Double-tooth claw welding process and device
Through the double-layer surfacing process and electron beam welding technology, the problem of unstable quality of hook claw welding is solved, the wear resistance and welding efficiency of hook claws are improved, the performance of hook claws meets the design requirements, and the service period is extended .
Patent Information
- Application Number
- CN202411293691.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-26
AI Technical Summary
In the existing hook jaw processing technology, the welding quality of the wear-resistant layer and the substrate is unstable, resulting in the actual performance of the hook jaw deviating from the design performance and the welding efficiency is low.
Using the double-layer surfacing process, multi-layer surfacing layers are surfacing through the surfacing platform and mandrel, and the material is removed and processed into a rectangular or cylindrical wear-resistant layer, and welding is carried out by electron beam welding to ensure the wear-resistant layer. Chemical composition consistency with the matrix and welding quality.
It improves the welding quality and efficiency in the hook claw welding process, ensures the wear resistance and impact resistance of the hook claws, extends the service period of the hook claws, and improves the reliability of reactor parts.
Smart Images

Figure CN119016852A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of manufacturing hooks of a stack control rod driving mechanism, and in particular to a double-tooth hook welding process and device. Background Art
[0002] The control rod drive mechanism is used to drive the control rod assembly up and down in the core, thereby achieving important functions such as reactor startup, power regulation and safe shutdown. At present, an important way for the reactor control rod drive mechanism to drive the control rod is the magnetic drive based on the claw. Specifically, the control rod drive mechanism acts on the drive rod through the claw under the action of electromagnetic force, and the interaction between the claw and the drive rod is that the teeth on the claw bite on the teeth of the drive rod. In order to extend the service life of the claw and improve the reliability of the nuclear reactor, an important form of the claw is a double-toothed claw (with two teeth on the claw).
[0003] At the same time, the working environment and stress of the hook during service are complex. In order to ensure the mechanical properties and wear resistance of the hook, a common method in manufacturing is to set a wear-resistant layer on a substrate as the main body of the hook. The substrate can be made of austenitic stainless steel, and the wear-resistant layer can be made of cobalt-based alloy. The wear-resistant layer includes a wear-resistant layer for processing the tooth shape and a wear-resistant layer for processing the center hole. The wear-resistant layer is formed on the substrate by welding, such as using a surfacing process or a vacuum electron beam welding process to complete the connection between the wear-resistant layer and the substrate, and then, a tooth shape of a designed size and a pin hole of a designed size are processed on the corresponding wear-resistant layer. The specific structure of the double-tooth hook is as follows: Figure 1 shown.
[0004] At the same time, in order to reduce the heat introduction in the forming process of the wear-resistant layer on the substrate and improve the welding quality, the existing mainstream wear-resistant layer welding method is: after preparing the corresponding wear-resistant layer by surfacing welding, the wear-resistant layer is welded to the substrate by electron beam welding or high-energy beam welding. The specific technical solution is such as the technical solution provided in the patent application document with patent application number: CN201911326837.4.
[0005] In order to promote the further development of the nuclear power industry and optimize the performance of reactor-related parts, it is necessary to further optimize the claw processing technology. Summary of the invention
[0006] In order to further optimize the hook claw processing technology mentioned above, the present invention provides a double-tooth hook claw welding process and device. This solution can effectively ensure the hook claw welding efficiency and welding quality.
[0007] In view of the above problems, a double-tooth hook claw welding process and device provided by the present invention solves the problems through the following technical points: a double-tooth hook claw welding process, the process includes a first welding process and a second welding process, the first welding process is to weld a first wear-resistant layer for tooth forming on the base of the hook claw, the second welding process is to weld a second wear-resistant layer for pin hole forming on the base of the hook claw, the first wear-resistant layer and the second wear-resistant layer are both connected to the base by electron beam welding, the first wear-resistant layer and the second wear-resistant layer are both formed by surfacing welding, and the surfacing welding forming method of the first wear-resistant layer is: after surfacing welding a third surfacing layer on the welding platform, further surfacing welding a fourth surfacing layer on the outer side of the third surfacing layer, and the thickness of the fourth surfacing layer satisfies: the fourth surfacing layer is used as the base material for processing the first wear-resistant layer; The method for obtaining the first wear-resistant layer is as follows: the fourth weld overlay layer is peeled off by material removal processing, and then the fourth weld overlay layer is processed into a rectangular block-shaped first wear-resistant layer by plastic processing, and in a first welding process, the first wear-resistant layer is embedded and fixed in a notch prefabricated on the substrate, and then the matching surface of the first wear-resistant layer and the substrate is welded by electron beam welding; The surfacing welding forming method of the second wear-resistant layer is: after surfacing the first surfacing layer on the mandrel, further surfacing the second surfacing layer on the outer side of the first surfacing layer, the thickness of the second surfacing layer satisfies: the second surfacing layer is used as the base material for processing the second wear-resistant layer; The method for obtaining the second wear-resistant layer is as follows: the second weld overlay layer is peeled off by material removal processing, and then the second weld overlay layer is processed into a cylindrical second wear-resistant layer by shaping processing; in the second welding process, the second wear-resistant layer is embedded in a prefabricated hole prefabricated on the substrate, and then the second wear-resistant layer and the mating surface of the substrate are welded by electron beam welding.
[0008] The welding process provided by the present invention includes a key step of forming a first wear-resistant layer, a key step of forming a second wear-resistant layer, and a method for welding the first wear-resistant layer and the second wear-resistant layer on a substrate. The key step of forming the first wear-resistant layer is: first, a third surfacing layer thickness is surfacing-welded on a welding platform by surfacing-welding, and then, on the basis of the third surfacing layer, a fourth surfacing layer is further surfacing-welded to obtain a stacked layer on the outer surface of the third surfacing layer. After the surfacing-welding is completed, the surfacing layer is peeled off from the welding platform, and the fourth surfacing layer is peeled off as a base material for processing the first wear-resistant layer by scraping, grinding, and other material removal processing methods. Subsequently, according to the size of the first wear-resistant layer, According to the requirement, the peeled fourth weld overlay layer is processed into the required first wear-resistant layer with a sheet structure; the key step of forming the second wear-resistant layer is: first, after the first weld overlay layer is welded on the outer surface of the core shaft, further welded on the basis of the first weld overlay layer to obtain the second weld overlay layer, the second weld overlay layer is a stacked layer on the outer surface of the first weld overlay layer, after the weld overlay is completed, the core shaft and the first weld overlay layer on the inner side of the second weld overlay layer are removed by drilling, grinding and other material removal processing methods, and the retained second weld overlay layer is used as the base material for processing the second wear-resistant layer, and subsequently, according to the size requirements of the second wear-resistant layer, the retained second weld overlay layer is processed into the required second wear-resistant layer with a cylindrical structure.
