terms of consumption ratio, the current consumption demand for hot-rolled H-beams in the manufacturing industry accounts for about 39.72%, the construction industry accounts for about 47.11%, and other consumer industries account for about 13.17%, and the market demand is huge.
[0003] H-beam, also known as wide flange H-beam, is a type of steel with an H-shaped cross-section, named for its cross-sectional shape. The two flanges of the H-beam are parallel and perpendicular to the web. This design makes the H-beam have high stability and load-bearing capacity in building structures. The flange width of low compression ratio H-beam (compression ratio is about 3:1) is relatively wide and the web is relatively thick, which makes it have higher load-bearing capacity and better stability when under pressure. Therefore, low compression ratio H-beam is suitable for structures that need to bear large loads or require higher stability.
[0004] Low compression ratio means that during the rolling process, the thickness of the material is reduced at a smaller ratio, which may lead to uneven material properties. Therefore, the lower the compression ratio during the rolling process, the more difficult it is to obtain low-temperature and high-performance H-beams. The current process is only suitable for the preparation of H-beams with a compression ratio of about 3, and is not applicable to special hot-rolled H-beams with extremely low compression ratios. Therefore, it is necessary to develop a hot-rolled H-beam with extremely low compression ratio and low temperature and high performance to meet the application requirements of high-rise buildings or large-span bridges. Summary of the invention
[0005] In view of the above problems, the present invention provides a method for producing low reduction ratio vanadium-containing hot-rolled H-beam.
[0006] To solve the above technical problems, the technical solution provided by the embodiment of the present invention is:
[0007] A production method of low-compression ratio vanadium-containing hot-rolled H-beam, wherein the compression ratio of the H-beam is 2.1-2.2, and the average longitudinal impact energy at 0°C is ≥100J. The production method comprises converter or electric furnace smelting, LF refining, full-protection continuous casting of profiled blanks, heating, rolling and cooling processes, wherein:
[0008] In the full-protection continuous casting process of the profiled blank, the flow ratio of the cooling water of the inner and outer arcs of the crystallizer to the left and right arcs is 1:1.5-1.8, the specific water volume of the secondary cooling water is 0.6L / kg-0.9kg / L, the secondary cooling is divided into 5 cooling zones, and the ratio of the total water volume of each zone is zone 1: zone 2: zone 3: zone 4: zone 5 = 1: 0.94-0.97: 0.6-0.75: 0.13-0.15: 0.1-0.11, wherein the water volume of the inner arc in zone 2: the water volume of the outer arc = 0.767-0.774: 1, the water volume of the inner arc in zone 3: the water volume of the outer arc = 0.5-0.56: 1, the water volume of the inner arc in zone 4: the water volume of the outer arc = 0.32-0.34: 1, and the water volume of the inner arc in zone 5: the water volume of the outer arc = 0.24-0.26: 1;
[0009] In the heating process: the continuous casting billets are loaded onto the walking beam in a manner of 2 empty spaces every 10 consecutive billets, put into the furnace for heating and insulation, and discharged after the insulation is completed; wherein, when discharging, the steel-discharging rhythm of the empty spaces at the outlet is controlled according to the total insulation time of the continuous casting billets in the heating furnace being 150min to 180min: if the continuous casting billets in the heating furnace do not reach the requirement of the total insulation time after the rolling of the previous continuous casting billet is completed, the steel-discharging rhythm of the empty spaces at the outlet is preset; if the continuous casting billets in the heating furnace reach or exceed the requirement of the total insulation time after the rolling of the previous continuous casting billet is completed, the steel-discharging rhythm of the empty spaces at the outlet is preset.
[0010] With respect to the prior art, the present invention provides a method for producing hot-rolled H-beam with low compression ratio and containing vanadium. By controlling the flow rate ratio of the cooling water of the inner and outer arcs and the left and right arcs of the crystallizer in the continuous casting process of the profiled blank, and the flow rate of the inner and outer arcs of the secondary cooling zone, the cooling speed of the profiled blank is precisely controlled, the growth of columnar grains is suppressed, and the growth of fine equiaxed grains is promoted. A fine equiaxed crystal zone with a thickness of 20 mm to 25 mm is formed on the surface of the profiled blank, thereby improving the microstructure uniformity and macroscopic mechanical properties of the steel; at the same time, a unique billet charging system is adopted, which can effectively control the steel-out rhythm according to the rolling time and the time in the furnace, thereby ensuring the consistency of the continuous casting billet time in the furnace, and avoiding the occurrence of the problem of unstable steel performance caused by uneven heating of the continuous casting billet. The present invention realizes the preparation of hot-rolled H-beam with low temperature, high strength and high toughness at an extremely low compression ratio by controlling the cooling process of the continuous casting process of the profiled blank and the charging and tapping time of the heating furnace, which meets the application requirements in the field of high-rise buildings or large-span bridges and has broad application prospects.
