High-toughness hydrogen storage alloy powder as well as powder preparation method and device thereof

Through liquid nitrogen deep-cold brittle enhancement technology and low-temperature mechanical crushing, the problem of impurities introduction and oxidation of vanadium-based and zirconium-based hydrogen storage alloys during the powder making process is solved, and a high-purity and defect-free hydrogen storage alloy preparation is achieved. Improves powder making efficiency and cycle stability.

CN119016731APending Publication Date: 2024-11-26GRIMAT ENG INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410672576.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-28
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to effectively prepare high-purity, defect-free, uniform particle size vanadium-based and zirconium-based hydrogen storage alloy powders, especially strong and high-strength hydrogen storage alloy materials, which are prone to introduce impurities and oxidation during the powder making process. Moreover, traditional methods are difficult to meet actual production needs.

Method used

Using liquid nitrogen deep-cold brittle enhancement technology combined with low-temperature mechanical crushing, a deep-cold-low-temperature crushing powder preparation device and method was developed. By crushing and crushing the hydrogen storage alloy under low temperature conditions, the hydrogenation process is avoided and defect-free and high Preparation of alloy powder of purity.

Benefits of technology

The preparation of hydrogen storage alloy powders without impurities, low defects, and controllable particle size distribution is achieved, which significantly improves the powdering efficiency, reduces material toxicity, and improves circulation stability and powder quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016731A_ABST
    Figure CN119016731A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of hydrogen storage materials, and particularly relates to high-toughness hydrogen storage alloy powder and a powder preparation method and device thereof. The powder preparation method comprises the following steps: freezing a block body of a hydrogen storage alloy cast ingot, so that the material is cooled to be below the hot brittle transition temperature-60 DEG C; crushing twice to obtain a material with the fineness of less than or equal to 20 meshes; and finally, under the vacuum condition, heating to the room temperature to obtain the hydrogen storage alloy powder. According to the invention, a cryogenic embrittlement increasing technology is utilized, and the material is cryogenically cooled to a temperature below a thermal brittle transition temperature, so that the brittleness of the material is effectively enhanced, brittle fracture occurs in an alloy powder preparation process, and lattice distortion is reduced; and the high-temperature oxidation phenomenon in the traditional powder preparation process is effectively avoided, and defect-free and high-quality powder preparation is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of hydrogen storage materials, and in particular relates to a strong and tough hydrogen storage alloy powder and a powder making method and device thereof. Background Art

[0002] Hydrogen energy is a secondary energy source with abundant sources, green and low carbon, and wide applications. It can help to absorb renewable energy on a large scale, realize large-scale peak load regulation of power grids, and cross-seasonal and cross-regional energy storage, and accelerate the low-carbonization of industries, construction, transportation, etc. Accelerating the development of the hydrogen energy industry is an important path to help my country achieve its carbon peak and carbon neutrality goals. The development and utilization of hydrogen energy is triggering a profound energy revolution. Hydrogen energy has become a new code to solve the energy crisis and build a clean, low-carbon, safe and efficient modern energy system.

[0003] However, the use of hydrogen energy requires solving the following three problems: hydrogen production, storage and transportation, and application. Among them, the storage and transportation of hydrogen energy is the key to hydrogen energy application. Solid-state hydrogen storage uses the physical adsorption or chemical reaction of solids on hydrogen to store hydrogen in solid materials. Solid-state hydrogen storage can generally be safe, efficient, and high-density, and is the most promising research discovery after gaseous storage and liquid storage.

[0004] As solid hydrogen storage materials, vanadium-based and zirconium-based hydrogen storage alloys have the advantage of high hydrogen storage capacity compared to rare earth LaNi5, TiFe, TiMn2 and other widely used hydrogen storage materials. The maximum hydrogen absorption of vanadium-based hydrogen storage alloys at room temperature is higher than 3.6wt%. However, they show higher hardness and stronger toughness, and the Mohs hardness is usually above 6. The powdering process of such hydrogen storage alloy materials is easy to introduce impurity elements such as C and O, and it is difficult to obtain high-purity alloy powder. At present, the commonly used powdering methods for vanadium-based and zirconium-based hydrogen storage alloys are mechanical crushing powdering method and hydrogenation crushing powdering method.

