Method for regulating and controlling forming quality of directional energy deposition component through thermal cycle

Through gradient decreasing heat input strategy and reciprocating scanning path planning, the thermal cycle during directional energy deposition is regulated, and the problem of deformation and cracking of materials such as nickel-based alloys during directional energy deposition is solved, forming accuracy and quality are improved, and the formation accuracy and quality are avoided. Increased manufacturing cycle and cost.

CN119016740APending Publication Date: 2024-11-26KUNMING UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411137807.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

During directional energy deposition, high solidification temperature intervals of materials such as nickel-based alloys lead to deformation or cracking, affecting forming accuracy and surface quality, and existing solutions increase manufacturing cycle and cost.

Method used

Through the thermal input strategy of decreasing gradients and reciprocating scanning path planning, the thermal cycle parameters during the deposition process are regulated, the peak temperature and residual stress are reduced, and the inhomogeneity of the heat accumulation area is avoided.

Benefits of technology

It effectively reduces the residual stress and surface roughness of the molded parts, improves the forming accuracy and quality, and avoids the increased manufacturing cycle and cost of the new process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016740A_ABST
    Figure CN119016740A_ABST
Patent Text Reader

Abstract

The invention discloses a method for regulating and controlling the forming quality of a directional energy deposition component through thermal circulation, and belongs to the field of metal additive manufacturing. According to the method, through a gradient decreasing heat input strategy and a unique path planning form, heat cycle parameters such as peak temperature, heating speed, residence time above phase change temperature, cooling speed and the like at different positions of a component in the deposition process are changed, so that a deposition layer is subjected to a remelting-heat cycle process for fewer times; therefore, a temperature interval for forming a hard-brittle phase in the material is ingeniously avoided, formation of the hard-brittle phase is avoided, residual stress and deformation of a component are reduced, the residual stress and deformation are uniformly distributed, the cracking tendency of a deposition layer is reduced, and cracking of the deposition layer is avoided to the maximum extent.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for regulating the forming quality of a directed energy deposition component through a thermal cycle, and belongs to the field of metal additive manufacturing. Background Art

[0002] Metal additive manufacturing technology is an intelligent manufacturing technology that integrates materials, structures, and processes. It has the advantages of no need for molds, short new product development cycle, and no additional cost for manufacturing complex-shaped parts. Depending on the different ways of supplying raw materials, this technology mainly includes powder bed melting technology with powder laying as its technical feature and directed energy deposition technology with synchronous powder or wire feeding as its technical feature. Of these two technologies, directed energy deposition technology is considered to be the preferred metal additive manufacturing technology for forming heterogeneous structures due to its advantages such as higher degrees of freedom and faster deposition efficiency.

[0003] The directed energy deposition process mainly involves rapid melting and rapid solidification of metal materials. The repeated rapid heating and rapid cooling characteristics in this process inevitably cause the deposited layer to have problems such as coarse structure, deformation and even cracking. When nickel-based alloys are used to manufacture blade structures, the alloy elements such as Hf and Zr increase the solidification temperature range of the alloy, which is conducive to the formation of a low-melting-point eutectic phase, which is more prone to deformation or cracking during the directed energy deposition process, causing the molten pool to deviate from the solidified area, resulting in changes in the defocus amount, changing the size of the molten pool, hindering the subsequent deposition process, and significantly increasing the surface roughness of the formed component and reducing the dimensional accuracy of the formed component.

[0004] In response to the above problems, some people have repaired the components through post-processing and other methods; for example, the patent (patent number: 202311376910.5) discloses a method of controlling the epitaxial growth of columnar crystals by adjusting laser process parameters, thereby reducing the proportion of impurity crystals; in addition, the residual stress is reduced on the basis of maintaining the deposited columnar crystal structure through a reasonable heat treatment process; the patent (patent number: 201810385756.0) discloses a method of forming turbine blades by alternating between additive forming and subtractive processing cycles, which solves the problem of low quality of directed energy deposition formed components; the above two schemes are new processes based on existing processes, which undoubtedly increase the manufacturing cycle and production cost of the components.

[0005] The essence of the above problem is that different areas of the deposition layer undergo complex thermal cycles during the directed energy deposition process, and the forming quality of the component is closely related to this thermal cycle that varies with time and space; therefore, the idea of ​​regulating the directed energy deposition thermal cycle by adjusting the heat input strategy and path planning is expected to solve the problems of forming accuracy and surface quality of directed energy deposition components. Summary of the invention

[0006] The present invention provides a method for regulating the forming quality of directed energy deposition components through thermal cycles. Through a gradient-decreasing heat input strategy and a unique path planning form, thermal cycle parameters such as peak temperature, heating rate, residence time above phase change temperature and cooling rate at different positions of the component during the deposition process are changed, thereby regulating the forming quality of the directed energy deposition component, mainly solving the component forming quality problem caused by thermal cycles during the directed energy deposition process.

