Aero-engine sector support ring positioning edge size recovery method

Through measurement, damage removal, manual crack removal, welding treatment and cold calibration methods, the problem of repairing the positioning edge of the support ring of the aero engine sector parts is solved, achieving high-quality repair and welding improvement.

CN119017006AActive Publication Date: 2024-11-26CIVIL AVIATION UNIV OF CHINA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411357697.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-11-26
Estimated Expiration
2044-09-27

AI Technical Summary

Technical Problem

The positioning edges of the supporting ring of the aero engine sector are prone to defects such as burning and thermal cracks in high temperature environments, resulting in reduced weldability and cannot be reinstalled after disassembly. It is difficult for existing repair technologies to achieve high-quality repair.

Method used

By measuring the characteristic size of the support ring, removing damaged materials, manually removing residual cracks, performing pre-weld heat treatment, manual surfacing and repairing, automatic track welding and surfacing, post-weld heat treatment and cold correction, and finally machine forming to achieve support ring positioning High-quality repair of the edge.

Benefits of technology

The damage repair quality of the supporting ring positioning edge is improved, the deformation of the supporting ring is eliminated, the high-quality repair of the supporting ring is achieved, and the welding and reliability are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119017006A_ABST
    Figure CN119017006A_ABST
Patent Text Reader

Abstract

The invention relates to an aero-engine sector support ring positioning edge size recovery method. The method comprises the following steps: step 1), measuring the feature size of a support ring; (2) machining a damaged positioning edge of the supporting ring; (3) residual cracks of the supporting ring are manually removed; (4) carrying out pre-welding heat treatment on the support ring; (5) the supporting ring is subjected to manual surfacing modification; (6) build-up welding additional materials are conducted on the positioning edge of the supporting ring; (7) carrying out post-weld heat treatment on the support ring; (8) the shape of the supporting ring is subjected to cold correction; and (9) machining and forming the positioning edge of the supporting ring. According to the aero-engine sector piece supporting ring positioning edge size recovery method, the damage repair quality of the supporting ring positioning edge is improved, meanwhile, deformation of the supporting ring is eliminated, and high-quality repair of the supporting ring is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of repairing aircraft engine structural parts, and in particular relates to a method for restoring the size of a positioning edge of a support ring of an aircraft engine sector part. Background Art

[0002] The support ring is an important structural part of the aircraft engine. The installation and positioning of fan-shaped parts such as sealing parts and guide blades are achieved by setting the positioning edge on the support ring. It is generally made of high-temperature alloy with high alloy content, which reduces the weldability while increasing the service life of the component. The support ring works in a high-temperature environment for a long time, resulting in a decrease in strength. It deforms under high stress, uneven temperature field and stress. It cannot be reinstalled after being disassembled during overhaul. The positioning edge is a thin-walled structure with poor ablation resistance. Under the action of high temperature, high speed and highly corrosive gas, it is easy to have defects such as burning and thermal cracking. Sulfur, phosphorus and other elements in the gas penetrate into the damaged surface and reduce the weldability of the base material. The use of surfacing welding, processing subtractive forming, and correction technology to restore the outer dimensions of the support ring can avoid the expensive cost of purchasing new accessories. Summary of the invention

[0003] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for restoring the size of the positioning edge of an aircraft engine fan-shaped support ring, which improves the quality of repairing the damage of the positioning edge of the support ring, eliminates the deformation of the support ring, and realizes high-quality repair of the support ring.

[0004] The present invention solves the technical problem by the following technical solutions:

[0005] A method for restoring the size of the positioning edge of a support ring of an aircraft engine sector, the repair method comprising the following steps:

[0006] Step 1): Measuring characteristic dimensions of the support ring: measuring and determining the outer diameter of the outer surface A of the support ring, and measuring and determining the characteristic dimensions of the first positioning edge and the second positioning edge;

[0007] Step 2): Machining of the damaged positioning edge of the support ring: machining to remove the powdered and burned materials on the surface of the first positioning edge and the second positioning edge;

[0008] Step 3): Manually remove the remaining cracks on the support ring: Grind and remove the remaining cracks, and shape the grinding notch into a regular "V" shape, with the chamfer radius of the bottom notch not less than 2mm;

[0009] Step 4): Heat treatment before support ring welding: The support ring is heated to 850-1000°C in a vacuum or argon atmosphere furnace for 30-100 minutes, and then taken out after cooling to room temperature.