[0005] Patent CN2023107042396 discloses a high-platform vanadium-based hydrogen storage alloy and its preparation method. The obtained vanadium-based hydrogen storage alloy is crushed by mechanical methods, and the average particle size of the alloy obtained after screening is 0.3 cm. In the actual production and application process, the powder particle size suitable for high-density, fast-response hydrogen storage devices is usually below 20 mesh (about 0.85 mm). Larger particle size is not conducive to the rapid penetration and release of hydrogen. Therefore, the mechanical crushing method used in this patent cannot obtain alloy powder suitable for actual production application needs.

[0006] Patent CN2020104230559 discloses a method for hydrogenating, crushing and powdering vanadium-based hydrogen storage alloys. For vanadium-based hydrogen storage alloy materials with strong toughness, the internal stress during the hydrogenation of the alloy is used to crush the alloy into powder. However, the surface of the hydrogenated alloy has high activity and must be avoided from contact with air during subsequent use. Contact with air will cause the alloy to be poisoned and its performance to decay. Therefore, it is not suitable for large-scale preparation and use.

[0007] The frozen powder making method is a powder making method commonly used in the fields of traditional Chinese medicine, food and rubber. Patent CN981034926 discloses a low-temperature powder making method for traditional Chinese medicine. Fresh Chinese medicinal materials are frozen at a low temperature of 0-196°C using liquid nitrogen refrigerant. The frozen Chinese medicinal materials are sent to a deep-cold grinder to be crushed into powder. This method has a simple manufacturing process and can ensure the efficacy of traditional Chinese medicine.

[0008] Patent CN2021109805684 discloses a system for cryogenic powdering of solid waste such as waste tires and waste plastics using liquid nitrogen. A liquid nitrogen ball mill is used to crush waste tires and waste plastics. The brittleness of the waste tire plastics obtained after deep cooling increases. This method can effectively improve the crushing efficiency. For low-toughness and low-strength hydrogen storage alloy materials, such as AB, AB2, and AB5 series hydrogen storage alloys, mechanical crushing can be directly used, and then the desired powder particle size can be achieved through ball milling. However, there is currently no mature powdering method for strong and tough, high-strength hydrogen storage alloy materials, such as vanadium-based hydrogen storage alloys and zirconium-based hydrogen storage alloys.

[0009] Patent CN2019106915596 discloses a preparation method of a high-power hydrogen storage alloy powder and a high-power hydrogen storage alloy powder. The powder making step includes first mechanically crushing the hydrogen storage alloy in an oxygen-free environment (particle size is 10-100 μm); then secondary crushing (particle size is less than 5 μm) in an oxygen-free environment below 5°C (using ethanol, isopropanol, etc. as the medium; the low-temperature environment is manufactured by including but not limited to a liquid nitrogen environment); wherein the first mechanical crushing uses a jaw crusher, and the secondary crushing uses an ultrasonic crushing method or a high-energy ball milling method. The applicable alloy system is a lanthanum-cerium-nickel-cobalt-manganese-aluminum alloy material, which has a low hardness and the alloy is not ductile. Conventional crushing equipment can be used for crushing and powder making, such as a jaw crusher, a ball mill, etc., and it is only necessary to pay attention to avoiding oxidation of the powder during the powder making process. For vanadium-based and zirconium-based alloys with high hardness and toughness, the conventional mechanical crushing method cannot achieve the powder making effect, and oxidation and the introduction of impurities must also be avoided during the powder making process. There is currently no mature powder making method.

[0010] Patents CN201110152699X and CN2012102154787 disclose a method of directly subjecting an alloy block to low-temperature liquid nitrogen cooling and impact grinding, that is, the heat-treated alloy (800-1200°C) is directly placed in liquid nitrogen for rapid cooling and then subjected to impact grinding for powder. The rapid cooling of liquid nitrogen here is beneficial to improving the electrochemical properties of the material and has no direct relationship to the alloy powder making process.

[0011] Patent CN2020112502199 discloses a method for preparing metallic chromium powder by ultra-low temperature grinding. During the crushing and powdering process, a liquid nitrogen environment is used throughout the process. This method has high requirements for supporting equipment and the process is cumbersome, which is not conducive to large-scale production and application.