[0007] The method described in the present invention is specifically as follows: the forming quality of directed energy deposition components is improved through a gradient-decreasing heat input strategy and a reciprocating scanning path planning form; based on a thermal cycle curve, an area with large heat accumulation is determined, and the deposition component is divided into several parts according to the degree of heat accumulation in the area, and the deposition direction is adjusted to reduce the heat input in turn, thereby realizing a gradient-decreasing heat input process strategy.

[0008] Preferably, the region of greater heat accumulation in the present invention refers to: as the number of deposition layers increases, the accumulated temperature of the first mth layer in the accumulation process is T m , the temperature of the nth layer is T n , when T n -T m When the temperature is 200-250°C, the mth layer and the nth layer are divided into one area; when the n+1th layer is deposited, the laser power is reduced by 80-100W.

[0009] Preferably, the method of the present invention specifically comprises the following steps:

[0010] (1) Establish a computational model for the multi-physics field thermal-mechanical coupling of the deposition component: Use a sparse transition method to mesh the entire deposition component, use material performance calculation software to calculate a series of thermal physical parameters required for multi-physics field thermal analysis in the directed energy deposition process (such as specific heat capacity, thermal conductivity, Young's modulus, thermal expansion coefficient, etc.), load them into the computational model, set the path planning form, heat input strategy, and boundary conditions and initial conditions required by the computational model (such as initial conditions, thermal boundary conditions, force boundary conditions, etc.), simulate the layer-by-layer deposition process of the material through the birth-and-death unit method, and use a small step intermittent jump movement method to simulate the movement of the actual heat source;

[0011] (2) Obtaining a thermal cycle curve: Based on the thermal cycle curve, determine the area where the deposition component structure has a large heat accumulation, divide the deposition component into multiple parts, and reduce the heat input from the bottom to the top of the deposition component in the printing direction, so as to achieve a gradient-reduced heat input process strategy;

[0012] (3) Establish a three-dimensional visual digital model of the sedimentary structure;

[0013] (4) Setting heat input parameters and path planning; slicing the designed three-dimensional digital model with the help of slicing software, and then performing path planning, adopting a gradient decreasing heat input strategy from the bottom to the top of the deposition component.

[0014] Preferably, the present invention adopts a reciprocating scanning path planning form, with every two layers being one cycle; Figure 1 As shown in a, A, B, C, D, E, and F are specific positions on the surface of the cylindrical substrate material, respectively, and the path planning form is: the scanning direction of the first layer is A→B→C→D→E→F, and the scanning direction of the second layer is F→E→D→C→B→A, and every two layers are a cycle, and this cycle is repeated; thereby changing the time interval of the temperature peak experienced by the specific position of the deposition component, avoiding the regular repetition of the temperature peak at the specific position of the deposition component, thereby avoiding the generation of large residual stress or even deformation at the specific part of the deposition component.

[0015] Beneficial Effects of the Invention

[0016] (1) The present invention provides a unique method for regulating the thermal cycle of the directed energy deposition process, thereby reducing the residual stress of the formed part and lowering the tendency of the deposited layer to crack. This method breaks through the limitation of the current method of regulating the forming quality of the component by assisting directed energy deposition with new processes (such as ultrasonic vibration, micro-rolling, etc.).

[0017] (2) The gradient decreasing heat input strategy and reciprocating scanning path planning proposed in the present invention fundamentally change the time interval of the peak temperature experienced at different positions, so that the heat exchange in the deposition process can reach a balanced state as much as possible, and the residual stress is smaller and more evenly distributed. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The advantages of the method proposed by the present invention will become clear to those skilled in the art by reading the detailed description of the preferred embodiments below; the accompanying drawings are only used to illustrate the preferred embodiments and are not to be considered as limiting the present application.

[0019] Figure 1 It is the path planning form of the directed energy deposition blade and the blade partition diagram;

[0020] Figure 2 This is a physical picture of a blade formed based on the deposition strategy proposed by the present invention;

[0021] Figure 3 is a flow chart of the method of the present invention. DETAILED DESCRIPTION

[0022] The specific implementation modes of the present invention are further described in detail below in conjunction with the drawings and examples; the following examples are used to illustrate the present invention but are not used to limit the scope of the present invention.