[0011] In the actual production process, the normal production rhythm is that after the rolling process completes the rolling of a continuous casting billet, a continuous casting billet comes out of the heating furnace. However, the time of the rolling process cannot usually be accurately controlled, and the rolling time of each casting billet will have a certain deviation, or it will be shorter than the standard time or longer than the standard time. After a large number of continuous casting billets are rolled, the time for the front continuous casting billet in the heating furnace will be obviously insufficient or significantly extended. If the heating time is insufficient, the internal structure and performance of the billet will be uneven. If the heating time is too long, it will cause oxidation and decarburization on the surface of the billet, affecting product performance. The present invention creatively proposes to adopt a loading system of adding two empty spaces for every 10 continuous casting billets loaded on the walking beam, and adjust the insulation time of the continuous casting billet in the heating furnace by the steel-out time of the empty spaces. When the rolling process is too long, resulting in the continuous casting billet staying in the heating furnace for longer than the standard time, when the vacant space is transported to the furnace outlet, the vacant space is quickly transported out using the normal steel loading time. If the rolling time is short, resulting in the continuous casting billet staying in the heating furnace for insufficient time, the vacant space is transported out according to the normal steel tapping time, thereby extending the time the continuous casting billet stays in the heating furnace. Through the above simple charging system and the regulation of the vacant space steel tapping speed, the time the continuous casting billet stays in the heating furnace can be regulated in a timely manner, thereby ensuring the uniformity of the time the continuous casting billet stays in the furnace and improving the stability of product performance.
[0012] Furthermore, the raw material of the hot-rolled H-beam in the present invention is a special-shaped continuous casting billet, and the cross-sectional dimensions of the continuous casting billet are 555mm×440mm×105mm×78mm (web height×flange width×web thickness×flange thickness).
[0013] Specifically, for the above-mentioned specifications of the continuous casting billet walking beam, the step distance is 900mm, that is, a large step distance setting is adopted, one billet is placed within the step distance, and the position of the empty position is set according to the normal step distance, but the continuous casting billet is not installed.
[0014] Furthermore, in order to ensure the stability of product performance, after a total of 30 special-shaped continuous casting billets are loaded, 40 ordinary product billets (that is, products that can meet the performance requirements without special control of each process) are loaded continuously to ensure that the time each billet spends in the heating furnace is almost consistent.
[0015] Furthermore, in the heating process, the heating furnace is divided into heating stage one, heating stage two, heating stage three and a soaking stage, wherein the temperature of heating stage one is 910°C to 1100°C, the temperature of heating stage two is 1100°C to 1150°C, the temperature of heating stage three is 1240°C to 1260°C, and the temperature of the soaking stage is 1230°C to 1250°C.
[0016] Furthermore, in the heating process, the holding time of the continuous casting billet in the first heating stage is ≥35 min, the holding time in the second heating stage is ≥35 min, the holding time in the third heating stage is 30 min to 45 min, and the holding time in the equalizing stage is 30 min to 45 min.
[0017] The optimal heating temperature and heating time can improve the uniformity of the structure, ensure sufficient transformation of the structure, and also help reduce the residual stress of the ingot.
[0018] Furthermore, the LF refining process comprises the following steps: adding molten steel into the LF refining furnace, blowing argon, adding refining slag, lime, calcium carbide and silicon-based deoxidizer in sequence, the slagging time is less than 3 minutes, and refining is 8 minutes to 15 minutes.
[0019] Furthermore, in the LF refining process, the amount of the refined slag added is 1kg / t to 3kg / t, the amount of the lime added is 5kg / t to 10kg / t, the amount of the calcium carbide added is 3kg / t to 5kg / t, and the amount of the silicon-based deoxidizer added is 1kg / t to 3kg / t.
[0020] Furthermore, in the LF refining process, the temperature of the molten steel entering the furnace is 1560°C to 1580°C.
[0021] The optimal refining process can improve the shape, size and quantity of inclusions in the molten steel, increase the purity of the molten steel, and further improve the strength and low-temperature toughness of the steel.
[0022] Furthermore, in the full-protection continuous casting process of the special-shaped blank, when the molten steel flows from the large ladle into the tundish, a long shroud is used for protection casting, a covering agent is added to the surface of the tundish, the tundish cover is protected by argon sealing at three points on both sides and in the middle, the crystallizer is protected by an argon-sealed long shroud, and the gap between the tundish slide plates is protected by an argon-sealed tube.
[0023] Through the above-mentioned full-protection pouring process, the total oxygen content in the molten steel can be controlled below 50ppm, and the nitrogen content can be controlled below 80ppm, ensuring the stability of product performance.