[0012] Therefore, how to improve the preparation efficiency of solid hydrogen storage materials, especially vanadium-based, zirconium-based and other high-strength, high-toughness hydrogen storage alloy powders, to obtain pollution-free powders with high particle size uniformity is a key issue that urgently needs to be solved in this field. Summary of the invention

[0013] The present application introduces the liquid nitrogen cryogenic powder making method into the field of toughness, high-strength hydrogen storage alloy material powder making, and utilizes the characteristics of the alloy undergoing toughness-brittleness transition under low temperature conditions to achieve mechanical crushing of the alloy, avoid the hydrogenation process, and obtain defect-free, high-purity alloy powder.

[0014] In order to solve the problem of difficulty in crushing and powdering due to the high strength and toughness of vanadium-based and zirconium-based hydrogen storage alloys, we use liquid nitrogen deep-cold embrittlement technology, combined with low-temperature mechanical crushing and powdering technology, to develop a semi-continuous deep-cold-low-temperature crushing powder preparation device and method of use, and to develop a powder preparation technology with low defects, no impurities, and controllable particle size distribution.

[0015] In order to solve the above problems, the present invention proposes a method for preparing a strong and tough hydrogen storage alloy, comprising the following steps:

[0016] 1) splitting and pre-treating the ingot of hydrogen storage alloy to obtain alloy blocks;

[0017] 2) Freeze the alloy block to cool the material to below the hot brittle transition temperature of -60°C;

[0018] 3) crushing the alloy block frozen in step 2) to obtain a material with a fineness of ≤2 cm;

[0019] 4) further crushing and grinding the material obtained in step 3) to obtain a material with a fineness of ≤20 mesh;

[0020] 5) The crushed material is placed under vacuum conditions and heated to room temperature to obtain hydrogen storage alloy powder.

[0021] In some preferred embodiments, the step 2) has a hot brittle transition temperature of -150°C to -60°C, preferably -90°C;

[0022] and / or

[0023] The step 2) uses liquid nitrogen as a cryogenic medium for freezing;

[0024] and / or

[0025] The freezing time of step 2) is 5-60 minutes.

[0026] In some preferred embodiments, the diameter of the alloy block in step 1) is ≤10 cm, preferably ≤9 cm, ≤8 cm, ≤7 cm, ≤6 cm, ≤5 cm; more preferably 2 to 5 cm;

[0027] and / or

[0028] The method of segmentation pretreatment in step 1) includes wire cutting and / or mechanical impact;

[0029] and / or

[0030] The hydrogen storage alloy is selected from any one or more of the following: x Ti 1-x , V x Cr y Ti z , V x Cr y Ti z Ce m , Zr a Co b , Zr a Ti b Co c , among which, 0.4≤x≤100, 0.2≤y≤0.5, 0.2≤z≤0.5, 0≤m≤0.1, 0.4≤a≤0.6, 0.4≤b≤0.6.

[0031] In some preferred embodiments, the step 3) crushing is carried out by any of the following methods: jaw crusher, hammer crusher;

[0032] and / or

[0033] The step 4) of preparing the powder is carried out by any of the following methods: a sample preparation pulverizer, a ball mill, a cutting pulverizer, or a Raymond pulverizer;

[0034] and / or

[0035] In the Raymond mill, during the pulverizing process, the main engine speed is 10 rpm to 150 rpm, the air temperature is -30°C to 0°C, and the air flow speed is 2 to 100 m / s;

[0036] and / or

[0037] The gas used in the Raymond mill is an inert gas;

[0038] and / or

[0039] The gas used is selected from any one of the following: argon, nitrogen, and helium.

[0040] In some preferred embodiments, the vacuum condition in step 5) is P≤0.001MPa;

[0041] and / or

[0042] The time of placing the device under vacuum condition in step 5) is 1 to 4 hours, preferably 2 hours or 3 hours.

[0043] The hydrogen storage alloy powder prepared in step 5) is sealed and stored under vacuum conditions.

[0044] The present invention also provides a strong and tough hydrogen storage alloy powder prepared by the powder making method.