[0023] Example 1

[0024] This embodiment takes a stainless steel blade structure deposited by laser directed energy deposition as an example, and provides a method for regulating the forming quality of a directed energy deposition blade by thermal cycling; the method comprises the following steps:

[0025] (1) Establishment of the multi-physics field calculation model of the forming process: The entire blade is meshed using a sparse transition method. The material performance calculation software is used to calculate a series of thermophysical parameters (including specific heat capacity, thermal conductivity, Young's modulus, thermal expansion coefficient, etc.) required for the multi-physics field in the directed energy deposition process. The parameters are loaded into the calculation model, and the path planning form, heat input strategy, and boundary conditions and initial conditions (including initial conditions, thermal boundary conditions, force boundary conditions, etc.) required by the calculation model are set. The layer-by-layer deposition process of the material is simulated using the birth-and-death unit method, and the movement of the actual heat source is simulated using a small step intermittent jump movement method.

[0026] (2) Obtain thermal cycle curves of the blade structure at the same position at different times and at the same position at different times; and determine the area of ​​the blade structure where greater heat accumulation occurs based on the thermal cycle curves.

[0027] Finally, the entire blade is divided into 3000 layers, each with a thickness of 300μm, and the blade is divided into three parts: upper, middle and lower according to the degree of heat accumulation in the area. Along the deposition direction, the heat input is reduced from the lower part, middle part to the upper part of the blade, thus realizing a gradient-reduced heat input process strategy.

[0028] Specifically: the lower part (the first area, the 1st to 1000th layers), the middle part (the second area, the 1001st to 2000th layers), and the upper part (the third area, the 2001st to 3000th layers), the given laser power decreases successively, which are: 900W, 800W, and 700W, respectively.

[0029] At the bottom of the blade, before deposition, the substrate is at room temperature. During the deposition process, the substrate will produce large residual stress, and a larger heat input parameter is used; when depositing to the middle part, the previous deposition layer has an obvious preheating effect on the subsequent deposition layer, and the subsequent deposition layer has a significant heat treatment effect on the previous deposition layer, which is helpful to release the residual stress of the previous deposition layer, and a smaller heat input parameter is used than the bottom; when depositing to the top, the ability of heat transfer to the substrate becomes worse, and the heat accumulation of the component is serious. In order to avoid the deposition layer undergoing more times of "remelting-thermal cycle", a smaller heat input parameter is used than the middle part.

[0030] (3) Establishing a three-dimensional digital model of the blade: Establishing a three-dimensional digital model of the blade using computer-aided software and exporting it in STL format.

[0031] (4) Model slicing and path planning: Import the STL file into the layered slicing software, slice the digital model, and then perform path planning; Figure 1 The path planning form shown in a;

[0032] (5) Setting of heat input parameters: The given laser power values ​​of 900 W, 800 W, and 700 W correspond to the lower, middle, and upper parts of the blade respectively; Figure 1 As shown in b.

[0033] (6) Setting of other process parameters and selection of materials: 99.99% argon was used as the protective gas, the gas flow rate was 9.0 L / min, and the scanning speed was 30 mm / s; the deposition material was 304L stainless steel powder with a powder particle size between 53 and 150 μm; the substrate was a stainless steel pipe with an outer diameter of 108 mm and a wall thickness of 3 mm.

[0034] (7) Visual verification: Based on the above calculation model, the temperature field, stress field and strain field results are obtained to determine whether the residual stress is low and whether the deformation is uniform; the calculation results assist the deposition process, and the deposition process verifies the calculation results.

[0035] Example 2

[0036] This embodiment takes the arc directed energy deposition nickel-based alloy blade structure as an example, and provides a method for regulating the forming quality of a directed energy deposition blade through a thermal cycle; the method comprises the following steps:

[0037] (1) Establishment of the multi-physics field computational model of the forming process: The three-dimensional model of the entire blade is meshed using a sparse transition method. A series of thermophysical parameters (including specific heat capacity, thermal conductivity, Young's modulus, thermal expansion coefficient, etc.) required for multi-physics field simulation in the directed energy deposition process are calculated with the help of material performance calculation software. The parameters are loaded into the computational model, and the path planning form, heat input strategy, and boundary conditions and initial conditions (including initial conditions, thermal boundary conditions, force boundary conditions, etc.) required by the computational model are set. The layer-by-layer deposition process of the material is simulated using the birth-and-death unit method, and the movement of the actual heat source is simulated using a small step intermittent jump movement method.

[0038] (2) Obtain thermal cycle curves of the blade structure at the same position at different times and at the same position at different times; determine the area of ​​the blade structure with large heat accumulation based on the thermal cycle curve, and divide the blade into three parts: upper, middle and lower parts according to the degree of heat accumulation in the area. Reduce the heat input from the lower part, middle to the upper part of the blade along the printing direction, thereby realizing a gradient-reduced heat input process strategy.