[0009] By adopting the above key steps, the following problems can be solved: In the prior art, the first wear-resistant layer is used to form the hook claw, and the second wear-resistant layer provides the hole wall of the pin hole. The first wear-resistant layer and the second wear-resistant layer are usually special metal materials, such as cobalt-based alloys. At the same time, the chemical composition of the first wear-resistant layer has a significant effect on the wear resistance and impact resistance of the hook claw, and the chemical composition of the second wear-resistant layer has a significant effect on the wear resistance and impact resistance of the pin hole. When preparing the first wear-resistant layer and the second wear-resistant layer, the bearing structure (welding platform, core shaft) used to bear the surfacing material is usually made of non-cobalt-based alloy materials, such as austenitic stainless steel. Therefore, during the surfacing process, During the welding process, since the material used for cladding and the load-bearing structure are dissimilar materials with obvious chemical composition differences, especially at the cladding fusion line between the cladding layer and the load-bearing structure, the chemical composition of the cladding layer at this position will be significantly affected by the chemical composition of the load-bearing structure, resulting in the actual chemical composition of the cladding layer being significantly different from the target chemical composition. For example, the load-bearing structure will cause the cladding layer at the fusion line to be chromium-depleted and decarburized, ultimately resulting in the actual cladding layer having obvious material property differences from the designed cladding layer. After the tooth shape and pin holes are machined on such cladding layer, the actual performance of the hook will deviate from the designed performance.
[0010] When implementing the above scheme, the third surfacing layer and the fourth surfacing layer are both made of the same surfacing material, and the first wear-resistant layer and the second wear-resistant layer are both made of the same surfacing material. In the process of implementing the surfacing forming of the first wear-resistant layer and the surfacing forming of the second wear-resistant layer, the third surfacing layer is used as an interlayer between the welding platform and the fourth surfacing layer, and the first surfacing layer is used as an interlayer between the mandrel and the second surfacing layer. From the perspective of the transition of the chemical composition of the heat-affected zone, the influence of the welding platform on the chemical composition of the surfacing layer is mainly concentrated on the third surfacing layer, and the influence of the mandrel on the chemical composition of the surfacing layer is mainly concentrated on the first surfacing layer. In this way, after surfacing the corresponding surfacing layer, According to the welding thickness of the third welding layer, corresponding material removal processing is performed to obtain the base material for processing the first wear-resistant layer. According to the welding thickness of the first welding layer, corresponding material removal processing is performed to obtain the base material for processing the second wear-resistant layer. By utilizing the characteristics of the third welding layer and the fourth welding layer having similar chemical compositions and the characteristics of the first welding layer and the second welding layer having similar chemical compositions, the retained fourth welding layer and the second welding layer have chemical compositions that are consistent with or very close to the designed first wear-resistant layer and the second wear-resistant layer. Therefore, this scheme achieves the purpose of ensuring the welding quality in the double-tooth hook claw welding process by improving the stability of the chemical compositions of the first wear-resistant layer and the second wear-resistant layer.
[0011] In addition, unlike the prior art in which the cladding layer is finally completed by cladding one point at a time, in the process of forming the first wear-resistant layer and the second wear-resistant layer, it is only necessary to first clad the inner cladding layer (the third cladding layer and the first cladding layer) and then further clad the outer cladding layer (the fourth cladding layer and the second cladding layer) on the basis of the inner cladding layer. Therefore, in terms of welding efficiency, this solution will not lead to a decrease in cladding efficiency and prolong the heat impact time of the material during welding.
[0012] Furthermore, on the basis of obtaining the first wear-resistant layer and the second wear-resistant layer of reliable quality, regarding the method of welding the first wear-resistant layer and the second wear-resistant layer on the substrate, electron beam welding is a welding method that is suitable for curved weld welding, has less heat introduction, a large welding depth-to-width ratio, and high welding efficiency. Compared with other welding methods, this welding method only has advantages in terms of welding efficiency, welding quality, stability of material performance after welding, and thermal deformation of material after welding of the first wear-resistant layer and the second wear-resistant layer.
[0013] As a further technical solution of the double-tooth hook welding process: In order to improve the efficiency of the first welding process and the second welding process, it is set as follows: the notch forms a step located at the end of the substrate, the bottom surface and the side surface of the step are both planes, and after the first wear-resistant layer is embedded in the notch, the bottom surface of the first wear-resistant layer and the bottom surface of the step have a surface-fitting relationship, and the side surface of the first wear-resistant layer and the side surface of the step have a surface-fitting relationship; The axial direction of the prefabricated hole is located in the width direction of the substrate, and the notch intersects with both ends of the substrate in the width direction. In this solution, the notch intersects with the end face of the substrate with the pin hole opening, and is set to be a plane with the bottom face and side faces of the step, so that when welding the first wear-resistant layer and the second wear-resistant layer, the electron beam can be introduced from the same end face of the substrate (the end face with the pin hole opening), and the first wear-resistant layer welding and the second wear-resistant layer welding can be completed sequentially without changing the fixed posture of the substrate, thereby helping the efficiency of the welding process.
[0014] In order to ensure the matching accuracy between the second wear-resistant layer and the prefabricated hole during the second welding process and to ensure the connection quality between the second wear-resistant layer and the substrate, it is set as follows: the outer diameter of the second wear-resistant layer is equal to the hole diameter of the prefabricated hole.
[0015] In order to reduce the influence of heat introduction on the internal stress of the welded materials, the influence on thermal deformation, the oxidation and burning of metal elements during the implementation of the first welding process and the second welding process, the substrate and the first wear-resistant layer are preheated before the first welding process. The preheating is carried out in a vacuum box. Before preheating, the vacuum box is evacuated. After the preheating is completed, the vacuum box is evacuated again. Before the second welding process is implemented, the substrate and the second wear-resistant layer are preheated in a vacuum box. Before preheating, the vacuum box is evacuated. After preheating, the vacuum box is evacuated again. In this solution, preheating after evacuating the vacuum box can protect the parts to be welded. After preheating, evacuating again can obtain more ideal vacuum conditions and allow more gas in the gap between the first wear-resistant layer and the substrate and gas in the gap between the second wear-resistant layer and the substrate to escape into the vacuum box.
[0016] As a method for ensuring the efficiency of electron beam welding preparation, it is set as follows: after the assembly formed by assembling the first wear-resistant layer, the substrate, and the second wear-resistant layer is placed in a vacuum box, the vacuum box is evacuated, and then the assembly is preheated, and after preheating, the vacuum box is evacuated again, and then the first welding process and the second welding process are performed in the vacuum box by electron beam welding. In this scheme, the preheating process and the vacuuming process before the first welding process and the second welding process are performed simultaneously, which can effectively shorten the preparation time for electron beam welding.