[0045] The present invention provides a cryogenic-low temperature pulverizing powder making equipment for the powder making method, comprising a liquid nitrogen cryogenic system, a primary crushing system, a low temperature pulverizing powder making system and a material collecting system connected in series in sequence;

[0046] a) The liquid nitrogen cryogenic system comprises a cryogenic tank 1, which is connected to a liquid nitrogen tank 12 for filling with liquid nitrogen; a cryogenic tank feeding port 11 is provided on the cryogenic tank 1, an inner jacket 14 is provided inside, and a liquid level sensor 13 is installed;

[0047] The inner jacket 14 is an irregular cylindrical structure or a funnel-shaped structure; the inner diameter of the feed port end of the inner jacket 14 is greater than the inner diameter of the discharge port end;

[0048] A spiral conveyor belt 15 is provided at the discharge port of the inner jacket 14 to convey the material to the primary crushing system;

[0049] The material enters from the feeding port 11 of the cryogenic tank, passes through the upper end and the lower end of the inner jacket 14 in sequence, and is conveyed from the discharge port of the inner jacket 14 to the primary crushing system via the spiral conveyor 15;

[0050] b) The primary crushing system includes a jaw crusher 2, a jaw crusher feed port 21, and a horizontal conveyor belt 22; the material enters the jaw crusher 2 through the jaw crusher feed port 21, and after the crushing is completed, the material is conveyed to the low-temperature crushing and powder making system through the horizontal conveyor belt 22;

[0051] c) The low-temperature pulverizing and milling system comprises a Raymond mill 3, a Raymond mill feed port 31, a Raymond mill discharge port 32, a drag shovel 33, a grinding roller device 34, a main shaft 35, an air supply port 36, and a sieve plate 37; the material is added into the machine from the Raymond mill feed port 31 of the Raymond mill 3, the grinding roller device 34 and the drag shovel 33 are suspended on the plum blossom frame of the main shaft 35 of the Raymond mill 3, and the drag shovel 33 is located vertically below the hanging grinding roller device 34; the main body shell of the Raymond mill 3 is provided with an air supply port 36; the Raymond mill discharge port 32 is located at the vertical upper part of the Raymond mill 3, and a sieve plate 37 is provided at the upstream of the material of the Raymond mill discharge port 32 near the Raymond mill discharge port 32; after the material is ground, the low-temperature inert gas generated by the fan is blown into the main body shell of the Raymond mill 3, and is sorted through the sieve plate 37 placed above the grinding chamber;

[0052] d) The material collection system includes a material collector 4, a material collection feed port 41, a material collection discharge port 42, a material storage 43, an air outlet 44, a vacuum valve 45, a heating sleeve 46, and an agitator 47; a material collection feed port 41 and an air outlet 44 are provided at the vertical upper part of the material collection system 4, and a material collection discharge port 42 is provided at the vertical lower part of the material collection system 4; the material is delivered from the Raymond mill discharge port 32 to the material collection feed port 41, enters the material collector 4, and then enters the material storage 43 through the material collection discharge port 42; the material storage 43 is a closed system, which is provided with a heating sleeve 46 and an agitator 47, and the pressure of the material storage 43 is adjusted by the vacuum valve 45.

[0053] The states of the alloy at different stages are: the liquid nitrogen deep cooling system is the alloy block; the primary crushing system is the alloy small block; the low-temperature crushing and powder making system is the alloy powder; the material collection system is the alloy powder.

[0054] The operation process is as follows:

[0055] The cut alloy block, with a diameter of 2-10 cm, is fed into the cryogenic tank 1 through the feeding port 11, and then the liquid nitrogen tank 12 is opened, and 10 L of liquid nitrogen is added to the inner jacket 14. The liquid nitrogen level is controlled by the liquid level sensor 13. The material is frozen for 5-60 minutes until the temperature drops below the thermal brittle transition temperature. The material is transported to the feeding port 21 of the jaw crusher 2 through the spiral conveyor belt 15, and the speed of the spiral conveyor belt is set to 1 m / s.

[0056] The jaw crusher 2 is turned on to perform preliminary crushing of the material, and the discharge particle size does not exceed 2 cm. The crushed material is transported to the entrance 31 of the Raymond mill along the horizontal conveyor belt 22, and the speed of the horizontal conveyor belt is set to 2 m / s.

[0057] Close the Raymond mill feed port 31, turn on the Raymond mill 3, open the air supply port 36, and continuously introduce low-temperature argon gas into the mill. The gas temperature is controlled at 0°C and the wind speed is set to 25m / s; the main shaft 35 speed is set to 82r / min, the drag shovel 33 lifts the material, and the grinding roller 34 rotates continuously while revolving with the main shaft 35. The material is crushed by the friction and extrusion between the grinding roller and the wall and between the grinding rollers. A 20-mesh sieve plate 37 is set at the top of the pulverizer, and the powder with a larger particle size falls back and is re-ground and crushed. The powder with a particle size smaller than 20 mesh is discharged through the Raymond mill discharge port 32, and the qualified powder further enters the material collection system 4 through the material collection feed port 41.