[0039] Finally, the entire blade is divided into 45 layers, each with a thickness of 2 mm, and the blade is divided into three parts: upper, middle and lower according to the degree of heat accumulation in the area. Along the printing direction, the heat input is reduced from the lower part, middle to the upper part of the blade, thus realizing a gradient-reduced heat input process strategy.

[0040] Specifically: the lower part (the first area, the 1st to 15th layers), the middle part (the second area, the 16th to 30th layers), and the upper part (the third area, the 31st to 45th layers), the given deposition current decreases in sequence, 130A, 120A, and 110A.

[0041] (3) Establishing a three-dimensional digital model of the blade: Establishing a three-dimensional digital model of the blade using computer-aided software and exporting it in STL format.

[0042] (4) Model slicing and path planning: Import the STL file into the layered slicing software, slice the digital model, and then perform path planning; Figure 1 The path planning form shown in a. Finally, the entire blade is divided into 45 layers, each with a thickness of 2 mm.

[0043] (5) Setting of heat input parameters: The deposition voltage is fixed at 20 V, and the deposition current is given as 130 A, 120 A, and 110 A, corresponding to the lower, middle, and upper parts of the blade, respectively. Figure 1 As shown in b;

[0044] (6) Setting of other process parameters and selection of materials: 99.99% argon was used as the shielding gas, and the scanning speed was 10 mm / s; the deposition material was Inconel 718 welding wire with a diameter of 1.2 mm, arc was used as the deposition heat source, and the wire feeding speed was 120 IPM; the substrate was a stainless steel pipe with an outer diameter of 108 mm and a wall thickness of 3 mm.

[0045] (7) Visual verification: Based on the above calculation model, the temperature field, stress field and strain field results are obtained to determine whether the residual stress is low and whether the deformation is uniform; the calculation results assist the deposition process, and the deposition process verifies the calculation results.

[0046] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the scope of the ideas and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for regulating the forming quality of a directed energy deposition component by thermal cycling, characterized in that: Improve the forming quality of directed energy deposition components through gradient-decreasing heat input strategy and reciprocating scanning path planning; Based on the thermal cycle curve, the area with large heat accumulation is judged, and the deposition component is divided into several parts according to the degree of heat accumulation in the area. The heat input is reduced successively along the deposition direction to realize the heat input process strategy with gradient reduction.

2. The method for regulating the forming quality of directed energy deposition components by thermal cycling according to claim 1, characterized in that: The area with large heat accumulation refers to the area where the accumulated temperature of the first mth layer in the accumulation process is T as the number of deposition layers increases. m , the temperature of the nth layer after is T n , when T n -T m When the temperature is 200-250°C, the mth layer and the nth layer are divided into one area; when the n+1th layer is deposited, the laser power is reduced by 80-100W.

3. The method for regulating the forming quality of directed energy deposition components by thermal cycling according to claim 1, characterized in that: The specific steps include: (1) Establish a computational model for the multi-physics field thermal-mechanical coupling of the deposition component: Use a sparse transition method to mesh the entire deposition component, use material performance calculation software to calculate a series of thermal physical parameters required for multi-physics field thermal analysis during directed energy deposition, load them into the computational model, set the path planning form, heat input strategy, and the initial and boundary conditions required by the computational model, simulate the layer-by-layer deposition process of the material through the birth-and-death unit method, and use a small step intermittent jump movement method to simulate the movement of the actual heat source; (2) Obtaining a thermal cycle curve: Based on the thermal cycle curve, determine the area where the deposition component structure has a large heat accumulation, divide the deposition component into multiple parts, and reduce the heat input from the bottom to the top of the deposition component in sequence along the deposition direction to achieve a gradient-reduced heat input process strategy; (3) Establish a three-dimensional visual digital model of the sedimentary structure; (4) Setting heat input parameters and path planning; slicing the designed three-dimensional digital model with the help of slicing software, and then performing path planning, adopting a gradient decreasing heat input strategy from the bottom to the top of the deposition component.

4. The method for regulating the forming quality of directed energy deposition components by thermal cycling according to claim 1, characterized in that: A reciprocating scanning path planning form is adopted, with every two layers as a cycle, and this cycle is repeated.

Citation Information

Patent Citations

  • Residual stress control method used in thin-wall special-shaped metal member material additive manufacturing process

    CN111318701A

  • Additive manufacturing component microstructure homogenization regulation and control method for solving heat accumulation effect based on multi-physics field coupling

    CN115186557A

  • Thermal modelling approach for powder bed fusion additive manufacturing

    EP4035802A1

  • Systems and methods for global thermal control of additive manufacturing

    US20190184494A1