[0017] In order to enable the corresponding surfacing to be carried out in a stable and controllable surfacing environment, the surfacing of the first wear-resistant layer and the second wear-resistant layer is completed in a surfacing box; For the surfacing welding of the first wear-resistant layer, the third surfacing layer can be obtained by surfacing welding at various positions of the surfacing area along the planned surfacing welding track on a flat welding platform, and then on the basis of the third surfacing layer, the fourth surfacing layer can be obtained by surfacing welding at various positions outside the third surfacing layer along the planned surfacing welding track. Since the surfacing welding forming process of the first wear-resistant layer can be to adjust the surfacing position according to the surfacing welding track on the plane, it is relatively easy and efficient to obtain an ideal surfacing layer; The surfacing box used for surfacing welding of the second wear-resistant layer comprises: a surfacing box body, a surfacing operation port is provided on the top surface or the side surface of the surfacing box body, a first connecting seat and a second connecting seat are arranged in the surfacing box body in a vertically opposite relationship, one of the first connecting seat and the second connecting seat is connected to the surfacing box body through a rotating motor, and the other is connected to the surfacing box body through a bearing seat; As for the shape requirement of the second wear-resistant layer, in order to conveniently and efficiently obtain the second wear-resistant layer, it is set as follows: when implementing the second wear-resistant layer surfacing welding forming, the two ends of the mandrel are respectively clamped on the first connecting seat and the second connecting seat, and the mandrel rotates around its own axis under the action of the rotating motor. When surfacing the first surfacing layer, surfacing is performed through the surfacing operation port, and a cylindrical first surfacing layer is surfacing on the side of the mandrel from bottom to top along the axial direction of the mandrel. For surfacing points at any axial position of the mandrel, surfacing is performed at a fixed position, and an annular surfacing layer is obtained during the rotation of the mandrel. When surfacing the second weld layer, surfacing is performed through the surfacing operation port, and a cylindrical second surfacing layer is surfacing on the side of the first surfacing layer from bottom to top along the axial direction of the core shaft. For surfacing points at any position of the core shaft axis, surfacing is performed at a fixed position, and an annular surfacing layer is obtained during the rotation of the core shaft. In this scheme, the first connecting seat and the second connecting seat are respectively used to fix the ends of the core shaft to fix the core shaft as a vertical rod, and under the action of the rotating motor and the bearing seat, the core shaft can rotate coaxially with the rotating motor. When the core shaft rotates, surfacing on the core shaft is performed through the surfacing operation port. For surfacing at any position of the core shaft axis, an annular surfacing layer can be obtained during the rotation of the core shaft, and then the first surfacing layer is surfacing on the corresponding section of the core shaft from bottom to top, and then, on the basis of the first surfacing layer, the second surfacing layer is obtained in the same way as the first surfacing layer. In this scheme, whether it is for the first weld layer or the second weld layer, when performing the weld on a certain core shaft axial position, since the weld is performed from bottom to top and during the rotation of the core shaft, the operator only needs to select the weld implementation position located at a suitable radial position of the core shaft and select the weld angle, other weld parameters, etc. As the core shaft rotates, the weld can be performed on each circumferential position under the axial position. When a weld layer has been formed below the axial position, the weld layer can be extended upward in sequence on the basis of the lower weld layer. By using this scheme to weld the second wear-resistant layer, the weld quality is easy to control, the weld efficiency is high, and it is easy to make each weld point have consistent weld quality.
[0018] In order to further ensure the quality of the second wear-resistant layer surfacing and the efficiency of the second wear-resistant layer surfacing, it is set as follows: an annular bearing plate is arranged on the core shaft, the core shaft passes through the bearing plate, and the surfacing starting positions of the first surfacing layer and the second surfacing layer both start from the upper end surface of the bearing plate; in this scheme, whether it is to obtain the first wear-resistant layer or the second wear-resistant layer, the core shaft surface and the first wear-resistant layer are respectively used as the attachment body of the surfacing molten material, and the bearing plate is used as the support body of the surfacing molten material at the lowest end position, and the bearing plate is used to prevent the molten material from falling at the starting moment of the surfacing of the first surfacing layer and the second surfacing layer, and the subsequent surfacing process uses the surfacing layer formed below to prevent the molten material from falling, so that the entire surfacing process can be easily controlled.
[0019] In order to make the cladding process have a good gas phase environment, during the cladding forming process of the first wear-resistant layer and the second wear-resistant layer, protective gas is injected into the cladding box through the air intake hood installed on the cladding box, and the gas in the cladding box is sucked through the air suction hood installed on the cladding box. In this scheme, the air intake hood and the air suction hood are preferably arranged on different sides of a pair of opposite sides of the cladding box, and the air intake hood is located below the air suction hood, so that there is gas convection between the air intake hood and the air suction hood. Such convection can not only provide anti-oxidation protection for the high-temperature cladding layer, but also help improve the cladding personnel to observe the cladding position.
[0020] The present solution also provides a welding device for implementing any of the above double-tooth hook claw welding processes, including a clamp for fixing the relative position of the first wear-resistant layer and the substrate, the clamp including a clamp in the shape of a channel steel, at least one of the two side plates of the clamp having a locking bolt threadedly connected thereto, the locking bolt being connected to an internal threaded hole of the side plate, the internal threaded hole being a through hole, and the end of the locking bolt being embeddable into the inner space of the clamp; A first oblique wedge groove is provided on the inner side of the horizontal plate of the clamp, the notch of the first oblique wedge groove is located on the side of the horizontal plate, and the width of the inner side of the first oblique wedge groove is smaller than the width of the outer side; A second oblique wedge groove is provided on the inner side of one of the side plates, the notch of the second oblique wedge groove is located on the side surface of the side plate, and the width of the inner side of the second oblique wedge groove is smaller than the width of the outer side; The first inclined wedge groove and the second inclined wedge groove are located on the same side of the clamp; The structural characteristics of the clamp satisfy the following requirements: after the assembly of the first wear-resistant layer and the base is embedded in the inner space, the assembly can be adjusted so that the outer surface of the first wear-resistant layer faces the first inclined wedge groove, and the side of the first wear-resistant layer close to the end of the base faces the second inclined wedge groove.
[0021] In summary, the implementation of this welding process depends on the cladding equipment and the electron beam welding equipment. During the implementation of electron beam welding, the prefabricated hole on the substrate for preparing the pin hole can be used to constrain the second wear-resistant layer, so as to ensure the matching accuracy between the second wear-resistant layer and the prefabricated hole to achieve the purpose of ensuring the welding quality of the second wear-resistant layer and the substrate. However, for the first wear-resistant layer, since it needs to be welded on the surface of the end of the substrate, specifically, it is welded to the bottom and side surfaces of the notch. In order to ensure the welding quality of the first wear-resistant layer when implementing the first welding process, it is necessary to constrain the relative position of the first wear-resistant layer and the substrate before welding. The fixture provided above is used to solve the corresponding fixing problem, specifically: The horizontal plate of the clamp and the two side plates form a channel steel structure. After the first wear-resistant layer is embedded in the notch, the locking bolt is used to clamp the base in the inner space. For the cooperation between the bottom surface of the first wear-resistant layer and the bottom surface of the notch, in order to obtain a state of always being in contact with each other, an inclined wedge can be inserted into the first inclined wedge groove to push the first wear-resistant layer so that the bottom surface is always in contact with the bottom surface of the notch. For the cooperation between the side surface of the first wear-resistant layer and the side surface of the notch, in order to obtain a state of always being in contact with each other, an inclined wedge can be inserted into the second inclined wedge groove to push the first wear-resistant layer deep into the notch to always be in contact with the side surface of the notch. The locking bolt is provided to enable the clamp to provide clamping function for substrates within a certain length range. The idea of this solution is that after clamping is completed, the bevel wedge block in the first bevel wedge groove is used to provide thrust to the first wear-resistant layer along the thickness direction of the first wear-resistant layer, and the bevel wedge block in the second bevel wedge groove is used to provide thrust to the first wear-resistant layer along the length direction of the substrate, so as to keep the corresponding two mating surfaces in full fit, thereby preparing for high-quality electron beam welding of the two mating surfaces.