[0058] After the powder enters the material collection system 4, the carrier gas is discharged from the gas outlet 44, and the powder enters the material storage 43 through the material collection outlet 42. Then, the inlet valve of the material storage 43 is closed, and the vacuum valve 45 is opened. After the pressure in the material storage is better than 0.001MPa, it is maintained for 2 hours, and the agitator 47 is turned on, the speed is set to 50r / min, and the temperature of the heating jacket 47 is set to 50°C. After the material is warmed up, it is vacuum sealed and stored.

[0059] b) crushing the alloy ingot with strong and tough characteristics by wire cutting or mechanical impact to obtain alloy blocks with a diameter of less than 5 cm;

[0060] c) 5 kg of the block alloy prepared in step b is added into the cryogenic tank through the feed port 11, and 10 L of liquid nitrogen is added into the cryogenic tank through the liquid nitrogen tank 12, and the freezing time is 30 min, so that the material is cooled to below the hot brittle transition temperature; then the spiral conveyor 15 is turned on, and the conveyor speed is set to 1 m / s, and the cryogenically cooled material is conveyed to the feed port 21 of the jaw crusher;

[0061] d) Turn on the jaw crusher to preliminarily crush the material after deep cooling. The preliminarily crushed material is discharged through the discharge port 32 of the Raymond mill. The outlet material size is less than 2 cm and is conveyed to the Raymond mill 3 through the conveyor belt 22;

[0062] e) The material is added into the machine from the Raymond mill feed port 31 on the side of the machine cover shell. The feed speed is set to 2.5kg / min. The grinding roller device suspended on the main shaft plum blossom frame revolves around the vertical axis. The main shaft speed is set to 82r / min. At the same time, the grinding roller itself rotates. Due to the centrifugal force during rotation, the grinding roller swings outward and presses against the grinding ring, so that the scraper scoops up the material and sends it to between the grinding roller and the grinding ring. The rolling and rolling of the grinding roller further crushes the material. After the material is ground, the fan blows low-temperature inert gas argon into the main housing to blow up the powder, which is sorted by the sieve plate 37 placed above the grinding chamber. The wind speed is set to 25m / s. The material with too coarse fineness falls into the grinding chamber for re-grinding. The powder with a fineness less than 20 mesh enters the material collector 4 with the wind flow, and is collected and discharged through the material collection outlet 42 to obtain the finished product.

[0063] f) placing the material in the material collector 4 into the material storage 43, subjecting it to vacuum treatment, maintaining the pressure at 0.001 MPa for 2 h, turning on the agitator 47 and the heating jacket 46, and transferring the material into a vacuum sealed bag and sealing it for storage after the temperature of the material returns to room temperature.

[0064] The beneficial effects of the present invention are:

[0065] The invention discloses a method for preparing powder of a strong and tough hydrogen storage alloy. The method comprises deep-cold-low temperature pulverizing and preparing powder.

[0066] 1) The cryogenic embrittlement technology used in the present invention can effectively enhance the brittleness of the material by cryogenically cooling the material to below the thermal brittle transition temperature, so that brittle fracture occurs during the alloy powder making process, reducing the generation of lattice distortion;

[0067] 2) The cryogenic-low temperature pulverizing and powder making equipment disclosed in the present invention can realize the powder making of materials under low temperature conditions, effectively avoid the high temperature oxidation phenomenon in the traditional powder making process, and realize the preparation of defect-free and high-quality powder;

[0068] The prepared alloy powder has uniform particle size distribution, easy to control particle size, few lattice defects, is not easy to oxidize, does not introduce other impurities, and has no dust pollution. It significantly improves the efficiency of strong and tough alloy powder making, reduces the toxicity of the material powder making process, and improves cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0069] Figure 1 : Schematic diagram of deep-cold-low temperature pulverizing and powder making device;

[0070] Cryogenic tank 1, cryogenic tank feeding port 11, liquid nitrogen tank 12, liquid level sensor 13, inner jacket 14, spiral conveyor belt 15;

[0071] Jaw crusher 2, jaw crusher feed port 21, horizontal conveyor belt 22;

[0072] Raymond mill 3, Raymond mill feed port 31, Raymond mill discharge port 32, drag shovel 33, grinding roller device 34, main shaft 35, air supply port 36, sieve plate 37;