[0010] Step 5): Manual surfacing welding of the support ring: fill the V-shaped gap of the support ring by welding until no cracks are visible;

[0011] Step 6): Additive surfacing welding of the positioning edge of the support ring: Based on the characteristic dimensions measured in step 1), surfacing welding of the first positioning edge and the second positioning edge is completed on the track automatic welding machine;

[0012] Step 7): Heat treatment after support ring welding: in a vacuum or argon atmosphere furnace, heat up to 850-1000°C and keep warm for 30-100 minutes, cool down to 700-800°C and keep warm for 200-300 minutes, cool to room temperature with the furnace and take out from the heat treatment furnace;

[0013] Step 8): Cold shaping of the support ring: placing the support ring on a shaping tool for cold shaping of the shape;

[0014] Step 9): Machining of the support ring positioning edge: Based on the characteristic dimensions measured in step 1), the first positioning edge and the second positioning edge are machined and formed.

[0015] Moreover, the specific operation of measuring the characteristic dimensions of the support ring in step 1 is:

[0016] ①Measure the outer diameter of the support ring outer surface A:

[0017] Measure the outer diameter of the outer surface A of the support ring at multiple positions, calculate the average outer diameter D1 of the outer surface A of the support ring, and select the outer diameter of the outer surface corresponding to the position M equal to D1;

[0018] ②Measure the characteristic dimensions of the first positioning edge and the second positioning edge:

[0019] Taking the lower surface of the support ring as the support ring reference plane B, measure the distance H1 between the upper surface of the first positioning edge and the support ring reference plane B, the distance H2 between the lower surface of the first positioning edge and the reference plane A, and the distance H3 between the upper surface of the second positioning edge and the reference plane B;

[0020] The inner diameters of multiple positions of the first positioning edge are measured to obtain an average value D2, the inner diameters of multiple positions of the second positioning edge are measured to obtain an average value D3, and the outer diameters of multiple positions of the second positioning edge are measured to obtain an average value D4.

[0021] Moreover, the specific operation of machining the damaged positioning edge in the step 2) is: installing the damaged support ring on the processing table of the vertical lathe, taking the reference plane B and the position M as the reference, machining and removing the powdered and burned materials on the surface of the first positioning edge and the second positioning edge, until the machined surface all presents a continuous metallic luster, and detecting surface defects by penetrant testing. If clustered cracks appear, continue to process the positioning edge surface, and then perform penetrant testing until no clustered cracks are displayed.

[0022] Moreover, the specific operation of manually removing the residual cracks in the support ring in the step 3) is: manually grinding and removing the residual cracks on the positioning edge with an electric grinder and a small-diameter electric grinder head, and detecting the surface defects of the positioning edge by penetrant testing. If crack defects are displayed, continue to use the electric grinder to remove them and then perform penetrant testing until no crack defects are displayed on the surface; the grinding notch is reshaped into a regular "V" shape, and the chamfer radius of the bottom notch is not less than 2mm.

[0023] Moreover, the specific operation of the heat treatment before the support ring welding in the step 4) is: placing the support ring on a high-temperature ceramic base plate with a flat surface to prevent the support ring from being deformed due to the decrease in high-temperature strength during the heat treatment process, placing the support ring and the base plate together in a vacuum or argon atmosphere furnace, heating to 850-1000°C and keeping warm for 30-100 minutes, and taking it out of the heat treatment furnace after cooling to room temperature.

[0024] Moreover, the specific operation of manual surfacing welding repair in the step 5) is: use sandpaper to grind and remove the oxide scale of the first positioning edge, the second positioning edge and the surrounding area, wipe and clean them with non-woven cloth dipped in a cleaning agent, use manual tungsten inert gas arc welding with welding wire, and use a small current, a small wire feed amount, and an intermittent repair welding method to fill the V-shaped notch; use an electric grinder to grind off excess material in the repair welding area, and use penetrant testing to detect surface defects in the repair welding area. If a crack defect is displayed, continue to repair welding and grinding with an electric grinder and perform penetrant testing until no crack defects are displayed.