[0022] As a further technical solution of the welding device: When the substrate, the first wear-resistant ring and the second wear-resistant ring are preheated before electron beam welding, the clamp needs to be heated together with the above parts. In order to make the corner on the side of the clamp away from the first wear-resistant layer adapt to the thermal deformation of the clamp and ensure the reliability of the clamp in fixing the relevant relative position, it is set as follows: locking bolts are installed on both side plates of the clamp, and the corner away from the first inclined wedge groove is an arc-shaped corner. This solution can fix the substrate by the locking bolts on each side plate; after clamping the corresponding parts, according to the configuration of the hook claw, the horizontal plate at the position of the arc-shaped corner has a large gap with the substrate, so that the arc-shaped corner can release thermal stress of the clamp through deformation.
[0023] In order to shorten the assembly time of the base on the clamp, the better application is: the spacing of the side plates is equal to the length of the base, and when the clamp is deformed, the locking bolt is used to maintain the reliability of the clamp clamping the base.
[0024] When welding the bottom surface of the first wear-resistant layer and the bottom surface of the notch, in order to prevent the electron beam welding position from affecting the clamp, it is set as follows: the inner side of the side plate where the second inclined wedge groove is set is also provided with an avoidance groove, the avoidance groove is located on the side of the second inclined wedge groove away from the cross plate, and the position of the avoidance groove satisfies: when the assembly is embedded in the inner space and the top surface of the first wear-resistant layer is supported by the cross plate, the avoidance groove forms a cavity between the side plate and the assembly, and the bottom surface of the notch is located in the middle of the cavity. By adopting this solution, the space provided by the avoidance groove can be used so that the welding position of the first wear-resistant layer on the substrate can involve the end of the substrate, and will not cause the corresponding parts to stick to the clamp.
[0025] The present invention has the following beneficial effects: In this scheme, the third weld overlay layer and the fourth weld overlay layer have similar chemical compositions, as well as the first weld overlay layer and the second weld overlay layer have similar chemical compositions, so that the retained fourth weld overlay layer and the second weld overlay layer have chemical compositions that are consistent with or very close to the designed first wear-resistant layer and the second wear-resistant layer. Therefore, this scheme achieves the purpose of ensuring the welding quality in the double-tooth hook claw welding process by improving the stability of the chemical compositions of the first wear-resistant layer and the second wear-resistant layer.
[0026] In this solution, during the process of forming the first wear-resistant layer and the second wear-resistant layer, it is only necessary to first build up the inner buildup layer and then further build up the outer buildup layer on the basis of the inner buildup layer. Therefore, in terms of welding efficiency, this solution will not lead to a decrease in buildup efficiency and prolong the heat impact time of the material during the welding process. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is a structural schematic diagram of a specific embodiment of a double-tooth hook claw in the prior art, in which the tooth shape and the pin hole have been formed; Figure 2 A structural schematic diagram showing the coordination between the fixture, the substrate and the first wear-resistant layer; Figure 3 An exploded view showing the matching relationship between the first wear-resistant layer, the second wear-resistant layer and the substrate; Figure 4 It is a structural diagram showing the matching state between the cladding box and the mandrel; Figure 5 It is a schematic diagram of the structure after obtaining the first cladding layer on the mandrel; Figure 6 It is a schematic diagram of the structure after obtaining the second cladding layer on the mandrel; Figure 7 It is a schematic diagram of the structure after the third cladding layer is obtained on the welding platform; Figure 8 This is a schematic diagram of the structure after the fourth weld layer is obtained on the welding platform.
[0028] The reference numerals in the figure are respectively: 1, first wear-resistant layer, 2, second wear-resistant layer, 3, substrate, 4, pin hole, 5, clamp, 6, locking bolt, 7, first oblique wedge groove, 8, avoidance groove, 9, second oblique wedge groove, 10, notch, 11, rotating motor, 12, first connecting seat, 13, bearing plate, 14, core shaft, 15, second connecting seat, 16, bearing seat, 17, air intake hood, 18, air suction hood, 19, first surfacing layer, 20, second surfacing layer, 21, prefabricated hole, 22, welding platform, 23, third surfacing layer, 24, fourth surfacing layer. DETAILED DESCRIPTION
[0029] The present invention is further described in detail below in conjunction with embodiments, but the present invention is not limited to the following embodiments: Embodiment 1: like Figures 1 to 8 As shown, a double-tooth hook claw welding process includes a first welding process and a second welding process. The first welding process is to weld a first wear-resistant layer 1 for tooth forming on a base 3 of the hook claw, and the second welding process is to weld a second wear-resistant layer 2 for pin hole 4 forming on the base 3 of the hook claw. The first wear-resistant layer 1 and the second wear-resistant layer 2 are both connected to the base 3 by electron beam welding. The first wear-resistant layer 1 and the second wear-resistant layer 2 are both formed by surfacing welding. The surfacing welding forming method of the first wear-resistant layer 1 is as follows: after surfacing welding a third surfacing layer 23 on a welding platform 22, further surfacing welding a fourth surfacing layer 24 on the outer side of the third surfacing layer 23, and the thickness of the fourth surfacing layer 24 satisfies: the fourth surfacing layer 24 is used as a base material for processing the first wear-resistant layer 1; The first wear-resistant layer 1 is obtained by: peeling off the fourth cladding layer 24 by material removal processing, and then processing the fourth cladding layer 24 into a rectangular block-shaped first wear-resistant layer 1 by plastic processing, in the first welding process, the first wear-resistant layer 1 is embedded and fixed in the notch 10 prefabricated on the substrate 3, and then the first wear-resistant layer 1 and the substrate 3 are welded by electron beam welding. The surfacing forming method of the second wear-resistant layer 2 is as follows: after surfacing a first surfacing layer 19 on the mandrel 14, further surfacing a second surfacing layer 20 on the outer side of the first surfacing layer 19, the thickness of the second surfacing layer 20 satisfies: the second surfacing layer 20 is used as a base material for processing the second wear-resistant layer 2; The method for obtaining the second wear-resistant layer 2 is as follows: the second weld overlay layer 20 is peeled off by material removal processing, and then the second weld overlay layer 20 is processed into a cylindrical second wear-resistant layer 2 by shaping processing. In the second welding process, the second wear-resistant layer 2 is embedded in the prefabricated hole 21 prefabricated on the substrate 3, and then the second wear-resistant layer 2 and the mating surface of the substrate 3 are welded by electron beam welding.