[0024] Furthermore, after the billet is taken out of the heating furnace, high-pressure water dephosphorization is performed, and the dephosphorization pressure is 20MPa to 26MPa.
[0025] Furthermore, in the rolling process, the rough rolling adopts 7 rolling passes, the start rolling temperature is 1050℃~1150℃, the finish rolling adopts 5 rolling passes, the roll speed is 1.3m / s~1.5m / s, and the final rolling temperature is 850℃~900℃.
[0026] During the rolling process of H-beam with low compression ratio, the thickness reduction ratio of the material is small, which can easily lead to uneven material properties after rolling. Therefore, it is necessary to accurately control the deformation distribution, temperature control and reduction rate during the rolling process to ensure the uniformity and consistency of material properties. The above process is conducive to improving the uniformity and consistency of material properties after rolling.
[0027] It should be noted that after the rough rolling is completed, the rollers are left to wait for 0 to 60 seconds to ensure that the temperature of the billet entering the finishing mill is less than 980°C.
[0028] As a specific implementation of the present invention, a two-roller reversible blanking mill is used for rough rolling, and a three-stand universal reversible finishing mill is used for finishing rolling.
[0029] Furthermore, after the rolling is completed, the finished rolled piece is water-cooled and then naturally cooled on a cooling bed, and then sent to a straightening machine for straightening after being cooled to a temperature below 120°C.
[0030] Furthermore, the chemical composition of the low reduction ratio vanadium-containing hot-rolled H-beam is: C 0.15%-0.22%, Si 0.15%-0.55%, Mn 1.25%-1.65%, P≤0.030%, S≤0.030%, V 0.015%-0.12%, Nb 0-0.03%, Ti 0-0.02%, Ceq 0.40%-0.47%; the balance is Fe and unavoidable impurities.
[0031] The design idea of the composition of the low reduction ratio hot-rolled H-beam of the present invention is as follows:
[0032] C: Controlling the carbon content is crucial to improving the strength of steel, but too high a carbon content will reduce the plasticity, toughness and weldability of the steel. Therefore, the C content is controlled to 0.15% to 0.22%.
[0033] Si: Appropriate content of Si can play a strong solid solution strengthening role, but too high Si content will accelerate high-temperature delamination, reduce toughness and lamellar tearing resistance, so the Si content is controlled to 0.15% to 0.55%.
[0034] Mn: Mn, as a strengthening element in steel, can improve the strength and hardenability of steel. However, too high a Mn content will increase the risk of composition and structural segregation of the continuous casting billet. Therefore, the Mn content is controlled to 1.25% to 1.65%.
[0035] As impurity elements, P and S will have an adverse effect on the plasticity, toughness and weldability of steel. In order to take into account the difficulty of steelmaking control, the P and S contents are controlled below 0.030%.
[0036] V: V can form V (C, N) dispersed compounds with C and N elements and distribute in the steel matrix to play a role of precipitation strengthening. It also serves as a ferrite phase deformation nucleus to refine the ferrite grains. However, too high a V content will lead to coarse precipitates and affect toughness. Therefore, the V content is controlled to 0.015% to 0.12%.
[0037] It should be noted that when the V content in the steel is less than 0.05%, the vanadium element is obtained through the vanadium-nitrogen alloy. When the V content is ≥ 0.05%, 70% of the vanadium element is obtained by adding the vanadium-nitrogen alloy and 30% is obtained by the vanadium-iron alloy.
[0038] Furthermore, the flange thickness of the H-shaped steel is 35 mm to 37 mm, the yield strength is ≥360 MPa, the tensile strength is 510 MPa to 600 MPa, the yield strength ratio is 0.7 to 0.8, and the elongation is 20% to 30%.
[0039] The hot-rolled H-shaped steel with the above composition adopts the production method of the present invention, and the prepared H-shaped steel has high strength and low-temperature impact toughness, the tensile strength can reach 510MPa-600MPa, the yield strength is ≥360MPa, and the impact energy at 0°C is ≥100J, which meets the application requirements of high-rise buildings or large-span bridges and other fields, provides a new process for hot-rolled H-shaped steel with extremely low compression ratio, fills the gap in the existing technology, and has high promotion and application value. DETAILED DESCRIPTION
[0040] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0041] In order to better illustrate the present invention, further examples are given below.
[0042] In the following embodiments, the production of hot-rolled H-beams is carried out by continuously loading 40 ordinary product billets (i.e., products that can meet the performance requirements without special control of each process) after a total of 30 special-shaped continuous casting billets are loaded, to ensure that the time each billet spends in the heating furnace is nearly consistent.