[0073] Material collector 4, material collection feed port 41, material collection discharge port 42, material storage container 43, air outlet 44, vacuum valve 45, heating jacket 46, stirrer 47;

[0074] Figure 2 : SEM image of powder prepared by cryogenic method;

[0075] Figure 3 : Particle size distribution diagram of powder prepared by cryogenic method;

[0076] Figure 4 : XRD pattern of alloy ingot;

[0077] Figure 5 : XRD pattern of powder prepared by cryogenic method;

[0078] Figure 6 : Hydrogen absorption kinetic curves of alloy ingot and powder prepared by cryogenic method;

[0079] Figure 7 : Cyclic performance curve of hydrogen absorption and desorption of powder prepared by cryogenic method. DETAILED DESCRIPTION

[0080] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments:

[0081] Example 1

[0082] A method for preparing powder of strong and tough hydrogen storage alloy, using Figure 1 The deep-cold-low-temperature pulverizing and powder-making device comprises the following steps:

[0083] (1) Using metal vanadium, titanium and chromium as raw materials, each metal raw material is prepared in a vacuum non-consumable arc furnace or a vacuum induction furnace according to the stoichiometric ratio between the elements in the hydrogen storage alloy, and the raw metals are smelted 3-5 times under an argon protective atmosphere to obtain V 75 Ti5Cr 20 Alloy ingot.

[0084] (2) breaking the alloy ingot obtained in step (1) into alloy blocks with a diameter of 5 cm by wire cutting;

[0085] (3) Add 5 kg of the alloy block cut in step (2) into a cryogenic tank, add 10 L of liquid nitrogen, and freeze the alloy block for 30 minutes;

[0086] (4) conveying the material after deep cooling in step (3) to a jaw crusher for crushing by a spiral conveyor belt, and the material size is less than 2 cm;

[0087] (5) Subsequently, the material obtained in step (4) was conveyed to a low-temperature Raymond mill via a horizontal conveyor belt. The main shaft speed of the Raymond mill was set to 82 r / min, argon was used as the air delivery gas, the gas temperature was set to 0°C, the wind speed was set to 25 m / s, and a 20-mesh sieve was provided at the material outlet.

[0088] (6) After crushing, qualified materials (i.e., below 20 mesh) are transported out by the rising air flow and collected by the material collector.

[0089] (7) Transfer the materials in the collector to the material storage, evacuate the barrel to prevent the materials from contacting moisture in the air and frosting, and store the materials in a sealed container after they have returned to temperature.

[0090] Figure 2 This is the SEM image of the powder prepared by the cryogenic method. It can be seen that the cross-section of the powder is brittle fracture;

[0091] Figure 3 The particle size distribution of powder prepared by cryogenic method is relatively concentrated, and 76.8% of the powder particle size is distributed in 40-200 mesh;

[0092] Figure 4 is the XRD result of the ingot, and the unit cell parameters of the ingot alloy are The unit cell volume is

[0093] Figure 5 The XRD results of powders prepared by cryogenic method, the unit cell parameters of the powders are The unit cell volume is The lattice parameters before and after powder making hardly changed, indicating that the alloy did not produce lattice distortion before and after powder making. In addition, the contents of impurity elements C and O in the ingot and powder after powder making were also analyzed. The contents of C and O in the ingot alloy were 52ppm and 125ppm, respectively, and the contents of C and O in the powder alloy prepared by deep cryogenic method were 66ppm and 137ppm, respectively. The content of impurity elements increased slightly. The increase in oxygen content was due to the increase in the specific surface area of ​​the powder after powder making, and the surface was slightly oxidized due to short-term contact with air. The increase in carbon content came from equipment pollution, but the increments of carbon and oxygen content were still within the controllable range of performance and would not affect the performance of the alloy. This proves that the deep cryogenic method of powder making is effective and feasible.

[0094] Figure 6The hydrogen absorption kinetics of powder alloys prepared by ingot casting and cryogenic method were compared. The maximum hydrogen absorption of ingot alloy was 3.611wt% for the first time, and hydrogen absorption saturation was achieved in 5min. The maximum hydrogen absorption of powder alloy was 3.602wt% for the first time, and hydrogen absorption saturation was achieved in 6min. The hydrogen absorption of alloys before and after powdering was similar, and the hydrogen absorption saturation time was slightly delayed, which corresponded to the slight increase in carbon and oxygen content.