[0030] The welding process provided in this scheme includes the key steps of forming the first wear-resistant layer 1, the key steps of forming the second wear-resistant layer 2, and the method of welding the first wear-resistant layer 1 and the second wear-resistant layer 2 on the substrate 3. The key step of forming the first wear-resistant layer 1 is: firstly, a third surfacing layer 23 is surfacing-welded on the welding platform 22 by surfacing welding, and then, on the basis of the third surfacing layer 23, a fourth surfacing layer 24 is further surfacing-welded to obtain the fourth surfacing layer 24, wherein the fourth surfacing layer 24 is a stacked layer on the outer surface of the third surfacing layer 23. After the surfacing welding is completed, the surfacing layer is peeled off from the welding platform 22, and the fourth surfacing layer 24 is peeled off as the base material for processing the first wear-resistant layer 1 by scraping, grinding and other material removal processing methods. Subsequently, according to the size requirements of the first wear-resistant layer 1, The peeled fourth weld overlay layer 24 is processed into the required first wear-resistant layer 1 with a sheet structure; the key step of forming the second wear-resistant layer is: first, after the first weld overlay layer 19 is overlaid on the outer surface of the core shaft 14, the second weld overlay layer 20 is further overlaid on the basis of the first weld overlay layer 19. The second weld overlay layer 20 is a stacked layer on the outer surface of the first weld overlay layer 19. After the overlay is completed, the core shaft 14 and the first weld overlay layer 19 on the inner side of the second weld overlay layer 20 are removed by drilling, grinding and other material removal processing methods, and the retained second weld overlay layer 20 is used as the base material for processing the second wear-resistant layer 2. Subsequently, according to the size requirements of the second wear-resistant layer 2, the retained second weld overlay layer 20 is processed into the required second wear-resistant layer 2 with a cylindrical structure.
[0031] By adopting the above key steps, the following problems can be solved: In the prior art, the first wear-resistant layer 1 is used to form the hook claw, and the second wear-resistant layer 2 provides the hole wall of the pin hole 4. The first wear-resistant layer 1 and the second wear-resistant layer 2 are usually special metal materials, such as cobalt-based alloys. At the same time, the chemical composition of the first wear-resistant layer 1 has a significant effect on the wear resistance and impact resistance of the hook claw, and the chemical composition of the second wear-resistant layer 2 has a significant effect on the wear resistance and impact resistance of the pin hole 4. When preparing the first wear-resistant layer 1 and the second wear-resistant layer 2, the bearing structure (welding platform, core shaft 14) used to bear the cladding material is usually made of non-cobalt-based alloy materials, such as austenitic stainless steel. Therefore, during the surfacing process, since the material used for surfacing and the load-bearing structure are dissimilar materials with obvious chemical composition differences, especially at the surfacing fusion line between the surfacing layer and the load-bearing structure, the chemical composition of the surfacing layer at this position will be significantly affected by the chemical composition of the load-bearing structure, resulting in the actual chemical composition of the surfacing layer being significantly different from the target chemical composition. For example, the load-bearing structure will cause the surfacing layer at the fusion line to be chromium-poor and decarburized, ultimately resulting in the actual surfacing layer having obvious material property differences from the designed surfacing layer. After the tooth shape and the pin hole 4 are machined on such a surfacing layer, the actual performance of the hook will deviate from the designed performance.
[0032] When implementing the above scheme, the third surfacing layer 23 and the fourth surfacing layer 24 are both made of the same surfacing material, and the first wear-resistant layer 1 and the second wear-resistant layer 2 are both made of the same surfacing material. In the process of surfacing the first wear-resistant layer 1 and the second wear-resistant layer 2, the third surfacing layer 23 is used as a partition between the welding platform 22 and the fourth surfacing layer 24, and the first surfacing layer 19 is used as a partition between the mandrel 14 and the second surfacing layer 20. From the perspective of the transition of the chemical composition of the heat-affected zone, the influence of the welding platform 22 on the chemical composition of the surfacing layer thereon is mainly concentrated on the third surfacing layer 23, and the influence of the mandrel 14 on the chemical composition of the surfacing layer thereon is mainly concentrated on the first surfacing layer 19. In this way, when the corresponding surfacing is formed, After the layers are formed, the corresponding material removal processing is performed according to the cladding thickness of the third cladding layer 23 to obtain the base material for processing the first wear-resistant layer 1, and the corresponding material removal processing is performed according to the welding thickness of the first cladding layer 19 to obtain the base material for processing the second wear-resistant layer 2. By utilizing the characteristics that the third cladding layer 23 and the fourth cladding layer 24 are close in chemical composition and the characteristics that the first cladding layer 19 and the second cladding layer 20 are close in chemical composition, the retained fourth cladding layer 24 and the second cladding layer 20 have a chemical composition composition that is consistent with or very close to the designed first wear-resistant layer 1 and the second wear-resistant layer 2. Therefore, this scheme achieves the purpose of ensuring the welding quality in the double-tooth hook claw welding process by improving the stability of the chemical composition of the first wear-resistant layer 1 and the second wear-resistant layer 2.
[0033] In addition, unlike the prior art in which the cladding layer is finally obtained by cladding one point at a time, in the process of forming the first wear-resistant layer 1 and the second wear-resistant layer 2, it is only necessary to first clad the inner cladding layer (the third cladding layer 23 and the first cladding layer 19) and then further clad the outer cladding layer (the fourth cladding layer 24 and the second cladding layer 20) on the basis of the inner cladding layer. Therefore, in terms of welding efficiency, this solution will not lead to a decrease in cladding efficiency and prolong the heat impact time of the material during welding.
[0034] Furthermore, on the basis of obtaining the first wear-resistant layer 1 and the second wear-resistant layer 2 of reliable quality, regarding the method of welding the first wear-resistant layer 1 and the second wear-resistant layer 2 on the substrate 3, electron beam welding is a welding method that is suitable for curved weld welding, has less heat introduction, a large welding depth-to-width ratio, and high welding efficiency. Compared with other welding methods, this welding method only has advantages in terms of welding efficiency, welding quality, post-welding material performance stability, and post-welding material thermal deformation of the first wear-resistant layer 1 and the second wear-resistant layer 2.
[0035] Embodiment 2: This embodiment is further refined on the basis of embodiment 1: In order to improve the efficiency of the first welding process and the second welding process, it is set as follows: the notch 10 forms a step located at the end of the substrate 3, the bottom surface and the side surface of the step are both planes, and after the first wear-resistant layer 1 is embedded in the notch 10, the bottom surface of the first wear-resistant layer 1 has a surface-fitting relationship with the bottom surface of the step, and the side surface of the first wear-resistant layer 1 has a surface-fitting relationship with the side surface of the step; The axial direction of the prefabricated hole 21 is located in the width direction of the substrate 3, and the notch 10 intersects with both ends of the width direction of the substrate 3. In this solution, the notch 10 intersects with the end face of the substrate 3 having the pin hole 4 opening, and is set to be a plane on the bottom face and side face of the step, so that when welding the first wear-resistant layer 1 and the second wear-resistant layer 2, the electron beam can be introduced from the same end face of the substrate 3 (the end face having the pin hole 4 opening), and the welding of the first wear-resistant layer 1 and the second wear-resistant layer 2 can be completed sequentially without changing the fixed posture of the substrate 3, thereby helping the efficiency of the welding process.
[0036] Embodiment 3: This embodiment is further refined on the basis of embodiment 1: In order to ensure the matching accuracy between the second wear-resistant layer 2 and the prefabricated hole 21 during the second welding process and to ensure the connection quality between the second wear-resistant layer 2 and the substrate 3 , it is set as follows: the outer diameter of the second wear-resistant layer 2 is equal to the aperture of the prefabricated hole 21 .