[0043] Example 1
[0044] The embodiment of the present invention provides a low reduction ratio, low temperature and high strength hot-rolled H-shaped steel, the chemical composition of which is:
[0045] C 0.16%, Si 0.28%, Mn 1.44%, P 0.020%, S 0.006%, V 0.054%, Ceq 0.42%; the balance is Fe and unavoidable impurities.
[0046] The production method of the above-mentioned low reduction ratio, low temperature and high strength hot-rolled H-beam has the following steps:
[0047] S1, smelting the steel-making raw materials in a converter to obtain molten steel meeting the above composition requirements;
[0048] S2, tap the molten steel into the LF refining furnace, the molten steel inlet temperature is 1565℃, adopt the three-phase graphite electrode heating process, open the ladle argon system, add 2kg / t refining slag, 8kg / t lime, 3kg / t calcium carbide, and 2kg / t silicon-based deoxidizer into the ladle in sequence, ensure that the slagging time does not exceed 3min, refine for 12min, raise the electrode to measure the temperature, take steel samples and slag samples, and adjust according to the temperature, steel sample composition and slag sample conditions;
[0049] S3, full protection casting is adopted in the continuous casting process. When the molten steel flows from the large ladle to the tundish, the long shroud is protected by argon sealing. A covering agent is added to the surface of the tundish. The tundish cover is protected by argon sealing at three points on both sides and in the middle. The crystallizer is protected by argon sealing of the long shroud. The gap of the tundish slide is protected by argon sealing tube. The profiled blank with the cross-sectional size of 555mm×440mm×105mm×78mm is obtained.
[0050] During the casting process, the flow ratio of cooling water between the inner and outer arcs and the left and right arcs of the crystallizer is 1:1.56, the specific water volume of the secondary cooling water is 0.7kg / L, and the secondary cooling is divided into 5 cooling zones. The ratio of the total water volume of each zone is zone 1: zone 2: zone 3: zone 4: zone 5 = 1:0.97:0.6:0.13:0.1, among which, the water volume of the inner arc in zone 2: the water volume of the outer arc = 0.77:1, the water volume of the inner arc in zone 3: the water volume of the outer arc = 0.56:1, the water volume of the inner arc in zone 4: the water volume of the outer arc = 0.33:1, and the water volume of the inner arc in zone 5: the water volume of the outer arc = 0.25:1;
[0051] S4, the special-shaped billets are put into the furnace with fully cold room temperature billets, the step distance of the walking beam is set to 460*2mm, and the steel-out rhythm is controlled according to the table before the billets are put into the furnace. Two empty positions are set before and after 10 special-shaped billets are continuously loaded, and the special-shaped billets are put into the furnace for heating. The temperature of the first heating stage is 930℃, and the holding time is 55min. The temperature of the second heating stage is 1130℃, and the holding time is 45min. The temperature of the third heating stage is 1252℃, and the holding time is 39-42min. The temperature of the equalizing stage is 1245℃, and the holding time is 39-42min. The total time in the furnace is 172-181min; the two empty positions in front of the first group of 10 billets are all discharged according to the charging speed of 1.5min; the two empty positions in front of the second group of 10 billets are adjusted in the furnace time according to the charging speed of 1.5min for discharging, and one empty position in front of the third group of 10 billets is discharged according to the charging speed of 1.5min, and the other is discharged according to the discharging speed of 4.5min;
[0052] S5, after the profiled blank is taken out of the furnace, high-pressure water is used for dephosphorization, the dephosphorization pressure is 25MPa, the rough rolling adopts 7 rolling passes, the starting rolling temperature is 1140℃, after the rough rolling is completed, the roller waits for 10s to ensure that the temperature before entering the finishing mill is 965℃; the finishing rolling adopts 5 rolling passes, the roller speed is 1.3m / s, the final rolling temperature is 890℃, and the rolling adopts 8 times the length;
[0053] S6, after rolling is completed, the finished rolled piece is water-cooled and then naturally cooled on a cooling bed. After cooling to a temperature below 120°C, it is straightened in a straightening machine to obtain a hot-rolled H-shaped steel with a flange thickness of 37 mm and a compression ratio of 2.10.
[0054] Example 2
[0055] The embodiment of the present invention provides a low reduction ratio, low temperature and high strength hot-rolled H-shaped steel, the chemical composition of which is:
[0056] C 0.17%, Si 0.31%, Mn 1.46%, P 0.022%, S 0.007%, V 0.055%, Ceq 0.43%; the balance is Fe and unavoidable impurities.