[0095] Figure 7 To prepare the hydrogen absorption and desorption cycle performance diagram of the powder alloy, after 50 cycles, the effective hydrogen storage capacity of the powder alloy is 2.205wt%, compared with the hydrogen absorption capacity at the 5th time, the capacity retention rate is 96.5%.

[0096] Example 2

[0097] According to step 1 of Example 1, a ZrCo alloy ingot is refined, and the remaining steps are the same as those of Example 1. The same equipment and conditions are used to conduct a powder making test on the smelted ZrCo alloy to obtain a low-oxygen and low-carbon ZrCo alloy powder with a carbon content of 58 ppm and an oxygen content of 126 ppm, which is not significantly increased compared with the ZrCo alloy ingot, indicating that this powder making method and equipment are generally applicable to alloys with high hardness and toughness.

[0098] Comparative Example 1

[0099] Using V in Example 1 75 Ti5Cr 20 The alloy powder is prepared by lathe turning-cutting powder making method at room temperature. The specific method is: the V 75 Ti5Cr 20 After grinding, the alloy ingot was fixed on an open lathe and turned at a speed of 150r / min to obtain strip-shaped alloy fragments. The collected fragments were then further crushed using a cutting crusher. The particle size, carbon and oxygen content of the obtained fragment powder were analyzed. The results showed that the median particle size of the fragment powder was about 1.5mm, the carbon content was 412ppm, and the oxygen content was 746ppm. The particle size of the obtained alloy powder was large, and the increase in carbon content was mainly due to pollution during the powder making process. The alloy was not protected by an inert atmosphere during the powder making process. The high temperature generated by the turning and cutting process caused the alloy to come into contact with CO2 and O2 in the air, and carburization and oxidation reactions occurred on the surface of the alloy, thereby leading to an increase in the content of impurities carbon and oxygen in the powder, indicating that this powder making method is not suitable for the preparation of ultrafine, low-carbon and low-oxygen alloy powders.

[0100] Comparative Example 2

[0101] In addition, various milling methods were compared, and V was refined by the method of step 1 of Example 1. 75 Ti5Cr 20The impurity carbon and oxygen contents of the alloy ingot before crushing are 52ppm and 125ppm respectively. The impurity carbon and oxygen contents of the alloy powders obtained by different powder making methods are compared: the impurity carbon and oxygen contents of the alloy powders obtained by hydrogenation + mechanical crushing method are 366ppm and 420ppm; the impurity carbon contents of the alloy powders obtained by hydrogenation + ball milling method are 324ppm and 370ppm; the impurity carbon contents of the alloy powders obtained by turning-cutting powder making method under inert atmosphere protection are 512ppm and 525ppm. By comparing different powder making methods, it can be found that the deep-cold-low temperature grinding powder making method under inert gas protection adopted in this patent can obtain high-purity alloy powders, realize a clean powder making process, and almost no impurities are introduced in the powder making process.

Claims

1. A method for preparing a powder of a strong and tough hydrogen storage alloy, comprising the following steps: 1) splitting and pre-treating the ingot of hydrogen storage alloy to obtain alloy blocks; 2) Freeze the alloy block to cool the material to below the hot brittle transition temperature of -60°C; 3) crushing the alloy block frozen in step 2) to obtain a material with a fineness of ≤2 cm; 4) further crushing and grinding the material obtained in step 3) to obtain a material with a fineness of ≤20 mesh; 5) The crushed material is placed under vacuum conditions and heated to room temperature to obtain hydrogen storage alloy powder.

2. The flour making method according to claim 1, wherein: The step 2) has a hot brittle transition temperature of -150°C to -60°C, preferably -90°C; and / or The step 2) uses liquid nitrogen as a cryogenic medium for freezing; and / or The freezing time of step 2) is 5-60 minutes.

3. The flour making method according to claim 1, wherein: The diameter of the alloy block in step 1) is ≤10 cm, preferably ≤9 cm, ≤8 cm, ≤7 cm, ≤6 cm, ≤5 cm; more preferably 2 to 5 cm; and / or The method of segmentation pretreatment in step 1) includes wire cutting and / or mechanical impact; and / or The hydrogen storage alloy is selected from any one or more of the following: x Ti 1-x , V x Cr y Ti z , V x Cr y Ti z Ce m , Zr a Co b , Zr a Ti b Co c , among which, 0.4≤x≤100, 0.2≤y≤0.5, 0.2≤z≤0.5, 0≤m≤0.1, 0.4≤a≤0.6, 0.4≤b≤0.