[0037] Embodiment 4: This embodiment is further refined on the basis of embodiment 1: In order to reduce the influence of heat introduction on the internal stress of the welded materials, the influence on thermal deformation, the influence on oxidation and burning of metal elements during the implementation of the first welding process and the second welding process, the substrate 3 and the first wear-resistant layer 1 are preheated before the first welding process is implemented. The preheating is carried out in a vacuum box. Before preheating, the vacuum box is evacuated. After preheating, the vacuum box is evacuated again. Before the second welding process is implemented, the substrate 3 and the second wear-resistant layer 2 are preheated. The preheating is performed in a vacuum box. Before preheating, the vacuum box is evacuated. After preheating, the vacuum box is evacuated again. In this solution, preheating after evacuating the vacuum box can protect the parts to be welded. After preheating, evacuating again can obtain more ideal vacuum conditions and allow more gas in the gap between the first wear-resistant layer 1 and the substrate 3 and gas in the gap between the second wear-resistant layer 2 and the substrate 3 to escape into the vacuum box.
[0038] Embodiment 5: This embodiment is further refined on the basis of Embodiment 4: As a method for ensuring the efficiency of electron beam welding preparation, it is set as follows: after the assembly formed by assembling the first wear-resistant layer 1, the substrate 3, and the second wear-resistant layer 2 is placed in a vacuum box, the vacuum box is evacuated, and then the assembly is preheated, and after preheating, the vacuum box is evacuated again, and then the first welding process and the second welding process are implemented in the vacuum box by electron beam welding. In this scheme, the preheating process and the vacuuming process before the implementation of the first welding process and the second welding process are carried out simultaneously, which can effectively shorten the preparation time for electron beam welding.
[0039] Embodiment 6: This embodiment is further refined on the basis of embodiment 1: In order to enable the corresponding surfacing to be carried out in a stable and controllable surfacing environment, the surfacing of the first wear-resistant layer 1 and the second wear-resistant layer 2 is completed in a surfacing box; For the surfacing welding of the first wear-resistant layer 1, the third surfacing layer 23 can be obtained by surfacing welding at various positions of the surfacing area along the planned surfacing welding track on the flat welding platform 22, and then on the basis of the third surfacing layer 23, the fourth surfacing layer 24 can be obtained by surfacing welding at various positions outside the third surfacing layer 23 along the planned surfacing welding track. Since the surfacing welding forming process of the first wear-resistant layer 1 can be to adjust the surfacing position according to the surfacing welding track on the plane, it is relatively easy and efficient to obtain an ideal surfacing layer; The surfacing box used for surfacing the second wear-resistant layer 2 comprises: a surfacing box body, a surfacing operation port is provided on the top surface or the side surface of the surfacing box body, a first connecting seat 12 and a second connecting seat 15 are arranged in the surfacing box body in a vertically opposite relationship, one of the first connecting seat 12 and the second connecting seat 15 is connected to the surfacing box body through a rotating motor 11, and the other is connected to the surfacing box body through a bearing seat 16; As for the shape requirement of the second wear-resistant layer 2, in order to conveniently and efficiently obtain the second wear-resistant layer 2, it is set as follows: when the second wear-resistant layer 2 is surfacing and forming, the two ends of the core shaft 14 are respectively clamped on the first connecting seat 12 and the second connecting seat 15, and the core shaft 14 rotates around its own axis under the action of the rotating motor 11. When surfacing the first surfacing layer 19, surfacing is performed through the surfacing operation port, and a cylindrical first surfacing layer 19 is surfacing on the side of the core shaft 14 from bottom to top along the axial direction of the core shaft 14. For any surfacing point at the axial position of the core shaft 14, surfacing is performed at a fixed position, and an annular surfacing layer is obtained during the rotation of the core shaft 14. When surfacing the second welding layer 20, surfacing is carried out through the surfacing operation port, and a cylindrical second welding layer 20 is surfacing on the side of the first welding layer 19 from bottom to top along the axial direction of the core shaft 14. For any surfacing point at the axial position of the core shaft 14, surfacing is carried out at a fixed position, and an annular surfacing layer is obtained during the rotation of the core shaft 14. In the present solution, the first connecting seat 12 and the second connecting seat 15 are respectively used to fix the ends of the core shaft 14 to fix the core shaft 14 as a vertical rod, and under the action of the rotating motor 11 and the bearing seat 16, the core shaft 14 can rotate coaxially with the rotating motor 11. When the core shaft 14 rotates, the cladding operation port is used to implement the cladding on the core shaft 14. For the cladding at any axial position of the core shaft 14, an annular cladding layer can be obtained during the rotation of the core shaft 14, and then the first cladding layer 19 is clad in the corresponding sections on the core shaft 14 from bottom to top, and then, on the basis of the first cladding layer 19, the second cladding layer 20 is obtained in the same way as the first cladding layer 19 is obtained. In this scheme, whether it is for the first weld layer 19 or the second weld layer 20, when the weld is performed at a certain axial position of the core shaft 14, since the weld is performed from bottom to top and during the rotation of the core shaft 14, the operator only needs to select a good weld implementation position at a suitable radial position of the core shaft 14 and select a good weld angle, other weld parameters, etc. As the core shaft 14 rotates, the weld can be performed at each circumferential position under the axial position. When a weld layer has been formed below the axial position, the weld layer can be extended upward in sequence on the basis of the lower weld layer. By using this scheme to weld the second wear-resistant layer 2, the weld quality is easy to control, the weld efficiency is high, and it is easy to make each weld point have consistent weld quality.
[0040] Embodiment 7: This embodiment is further refined on the basis of Embodiment 6: In order to further ensure the quality of the surfacing forming of the second wear-resistant layer 2 and to ensure the surfacing forming efficiency of the second wear-resistant layer 2, it is configured as follows: an annular bearing plate 13 is arranged on the core shaft 14, the core shaft 14 passes through the bearing plate 13, and the surfacing starting positions of the first surfacing layer 19 and the second surfacing layer 20 both start from the upper end surface of the bearing plate 13; in this scheme, whether it is to obtain the first wear-resistant layer 1 or the second wear-resistant layer 2, the surface of the core shaft 14 and the first wear-resistant layer 1 are respectively used as the attachment bodies of the surfacing molten material, and the bearing plate 13 is used as the support body of the surfacing molten material at the lowest position, and the surfacing starting moments of the first surfacing layer 19 and the second surfacing layer 20 use the bearing plate 13 to prevent the molten material from falling, and the subsequent surfacing process uses the surfacing layer already formed below to prevent the molten material from falling, so that the entire surfacing process can be easily controlled.
[0041] In order to make the surfacing process have a good gas phase environment, in the process of surfacing the first wear-resistant layer 1 and the second wear-resistant layer 2, protective gas is injected into the surfacing box through the air intake hood 17 installed on the surfacing box, and the gas in the surfacing box is sucked through the air suction hood 18 installed on the surfacing box. In this scheme, the air intake hood 17 and the air suction hood 18 are preferably arranged on different sides of a pair of opposite sides of the surfacing box, and the air intake hood 17 is located below the air suction hood 18, so that there is gas convection between the air intake hood 17 and the air suction hood 18. Such convection can not only provide anti-oxidation protection for the high-temperature surfacing layer, but also help improve the surfacing personnel to observe the surfacing position.