[0025] Moreover, the specific operation of the support ring positioning edge surfacing welding in the step 6) is: the surfacing welding is performed on the orbital automatic welding machine, and the spatial posture of the six-axis manipulator of the orbital automatic welding machine is adjusted so that the axis C of the inner surface of the first positioning edge processing of the support ring coincides with the rotation axis of the turntable, and the second positioning edge processing upper surface D is parallel to the first connecting plate of the turntable; the welding head is installed in the horizontal welding mode, the turntable of the orbital automatic welding machine is adjusted so that the welding gun points to the position M, and the six-axis manipulator is adjusted to move vertically up and down so that the vertical distance between the tungsten electrode tip of the welding gun and the reference plane B of the support ring is Adjust the scissor-type adjustment table of the orbital automatic welding machine so that the welding gun gun distance is the set value, set the welding gun arc starting and ending points and welding parameters, and execute the welding program to complete the first weld surfacing; set the second weld arc starting and ending points relative to the first weld arc starting and ending points 30° clockwise, adjust the scissor-type adjustment table of the orbital automatic welding machine so that the welding gun gun distance is the set value, and execute the welding program to complete the second weld surfacing; and so on, until the inner diameter of the first positioning edge is D2-(3~5)mm, the first positioning edge surfacing is completed; adjust the six-axis manipulator to move vertically downward to keep the support ring away from the welding head, install the welding head in vertical welding mode, adjust the turntable to point the welding gun to position M, adjust the scissor-type adjustment table so that the horizontal distance between the tungsten electrode tip of the welding gun and the outer surface A of the support ring is Adjust the vertical movement of the six-axis manipulator up and down so that the welding gun gun distance is the set value, set the welding gun arc starting and ending points and welding parameters, and then execute the welding program to complete the first weld surfacing; set the second weld arc starting and ending points relative to the first weld arc starting and ending points 30° clockwise, adjust the six-axis manipulator up and down vertical movement so that the welding gun gun distance is the set value, and execute the welding program to complete the second weld surfacing; and so on, until the vertical distance from the upper edge of the second positioning edge to the reference plane B is H3+(1.5~2.5)mm, and the second positioning edge surfacing is completed.

[0026] Moreover, the specific operation of the post-weld heat treatment in the step 7) is: placing the support ring on a high-temperature ceramic base plate with a flat surface to prevent the support ring from being deformed due to the decrease in high-temperature strength during the heat treatment process, placing the support ring and the base plate together in a vacuum or argon atmosphere furnace, heating to 850-1000°C and keeping it for 30-100 minutes, cooling to 700-800°C and keeping it for 200-300 minutes, and taking it out of the heat treatment furnace after cooling to room temperature.

[0027] Moreover, the specific operation of the cold shaping of the outer shape in the step 8) is as follows: placing the support ring on the base of the shaping tool, with the reference surface A in contact with the upper surface of the base; the first push rod, the second push rod, the third push rod, and the fourth push rod of the shaping tool are evenly distributed on the inner side of the support ring, and the screw push rods of the four push rods are screwed to drive the top plate to move outward, so that the outer surface of the top plate contacts the push surface E of the support ring; the outer diameter of the outer surface A of the support ring is measured at multiple positions, and the position with the smallest outer diameter is marked as position N1, and the support ring is adjusted so that position N1 is opposite to the first push rod, and the screw push rods of the second push rod and the fourth push rod are screwed to drive the top plate to move inward. Move so that the distance between the outer surface of the top plate and the pushing surface E of the support ring is 0.1-1.0mm, and screw the screw push column of the first push rod to drive the top plate to move outward to push the pushing surface E of the support ring, so that the support ring produces a slight deformation along the pushing direction; screw the screw push column of the first push rod to drive the top plate to move inward to unload the pushing force, measure the outer diameter of the support ring in multiple directions, mark the position with the smallest outer diameter as position N2, repeat the above pushing operation until the outer diameter of the support ring meets the roundness requirement; use penetrant flaw detection to detect the surface integrity of the first positioning edge and the second positioning edge. If crack defects are displayed, repeat from step 3.

[0028] Furthermore, the specific operation of machining the positioning edges in step 9) is as follows: the support ring (8) is mounted on a vertical lathe processing table, and the first positioning edge and the second positioning edge are machined based on the reference plane B and the characteristic dimensions measured in step 1).