[0057] The production method of the above-mentioned low reduction ratio, low temperature and high strength hot-rolled H-beam has the following steps:
[0058] S1, smelting the steel-making raw materials in a converter to obtain molten steel meeting the above composition requirements;
[0059] S2, tap the molten steel into the LF refining furnace, the molten steel inlet temperature is 1568℃, adopt the three-phase graphite electrode heating process, open the ladle argon system, add 2kg / t refining slag, 8kg / t lime, 3kg / t calcium carbide, and 2kg / t silicon-based deoxidizer into the ladle in sequence, ensure that the slagging time does not exceed 3min, refine for 10min, raise the electrode to measure the temperature, take steel samples and slag samples, and adjust according to the temperature, steel sample composition and slag sample conditions;
[0060] S3, full protection casting is adopted in the continuous casting process. When the molten steel flows from the large ladle to the tundish, the long shroud is protected by argon sealing. A covering agent is added to the surface of the tundish. The tundish cover is protected by argon sealing at three points on both sides and in the middle. The crystallizer is protected by argon sealing of the long shroud. The gap of the tundish slide is protected by argon sealing tube. The profiled blank with the cross-sectional size of 555mm×440mm×105mm×78mm is obtained.
[0061] During the casting process, the flow ratio of cooling water between the inner and outer arcs and the left and right arcs of the crystallizer is 1:1.6, the specific water volume of the secondary cooling water is 0.6L / kg, and the secondary cooling is divided into 5 cooling zones. The ratio of the total water volume of each zone is zone 1: zone 2: zone 3: zone 4: zone 5 = 1:0.94:0.65:0.15:0.1, among which, the water volume of the inner arc of zone 2: the water volume of the outer arc = 0.767:1, the water volume of the inner arc of zone 3: the water volume of the outer arc = 0.5:1, the water volume of the inner arc of zone 4: the water volume of the outer arc = 0.32:1, and the water volume of the inner arc of zone 5: the water volume of the outer arc = 0.26:1;
[0062] S4, the special-shaped billets are put into the furnace with fully cold room temperature billets, the step distance of the walking beam is set to 460*2mm, and the steel tapping rhythm is controlled according to the table before the billets are put into the furnace. Two empty spaces are set before and after 10 special-shaped billets are continuously loaded, and the special-shaped billets are put into the furnace for heating. The temperature of the first heating stage is 935℃, and the holding time is 55min. The temperature of the second heating stage is 1140℃, and the holding time is 42min. The temperature of the third heating stage is 1250℃, and the holding time is 39-42min. The temperature of the equalizing stage is 1245℃, and the holding time is 39-42min. The total time in the furnace is 175-181min; the two empty spaces in front of the first group of 10 billets are tapped at a steel loading speed of 1.5min; the two empty spaces in front of the second group of 10 billets are tapped at a steel loading speed of 1.5min, and the other is tapped at a steel tapping speed of 4.5min; the two empty spaces in front of the third group of 10 billets are both tapped at a steel loading speed of 1.5min;
[0063] S5, after the profiled blank is taken out of the furnace, high-pressure water is used for dephosphorization, the dephosphorization pressure is 20MPa, the rough rolling adopts 7 rolling passes, the starting rolling temperature is 1120℃, after the rough rolling is completed, the roller waits for 6s to ensure that the temperature before entering the finishing mill is 975℃; the finishing rolling adopts 5 rolling passes, the roller speed is 1.4m / s, the final rolling temperature is 890℃, and the rolling adopts 8 times the length;
[0064] S6, after rolling is completed, the finished rolled piece is water-cooled and then naturally cooled on a cooling bed. After cooling to a temperature below 120°C, it is straightened in a straightening machine to obtain a hot-rolled H-shaped steel with a flange thickness of 37 mm and a compression ratio of 2.10.
[0065] Example 3
[0066] The embodiment of the present invention provides a low reduction ratio, low temperature and high strength hot-rolled H-shaped steel, the chemical composition of which is:
[0067] C 0.15%, Si 0.30%, Mn 1.40%, P 0.025%, S 0.004%, V 0.039%, Ceq 0.41%; the balance is Fe and unavoidable impurities.
[0068] The production method of the above-mentioned low reduction ratio, low temperature and high strength hot-rolled H-beam has the following steps:
[0069] S1, smelting the steel-making raw materials in a converter to obtain molten steel meeting the above composition requirements;
[0070] S2, tap the molten steel into the LF refining furnace, the molten steel inlet temperature is 1558℃, adopt the three-phase graphite electrode heating process, open the ladle argon system, add 2.5kg / t refining slag, 6kg / t lime, 3kg / t calcium carbide, and 2kg / t silicon-based deoxidizer into the ladle in sequence, ensure that the slagging time does not exceed 3min, refine for 8min, raise the electrode to measure the temperature, take steel samples and slag samples, and adjust according to the temperature, steel sample composition and slag sample conditions;
[0071] S3, full protection casting is adopted in the continuous casting process. When the molten steel flows from the large ladle to the tundish, the long shroud is protected by argon sealing. A covering agent is added to the surface of the tundish. The tundish cover is protected by argon sealing at three points on both sides and in the middle. The crystallizer is protected by argon sealing of the long shroud. The gap of the tundish slide is protected by argon sealing tube. The profiled blank with the cross-sectional size of 555mm×440mm×105mm×78mm is obtained.