[0042] Embodiment 8: The present embodiment provides a welding device for implementing the double-tooth hook claw welding process described in Example 1, comprising a fixture for fixing the relative position of the first wear-resistant layer 1 and the substrate 3, the fixture comprising a clamp 5 in the shape of a channel steel, at least one of the two side plates of the clamp 5 is threadedly connected with a locking bolt 6, the locking bolt 6 is connected to the internal threaded hole of the side plate, the internal threaded hole is a through hole, and the end of the locking bolt 6 can be embedded in the inner space of the clamp 5; A first oblique wedge groove 7 is provided on the inner side of the transverse plate of the clamp 5, the notch of the first oblique wedge groove 7 is located on the side of the transverse plate, and the width of the inner side of the first oblique wedge groove 7 is smaller than the width of the outer side; A second oblique wedge groove 9 is provided on the inner side of one of the side plates, the notch of the second oblique wedge groove 9 is located on the side surface of the side plate, and the width of the inner side of the second oblique wedge groove 9 is smaller than the width of the outer side; The first inclined wedge groove 7 and the second inclined wedge groove 9 are located on the same side of the clamp 5; The structural characteristics of the clamp satisfy the following requirements: after the assembly of the first wear-resistant layer 1 and the base 3 is embedded in the inner space, the assembly can be adjusted so that the outer surface of the first wear-resistant layer 1 faces the first beveled wedge groove 7, and the side of the first wear-resistant layer 1 close to the end of the base 3 faces the second beveled wedge groove 9.
[0043] In summary, the implementation of this welding process depends on the cladding equipment and the electron beam welding equipment. During the implementation of electron beam welding, the prefabricated hole 21 on the substrate 3 for preparing the pin hole 4 can be used to constrain the second wear-resistant layer 2, so as to ensure the matching accuracy between the second wear-resistant layer 2 and the prefabricated hole 21 to achieve the purpose of ensuring the welding quality of the second wear-resistant layer 2 and the substrate 3. However, for the first wear-resistant layer 1, since it needs to be welded on the surface of the end of the substrate 3, specifically, it is welded to the bottom and side surfaces of the notch 10, in order to ensure the welding quality of the first wear-resistant layer 1 when implementing the first welding process, it is necessary to constrain the relative position of the first wear-resistant layer 1 and the substrate 3 before welding. The fixture provided above is used to solve the corresponding fixing problem, specifically: The horizontal plate of the clamp 5 and the two side plates form a channel steel structure. After the first wear-resistant layer 1 is embedded in the notch 10, the locking bolt 6 is used to clamp the base 3 in the inner space. For the cooperation between the bottom surface of the first wear-resistant layer 1 and the bottom surface of the notch 10, in order to obtain a state of always being in contact with each other, the first wear-resistant layer 1 can be pushed so that the bottom surface is always in contact with the bottom surface of the notch 10 by inserting a wedge into the first wedge groove 7. For the cooperation between the side surface of the first wear-resistant layer 1 and the side surface of the notch 10, in order to obtain a state of always being in contact with each other, the first wear-resistant layer 1 can be pushed deep into one side of the notch 10 by inserting a wedge into the second wedge groove 9 to always be in contact with the side surface of the notch 10. The locking bolt 6 is provided to enable the clamp to provide a clamping function for a substrate 3 within a certain length range. The idea of this solution is that after the clamping is completed, the inclined wedge block in the first inclined wedge groove 7 is used to provide a thrust for the first wear-resistant layer 1 along the thickness direction of the first wear-resistant layer 1, and the inclined wedge block in the second inclined wedge groove 9 is used to provide a thrust for the first wear-resistant layer 1 along the length direction of the substrate 3, so as to keep the corresponding two mating surfaces completely in contact, and prepare for the implementation of high-quality electron beam welding of the two mating surfaces.
[0044] Embodiment 9: This embodiment is further refined on the basis of Embodiment 8: When the substrate 3, the first wear-resistant ring and the second wear-resistant ring are preheated before electron beam welding, the fixture needs to be heated together with the above parts. In order to make the corner on the side of the fixture away from the first wear-resistant layer 1 adapt to the thermal deformation of the clamp 5 to ensure the reliability of the fixture in fixing the relevant relative position, it is set as follows: locking bolts 6 are installed on both side panels of the clamp 5, and the corner away from the first inclined wedge groove 7 of the two corners of the clamp 5 is an arc-shaped corner. This solution can fix the substrate 3 by the locking bolts 6 on each side panel; after clamping the corresponding parts, according to the configuration of the hook claw, the horizontal plate at the position of the arc-shaped corner has a large gap with the substrate 3, so that the arc-shaped corner can release the thermal stress of the clamp 5 through deformation.
[0045] Embodiment 10: This embodiment is further refined on the basis of Embodiment 8: In order to shorten the assembly time of the base 3 on the clamp 5, the preferred application is: the spacing of the side plates is equal to the length of the base 3, and when the clamp 5 is deformed, the locking bolt 6 is used to maintain the reliability of the clamp 5 clamping the base 3.
[0046] When welding the bottom surface of the first wear-resistant layer 1 to the bottom surface of the notch 10, in order to prevent the electron beam welding position from affecting the clamp 5, it is set as follows: the inner side of the side plate where the second inclined wedge groove 9 is set is also provided with an avoidance groove 8, the avoidance groove 8 is located on the side of the second inclined wedge groove 9 away from the horizontal plate, and the position of the avoidance groove 8 satisfies: when the assembly is embedded in the inner space and the top surface of the first wear-resistant layer 1 is supported by the horizontal plate, the avoidance groove 8 forms a cavity between the side plate and the assembly, and the bottom surface of the notch 10 is located in the middle of the cavity. By adopting this solution, the space provided by the avoidance groove 8 can be used so that the welding position of the first wear-resistant layer 1 on the substrate 3 can involve the end of the substrate 3, and will not cause the corresponding parts to adhere to the clamp 5.
[0047] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific embodiments of the present invention are limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, other embodiments obtained without departing from the technical solution of the present invention should be included in the protection scope of the present invention.
Claims
1. A double-tooth hook claw welding process, the process comprising a first welding process and a second welding process, the first welding process is to weld a first wear-resistant layer (1) for forming a tooth shape on a base (3) of the hook claw, the second welding process is to weld a second wear-resistant layer (2) for forming a pin hole (4) on the base (3) of the hook claw, the first wear-resistant layer (1) and the second wear-resistant layer (2) are both connected to the base by electron beam welding, the first wear-resistant layer (1) and the second wear-resistant layer (2) are both formed by surfacing welding, It is characterized in that The cladding forming method of the first wear-resistant layer (1) comprises: after cladding a third cladding layer (23) on a welding platform (22), further cladding a fourth cladding layer (24) on the outer side of the third cladding layer (23), wherein the thickness of the fourth cladding layer (24) satisfies: the fourth cladding layer (24) is used as a base material for processing the first wear-resistant layer (1); The method for obtaining the first wear-resistant layer (1) comprises: peeling off the fourth weld overlay layer (24) by material removal processing, and then processing the fourth weld overlay layer (24) into a rectangular block-shaped first wear-resistant layer (1) by shaping processing; in a first welding process, embedding and fixing the first wear-resistant layer (1) in a notch (10) prefabricated on a substrate (3); and then using electron beam welding to weld the mating surfaces of the first wear-resistant layer (1) and the substrate (3); The cladding forming method of the second wear-resistant layer (2) comprises: after cladding a first cladding layer (19) on a core shaft (14), further cladding a second cladding layer (20) on the outer side of the first cladding layer (19), wherein the thickness of the second cladding layer (20) satisfies: the second cladding layer (20) serves as a base material for processing the second wear-resistant layer (2); The method for obtaining the second wear-resistant layer (2) comprises: peeling off the second weld overlay layer (20) by material removal processing, and then processing the second weld overlay layer (20) into a cylindrical second wear-resistant layer (2) by shaping processing; in a second welding process, embedding the second wear-resistant layer (2) into a prefabricated hole (21) prefabricated on a substrate (3); and then using electron beam welding to weld the mating surfaces of the second wear-resistant layer (2) and the substrate (3).