6.

4. The flour making method according to claim 1, wherein: The step 3) crushing is carried out by any of the following methods: jaw crusher, hammer crusher; and / or The step 4) of preparing the powder is carried out by any of the following methods: a sample preparation pulverizer, a ball mill, a cutting pulverizer, or a Raymond pulverizer; and / or In the Raymond mill, during the pulverizing process, the main engine speed is 10 rpm to 150 rpm, the air temperature is -30°C to 0°C, and the air flow speed is 2 to 100 m / s; and / or The gas used in the Raymond mill is an inert gas; and / or The gas used is selected from any one of the following: argon, nitrogen, and helium.

5. The flour making method according to claim 1, wherein: The vacuum condition of step 5) is P≤0.001MPa; and / or The time of placing the device under vacuum condition in step 5) is 1 to 4 hours, preferably 2 hours or 3 hours.

6. A strong and tough hydrogen storage alloy powder prepared by the powder making method according to any one of claims 1 to 5.

7. A cryogenic-low temperature pulverizing powder making equipment for the powder making method according to any one of claims 1 to 5, comprising a liquid nitrogen cryogenic system, a primary crushing system, a low temperature pulverizing powder making system and a material collection system connected in series in sequence; a) The liquid nitrogen cryogenic system comprises a cryogenic tank (1), which is connected to a liquid nitrogen tank (12) for filling with liquid nitrogen; a cryogenic tank feeding port (11) is provided on the cryogenic tank (1), an inner jacket (14) is arranged inside, and a liquid level sensor (13) is installed; The inner jacket (14) is an irregular cylindrical structure or a funnel-shaped structure; the inner diameter of the feed port end of the inner jacket (14) is greater than the inner diameter of the discharge port end; A spiral conveyor belt (15) is provided at the discharge port of the inner jacket (14) to convey the material to the primary crushing system; The material enters from the feeding port (11) of the cryogenic tank, passes through the upper end and the lower end of the inner jacket (14) in sequence, and is conveyed from the discharge port of the inner jacket (14) to the primary crushing system via a spiral conveyor belt (15); b) the primary crushing system comprises a jaw crusher (2), a jaw crusher feed port (21), and a horizontal conveyor belt (22); the material enters the jaw crusher (2) through the jaw crusher feed port (21), and after the crushing is completed, the material is conveyed to the low-temperature crushing and milling system through the horizontal conveyor belt (22); c) The low-temperature pulverizing and milling system comprises a Raymond mill (3), a Raymond mill feed port (31), a Raymond mill discharge port (32), a shovel (33), a grinding roller device (34), a main shaft (35), an air supply port (36), and a screen plate (37); the material is added into the machine from the Raymond mill feed port (31) of the Raymond mill (3), and the grinding roller device (34) and the shovel (33) are suspended on the plum blossom frame of the main shaft 35 of the Raymond mill 3, and the shovel (33) is located at the suspension grinding roller. The device (34) is vertically below the main body of the Raymond mill (3); an air supply port (36) is arranged on the main body shell of the Raymond mill (3); the discharge port (32) of the Raymond mill is located at the vertical upper part of the Raymond mill (3), and a sieve plate (37) is arranged upstream of the material discharge port (32) of the Raymond mill and near the discharge port (32) of the Raymond mill; during the material grinding process, the fan blows low-temperature inert gas into the main body shell of the Raymond mill (3), blows up the powder, and sorts it through the sieve plate 37 placed above the grinding chamber; d) The material collection system comprises a material collector (4), a material collection feed port (41), a material collection discharge port (42), a material storage (43), an air outlet (44), a vacuum valve (45), a heating sleeve (46), and an agitator (47); the material collection feed port (41) and the air outlet (44) are provided at the vertical upper part of the material collection system (4), and the material collection discharge port (42) is provided at the vertical lower part of the material collection system (4); the material is delivered from the Raymond mill discharge port (32) to the material collection feed port (41), enters the material collector (4), and then enters the material storage (43) through the material collection discharge port (42); the material storage (43) is a closed system, in which a heating sleeve (46) and an agitator (47) are provided, and the pressure of the material storage (43) is adjusted by the vacuum valve (45).