[0029] The advantages and beneficial effects of the present invention are:

[0030] 1. The method for restoring the size of the positioning edge of the support ring of the fan-shaped part of the aircraft engine of the present invention reduces the amount of base material removal under the premise of completely removing the damage to the positioning edge through the combination of machining and manual machining, improves the weldability of the support ring through pre-welding heat treatment and post-welding heat treatment, improves the quality and reliability of welding additives through manual surfacing and track automatic surfacing, eliminates the deformation of the support ring through post-welding cold shaping, and completes the positioning edge processing and forming through machining. This method improves the quality of the repair of the positioning edge damage of the support ring while eliminating the deformation of the support ring, thereby achieving high-quality repair of the support ring. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a schematic diagram of damage to the support ring of the present invention;

[0032] Figure 2 This is a front view of the damaged support ring of the present invention;

[0033] Figure 3 A cross-sectional view of a damaged support ring of the present invention;

[0034] Figure 4 It is a cross-sectional view after machining of the positioning edge of the present invention;

[0035] Figure 5 This is a schematic diagram of the automatic welding structure of the positioning edge 1 track of the present invention;

[0036] Figure 6 It is a structural schematic diagram of a positioning edge 1 track automatic welding welding machine head of the present invention;

[0037] Figure 7 This is a schematic diagram of the automatic welding structure of the positioning edge 2 track of the present invention;

[0038] Figure 8 It is a structural schematic diagram of a positioning side 2 track automatic welding welding head of the present invention;

[0039] Fig. 9 It is a schematic diagram of the cold-shaping tool structure of the present invention;

[0040] Fig.10 It is a schematic diagram of the cold-correcting ejector structure of the present invention.

[0041] Description of Reference Numerals

[0042] 1 base, 2 column, 3 beam, 4 turntable, 5 welding head, 6 six-axis manipulator, 7 bottom plate, 8 support ring, 8-1 first positioning edge, 8-2 second positioning edge, 8-3 damage, 5-1 first connecting plate, 5-2 second connecting plate, 5-3 scissor-type adjustment table, 5-4 third connecting plate, 5-5 fourth connecting plate, 5-6 wire feeder, 5-7 welding gun bracket, 5-8 welding gun locking block, 5-9 welding gun, 9 base, 10 first push rod, 11 second push rod, 12 third push rod, 13 fourth push rod, 10-1 locking nut, 10-2 positioning pin, 10-3 screw push rod, 10-4 thrust bearing, 10-5 top plate. DETAILED DESCRIPTION

[0043] The present invention is further described in detail below through specific examples. The following examples are only illustrative and not restrictive, and the protection scope of the present invention cannot be limited thereto.

[0044] A method for restoring the size of a positioning edge of a support ring of an aircraft engine sector, comprising the following steps:

[0045] Step 1: Measurement of the characteristic dimensions of the support ring, such as Figure 1 , Figure 2 , Figure 3 As shown,

[0046] ①Measure the outer diameter of the support ring outer surface A:

[0047] Measure the outer diameter of the outer surface A of the support ring at multiple positions, calculate the average outer diameter D1 of the outer surface A of the support ring, and select the outer diameter of the outer surface corresponding to the position M equal to D1;

[0048] ②Measure the characteristic dimensions of the first positioning edge 8-1 and the second positioning edge 8-2:

[0049] Taking the lower surface of the support ring as the support ring reference plane B, measure the distance H1 between the upper surface of the first positioning edge 8-1 and the support ring reference plane B, the distance H2 between the lower surface of the first positioning edge 8-1 and the reference plane A, and the distance H3 between the upper surface of the second positioning edge 8-2 and the reference plane B;

[0050] The inner diameters of multiple positions of the first positioning edge 8-1 are measured to obtain an average value D2, the inner diameters of multiple positions of the second positioning edge 8-2 are measured to obtain an average value D3, and the outer diameters of multiple positions of the second positioning edge 8-2 are measured to obtain an average value D4.

[0051] Step 2: Support ring damage positioning edge machining, such as Figure 4As shown, the damaged support ring is installed on the processing table of the vertical lathe. With reference plane B and position M as reference, the powdered and burned materials on the surface of the first positioning edge 8-1 and the second positioning edge 8-2 are processed and removed until the machined surface all presents a continuous metallic luster. The surface defects are detected by penetrant testing. If clustered cracks appear, the positioning edge surface is further processed, and then the penetrant testing is performed until no clustered cracks are displayed.