2. A double-tooth hook welding process according to claim 1, It is characterized in that The notch (10) forms a step located at the end of the base (3), the bottom surface and the side surface of the step are both planes, and after the first wear-resistant layer (1) is embedded in the notch (10), the bottom surface of the first wear-resistant layer (1) and the bottom surface of the step have a surface-fitting relationship, and the side surface of the first wear-resistant layer (1) and the side surface of the step have a surface-fitting relationship; The axial direction of the prefabricated hole (21) is located in the width direction of the base body (3), and the notch (10) intersects with both ends of the base body (3) in the width direction.
3. A double-tooth hook welding process according to claim 1, It is characterized in that The outer diameter of the second wear-resistant layer (2) is equal to the diameter of the prefabricated hole (21).
4. A double-tooth hook welding process according to claim 1, It is characterized in that Before the first welding process is performed, the substrate (3) and the first wear-resistant layer (1) are preheated, the preheating being performed in a vacuum box, the vacuum box being evacuated before the preheating, and the vacuum box being evacuated again after the preheating is completed; Before the second welding process is performed, the substrate (3) and the second wear-resistant layer (2) are preheated. The preheating is performed in a vacuum box. Before the preheating, the vacuum box is evacuated. After the preheating is completed, the vacuum box is evacuated again.
5. A double-tooth hook welding process according to claim 4, It is characterized in that After the assembly formed by assembling the first wear-resistant layer (1), the substrate (3), and the second wear-resistant layer (2) is placed in a vacuum box, the vacuum box is evacuated, and then the assembly is preheated. After preheating, the vacuum box is evacuated again, and then electron beam welding is used in the vacuum box to perform a first welding process and a second welding process.
6. A double-tooth hook welding process according to claim 1, It is characterized in that The cladding of the first wear-resistant layer (1) and the second wear-resistant layer (2) is completed in a cladding box; A surfacing box for surfacing the second wear-resistant layer (2) comprises: a surfacing box body, a surfacing operation port is provided on the top surface or the side surface of the surfacing box body, a first connecting seat (12) and a second connecting seat (15) are provided in the surfacing box body, the first connecting seat (12) and the second connecting seat (15) are in a vertically opposite relationship, one of the first connecting seat (12) and the second connecting seat (15) is connected to the surfacing box body via a rotating motor (11), and the other is connected to the surfacing box body via a bearing seat (16); When the second wear-resistant layer (2) is formed by surfacing welding, the two ends of the core shaft (14) are respectively clamped on the first connecting seat (12) and the second connecting seat (15), and the core shaft (14) rotates around its own axis under the action of the rotating motor (11). When surfacing the first surfacing layer (19), surfacing welding is carried out through the surfacing operation port, and a cylindrical first surfacing layer (19) is surfacing welded on the side of the core shaft (14) from bottom to top along the axial direction of the core shaft (14). For any surfacing point at the axial position of the core shaft (14), surfacing welding is carried out at a fixed position, and an annular surfacing layer is obtained during the rotation of the core shaft (14); When surfacing the second surfacing layer (20), surfacing is performed through the surfacing operation port, and a cylindrical second surfacing layer (20) is surfacing on the side of the first surfacing layer (19) from bottom to top along the axial direction of the core shaft (14). For any surfacing point at the axial position of the core shaft (14), surfacing is performed at a fixed position, and an annular surfacing layer is obtained during the rotation of the core shaft (14).
7. A double-tooth hook welding process according to claim 6, It is characterized in that An annular bearing plate (13) is arranged on the core shaft (14), the core shaft (14) passes through the bearing plate (13), and the surfacing starting positions of the first surfacing layer (19) and the second surfacing layer (20) both start from the upper end surface of the bearing plate (13); During the process of cladding the first wear-resistant layer (1) and the second wear-resistant layer (2), protective gas is injected into the cladding box through an air inlet hood (17) installed on the cladding box, and gas in the cladding box is sucked through an air suction hood (18) installed on the cladding box.
8. A welding device for implementing the double-toothed hook welding process according to any one of claims 1 to 7, It is characterized in that The invention comprises a clamp for fixing the relative position of the first wear-resistant layer (1) and the base (3), the clamp comprising a clamp (5) in the shape of a channel steel, at least one of the two side plates of the clamp (5) being threadedly connected with a locking bolt (6), the locking bolt (6) being connected to an internal threaded hole of the side plate, the internal threaded hole being a through hole, and the end of the locking bolt (6) being capable of being embedded in the inner space of the clamp (5); A first oblique wedge groove (7) is provided on the inner side of the transverse plate of the clamp (5), the notch of the first oblique wedge groove (7) is located on the side of the transverse plate, and the width of the inner side of the first oblique wedge groove (7) is smaller than the width of the outer side; A second oblique wedge groove (9) is provided on the inner side of one of the side plates, the notch of the second oblique wedge groove (9) is located on the side surface of the side plate, and the width of the inner side of the second oblique wedge groove (9) is smaller than the width of the outer side; The first oblique wedge groove (7) and the second oblique wedge groove (9) are located on the same side of the clamp (5); The structural characteristics of the clamp satisfy the following requirements: after the assembly of the first wear-resistant layer (1) and the base (3) is embedded in the inner space, the assembly can be adjusted so that the outer surface of the first wear-resistant layer (1) faces the first inclined wedge groove (7), and the surface of the first wear-resistant layer (1) close to the end of the base (3) faces the second inclined wedge groove (9).
9. The welding device according to claim 8, It is characterized in that Locking bolts (6) are installed on both side plates of the clamp (5), and of the two corners of the clamp (5), the corner away from the first inclined wedge groove (7) is an arc-shaped corner.
10. The welding device according to claim 8, It is characterized in that The spacing between the side plates is equal to the length of the base (3); An avoidance groove (8) is also provided on the inner side of the side plate on which the second inclined wedge groove (9) is provided. The avoidance groove (8) is located on a side of the second inclined wedge groove (9) away from the transverse plate, and the position of the avoidance groove (8) satisfies that: when the assembly is embedded in the inner space and the top surface of the first wear-resistant layer (1) is supported by the transverse plate, the avoidance groove (8) forms a cavity between the side plate and the assembly, and the bottom surface of the notch (10) is located in the middle of the cavity.