[0072] During the casting process, the flow ratio of cooling water between the inner and outer arcs and the left and right arcs of the crystallizer is 1:1.7, the specific water volume of the secondary cooling water is 0.8kg / L, and the secondary cooling is divided into 5 cooling zones. The ratio of the total water volume of each zone is zone 1: zone 2: zone 3: zone 4: zone 5 = 1:0.95:0.7:0.14:0.11, among which, the water volume of the inner arc in zone 2: the water volume of the outer arc = 0.774:1, the water volume of the inner arc in zone 3: the water volume of the outer arc = 0.52:1, the water volume of the inner arc in zone 4: the water volume of the outer arc = 0.33:1, and the water volume of the inner arc in zone 5: the water volume of the outer arc = 0.24:1;
[0073] S4, the special-shaped billets are put into the furnace with fully cold room temperature billets, the step distance of the walking beam is set to 460*2mm, and the steel-out rhythm is controlled according to the table before the billets are put into the furnace. Two empty positions are set before and after 10 special-shaped billets are continuously loaded, and the special-shaped billets are put into the furnace for heating. The temperature of the first heating stage is 945℃, and the holding time is 55min. The temperature of the second heating stage is 1135℃, and the holding time is 39min. The temperature of the third heating stage is 1250℃, and the holding time is 39-42min. The temperature of the soaking stage is 1245℃, and the holding time is 39-42min. The total time in the furnace is 172-181min; the two empty positions in front of the first group of 10 billets are both discharged at a charging speed of 4.5min; the two empty positions in front of the second group of 10 billets are discharged at a charging speed of 1.5min, and the other is discharged at a discharge speed of 4.5min; the two empty positions in front of the third group of 10 billets are discharged at a charging speed of 1.5min, and the other is discharged at a discharge speed of 4.5min; the two empty positions in front of the third group of 10 billets are discharged at a charging speed of 1.5min, and the other is discharged at a discharge speed of 4.5min;
[0074] S5, after the profiled blank is taken out of the furnace, high-pressure water is used for dephosphorization, the dephosphorization pressure is 24MPa, the rough rolling adopts 7 rolling passes, the starting rolling temperature is 1080℃, after the rough rolling is completed, the roller waits for 3s to ensure that the temperature before entering the finishing mill is 955℃; the finishing rolling adopts 5 rolling passes, the roller speed is 1.5m / s, the final rolling temperature is 880℃, and the rolling adopts 8 times the length;
[0075] S6, after the rolling is completed, the finished rolled piece is water-cooled and then naturally cooled on a cooling bed. After being cooled to a temperature below 120°C, it is straightened in a straightening machine to obtain a hot-rolled H-shaped steel with a flange thickness of 35 mm and a compression ratio of 2.20.
[0076] Example 4
[0077] The embodiment of the present invention provides a low reduction ratio, low temperature and high strength hot-rolled H-shaped steel, the chemical composition of which is:
[0078] C 0.15%, Si 0.34%, Mn 1.38%, P 0.016%, S 0.007%, V 0.041%, Ceq 0.40%; the balance is Fe and inevitable impurities.
[0079] The production method of the above-mentioned low reduction ratio, low temperature and high strength hot-rolled H-beam has the following steps:
[0080] S1, smelting the steel-making raw materials in a converter to obtain molten steel meeting the above composition requirements;
[0081] S2, tap the molten steel into the LF refining furnace, the molten steel inlet temperature is 1563℃, adopt the three-phase graphite electrode heating process, open the ladle argon system, add 2.5kg / t refining slag, 6kg / t lime, 3.2kg / t calcium carbide, and 2kg / t silicon-based deoxidizer into the ladle in sequence, ensuring that the slagging time does not exceed 3min, refine for 15min, raise the electrode to measure the temperature, take steel samples and slag samples, and adjust according to the temperature, steel sample composition and slag sample conditions;
[0082] S3, full protection casting is adopted in the continuous casting process. When the molten steel flows from the large ladle to the tundish, the long shroud is protected by argon sealing. A covering agent is added to the surface of the tundish. The tundish cover is protected by argon sealing at three points on both sides and in the middle. The crystallizer is protected by argon sealing of the long shroud. The gap of the tundish slide is protected by argon sealing tube. The profiled blank with the cross-sectional size of 555mm×440mm×105mm×78mm is obtained.
[0083] During the casting process, the flow ratio of cooling water between the inner and outer arcs and the left and right arcs of the crystallizer is 1:1.8, the specific water volume of the secondary cooling water is 0.9kg / L, and the secondary cooling is divided into 5 cooling zones. The ratio of the total water volume of each zone is zone 1: zone 2: zone 3: zone 4: zone 5 = 1:0.96:0.75:0.13:0.1, among which, the water volume of the inner arc in zone 2: the water volume of the outer arc = 0.77:1, the water volume of the inner arc in zone 3: the water volume of the outer arc = 0.54:1, the water volume of the inner arc in zone 4: the water volume of the outer arc = 0.34:1, and the water volume of the inner arc in zone 5: the water volume of the outer arc = 0.25:1;
[0084] S4, the special-shaped billets are put into the furnace with fully cold room temperature billets, the step distance of the walking beam is set to 460*2mm, and the steel tapping rhythm is controlled according to the table before the billets are put into the furnace. Two empty spaces are set before and after 10 special-shaped billets are continuously loaded, and the special-shaped billets are put into the furnace for heating. The temperature of the first heating stage is 945℃, and the holding time is 55min. The temperature of the second heating stage is 1135℃, and the holding time is 45min. The temperature of the third heating stage is 1250℃, and the holding time is 39-42min. The temperature of the equalizing stage is 1245℃, and the holding time is 39-42min. The total time in the furnace is 172-181min; the two empty spaces in front of the first group of 10 billets are tapped at a steel loading speed of 4.5min; the two empty spaces in front of the second group of 10 billets are tapped at a steel loading speed of 1.5min, and the other is tapped at a steel tapping speed of 4.5min. The two empty spaces in front of the third group of 10 billets are tapped at a steel loading speed of 1.5min;
[0085] S5, after the profiled blank is taken out of the furnace, high-pressure water is used for dephosphorization, the dephosphorization pressure is 26MPa, the rough rolling adopts 7 rolling passes, the starting rolling temperature is 1130℃, after the rough rolling is completed, the roller waits for 8s to ensure that the temperature before entering the finishing mill is 975℃; the finishing rolling adopts 5 rolling passes, the roller speed is 1.3m / s, the final rolling temperature is 885℃, and the rolling adopts 8 times the length;
[0086] S6, after the rolling is completed, the finished rolled piece is water-cooled and then naturally cooled on a cooling bed. After being cooled to a temperature below 120°C, it is straightened in a straightening machine to obtain a hot-rolled H-shaped steel with a flange thickness of 35 mm and a compression ratio of 2.20.
[0087] The chemical composition of the hot-rolled H-shaped steel in the above-mentioned embodiments 1 to 4 may also adopt other contents defined in the present invention, as long as the carbon equivalent ceq=C%+Mn% / 6+(V%+Cr%+Mo) / 5+(Ni%+Cu%) / 15 is within the range of 0.40% to 0.47% defined in the present invention, the technical effects equivalent to those of embodiments 1 to 4 can be achieved.
[0088] Performance Testing
[0089] The sampling position of the specimens used for mechanical properties is on the flange of the H-shaped steel, 1 / 3 from the edge to the center, and the reference standard is GB / T 2975-2018 "Sampling Position and Specimen Preparation for Mechanical Properties Test of Steel and Steel Products"; the test methods for yield strength, tensile strength, and elongation refer to the standard national standard GB / T 228.1-2021 "Tensile test of metallic materials Part 1: Room temperature test method"; the impact energy test method refers to the standard national standard GB / T 229-2020 "Charpy Pendulum Impact Test Method for Metallic Materials".
[0090] Table 1 Mechanical properties
[0091]
[0092] It can be seen from the above table that the hot-rolled H-beams produced in each embodiment of the present invention have high strength and good low-temperature impact toughness, providing an excellent production process for low reduction ratio hot-rolled H-beams, filling the gap in the prior art, and having high practical value.
[0093] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for producing low-compression ratio vanadium-containing hot-rolled H-beam, wherein the compression ratio of the H-beam is 2.1-2.2, and the average longitudinal impact energy at 0°C is ≥100J, characterized in that: The production method includes converter or electric furnace smelting, LF refining, full-protection continuous casting of profiled blanks, heating, rolling and cooling processes, wherein: In the full-protection continuous casting process of the profiled blank, the flow ratio of the cooling water of the inner and outer arcs of the crystallizer to the left and right arcs is 1:1.5-1.8, the specific water volume of the secondary cooling water is 0.6L / kg-0.9kg / L, the secondary cooling is divided into 5 cooling zones, and the ratio of the total water volume of each zone is zone 1: zone 2: zone 3: zone 4: zone 5 = 1: 0.94-0.97: 0.6-0.75: 0.13-0.15: 0.1-0.11, wherein the water volume of the inner arc in zone 2: the water volume of the outer arc = 0.767-0.774: 1, the water volume of the inner arc in zone 3: the water volume of the outer arc = 0.5-0.56: 1, the water volume of the inner arc in zone 4: the water volume of the outer arc = 0.32-0.34: 1, and the water volume of the inner arc in zone 5: the water volume of the outer arc = 0.24-0.26: 1; In the heating process: the continuous casting billets are loaded onto the walking beam in a manner of 2 empty spaces every 10 consecutive billets, put into the furnace for heating and insulation, and discharged after the insulation is completed; wherein, when discharging, the steel-discharging rhythm of the empty spaces at the outlet is controlled according to the total insulation time of the continuous casting billets in the heating furnace being 150min to 180min: if the continuous casting billets in the heating furnace do not reach the requirement of the total insulation time after the rolling of the previous continuous casting billet is completed, the steel-discharging rhythm of the empty spaces at the outlet is preset; if the continuous casting billets in the heating furnace reach or exceed the requirement of the total insulation time after the rolling of the previous continuous casting billet is completed, the steel-discharging rhythm of the empty spaces at the outlet is preset.
2. The method for producing low reduction ratio vanadium-containing hot-rolled H-beam according to claim 1, characterized in that: In the heating process, the heating furnace is divided into heating stage one, heating stage two, heating stage three and a soaking stage, wherein the temperature of heating stage one is 910°C to 1100°C, the temperature of heating stage two is 1100°C to 1150°C, the temperature of heating stage three is 1240°C to 1260°C, and the temperature of the soaking stage is 1230°C to 1250°C.
3. The method for producing low reduction ratio vanadium-containing hot-rolled H-beam according to claim 2, characterized in that: In the heating process, the insulation time of the continuous casting billet in the first heating stage is ≥35 min, the insulation time in the second heating stage is ≥35 min, the insulation time in the third heating stage is 30 min to 45 min, and the insulation time in the equalizing stage is 30 min to 45 min.
4. The method for producing low reduction ratio vanadium-containing hot-rolled H-beam according to claim 1, characterized in that: The LF refining process comprises the following steps: adding molten steel into the LF refining furnace, blowing argon, adding refining slag, lime, calcium carbide and silicon-based deoxidizer in sequence, the slagging time is less than 3 minutes, and the refining time is 8 minutes to 15 minutes.
5. The method for producing low reduction ratio vanadium-containing hot-rolled H-beam according to claim 4, characterized in that: In the LF refining process, the amount of the refined slag added is 1kg / t to 3kg / t, the amount of the lime added is 5kg / t to 10kg / t, the amount of the calcium carbide added is 3kg / t to 5kg / t, and the amount of the silicon-based deoxidizer added is 1kg / t to 3kg / t.
6. The method for producing low reduction ratio vanadium-containing hot-rolled H-beam according to claim 4, characterized in that: In the LF refining process, the temperature of the molten steel entering the furnace is 1560°C to 1580°C.
7. The method for producing low reduction ratio vanadium-containing hot-rolled H-beam according to claim 1, characterized in that: In the full-protection continuous casting process of the profiled blank, when the molten steel flows from the large ladle into the tundish, a long shroud is used for casting with argon sealing protection, a covering agent is added to the surface of the tundish, the tundish cover is protected by argon sealing at three points on both sides and in the middle, the crystallizer is protected by an argon-sealed long shroud, and the gap of the tundish slide plate is protected by an argon-sealed tube.
8. The method for producing low reduction ratio vanadium-containing hot-rolled H-beam according to claim 1, characterized in that: In the rolling process, the rough rolling adopts 7 rolling passes, the start rolling temperature is 1050℃~1150℃, the finish rolling adopts 5 rolling passes, the roll speed is 1.3m / s~1.5m / s, and the final rolling temperature is 850℃~900℃.
9. The method for producing low reduction ratio vanadium-containing hot-rolled H-beam according to claim 1, characterized in that: The chemical composition of the low reduction ratio vanadium-containing hot-rolled H-beam is: C 0.15%-0.22%, Si 0.15%-0.55%, Mn 1.25%-1.65%, P≤0.030%, S≤0.030%, V0.015%-0.12%, Nb 0-0.03%, Ti 0-0.02%, Ceq0.40%-0.47%; the balance is Fe and unavoidable impurities.
10. The method for producing low reduction ratio vanadium-containing hot-rolled H-beam according to any one of claims 1 to 9, characterized in that: The flange thickness of the H-shaped steel is 35 mm to 37 mm, the yield strength is ≥360 MPa, the tensile strength is 510 MPa to 600 MPa, the yield strength ratio is 0.7 to 0.8, and the elongation is 20% to 30%.