[0052] Step 3: Manually remove the remaining cracks on the support ring. Use an electric grinder with a small diameter electric grinder to manually grind and remove the residual cracks on the positioning edge. Perform penetrant testing to detect surface defects on the positioning edge. If crack defects are displayed, continue to use the electric grinder to remove them and then perform penetrant testing until no crack defects are displayed on the surface; trim the grinding notch into a regular "V" shape, and the chamfer radius of the bottom notch should not be less than 2mm.

[0053] Step 4: Heat treatment before support ring welding. Place the support ring on a high-temperature ceramic base plate with a flat surface to prevent the support ring from deforming due to the decrease in high-temperature strength during the heat treatment process. Place the support ring and the base plate together in a vacuum or argon atmosphere furnace, heat to 850-1000℃ and keep warm for 30-100 minutes. Cool to room temperature with the furnace and take it out of the heat treatment furnace.

[0054] Step 5: Manual surfacing welding repair of the support ring, use sandpaper to grind and remove the oxide scale of the first positioning edge 8-1, the second positioning edge 8-2 and the surrounding area, wipe and clean with non-woven cloth dipped in cleaning agent, use manual tungsten inert gas arc welding with welding wire, use small current, small wire feed amount, and intermittent repair welding to fill the V-shaped gap; use an electric grinder to grind off excess material in the repair welding area, and use penetrant testing to detect surface defects in the repair welding area. If crack defects are displayed, use an electric grinder to grind and continue repair welding and grinding and penetrant testing until no crack defects are displayed.

[0055] Step 6: Support ring positioning and edge cladding are performed on a track automatic welding machine.

[0056] like Figure 5 , Figure 6 , Figure 7 , Figure 8As shown, the orbital automatic welding machine required for the above-mentioned support ring surfacing additive consists of a base 1, a column 2, a beam 3, a turntable 4, a welding head 5, a six-axis manipulator 6, a bottom plate 7, and a support ring 8; the base 1 is a horizontal plate structure, the six-axis manipulator 6 is installed on the left side of the base 1, the bottom plate 7 is a circular flat plate, installed on the execution end of the six-axis manipulator 6, the support ring 8 is installed on the bottom plate 7, the reference surface B is in contact with the bottom plate 7, the column 2 is installed on the right side of the base 1, the beam 3 is installed at the top of the column 2, pointing to the six-axis manipulator 6, the turntable 4 is installed below the cantilever end of the beam 3, and the welding head 5 is installed below the turntable 4; the welding head 5 consists of a first connecting plate 5-1, a second connecting plate 5-2, a scissor-type adjustment table 5-3, a third connecting plate 5-4, a fourth connecting plate 5-5, a wire feeder 5-6, a welding gun bracket 5-7, a welding gun locking block 5-8, and a welding gun 5-9; the first connecting plate 5-1 is a circular The fourth connecting plate 5-5 is a "C"-shaped flat plate, the second connecting plate 5-2 is a square cylinder, which is installed below the first connecting plate 5-1, the scissor-type adjustment table 5-3 is installed on the side of the second connecting plate 5-2, and the third connecting plate 5-4 is an L-shaped connecting plate, and the long end is installed on the scissor-type adjustment table 5-3; the fourth connecting plate 5-5 is a "C"-shaped flat plate, the welding gun bracket 5-7 is installed at one end of the fourth connecting plate 5-5, and there is a circular groove in the middle of the bottom end, and there is a circular groove in the middle of the upper end of the welding gun locking block 5-8, which cooperates with the groove at the bottom end of the welding gun bracket 5-7 to clamp and fix the welding gun 5-9, and the wire feeder 5-6 is installed at the other end of the fourth connecting plate 5-5, and the wire feeding direction points to the tungsten electrode tip of the welding gun; the fourth connecting plate 5-5 is installed at the short end of the third connecting plate 5-4, and the welding gun 5-9 points outward to form a horizontal welding mode; the fourth connecting plate 5-5 is installed at the long end of the third connecting plate 5-4, and the welding gun 5-9 is vertically downward to form a vertical welding mode.

[0057] Adjust the spatial posture of the six-axis manipulator 6 of the track automatic welding machine so that the axis C of the inner surface processed by the first positioning edge 8-1 of the support ring 8 coincides with the rotation axis of the turntable 4, and the upper surface D processed by the second positioning edge 8-2 is parallel to the first connecting plate 5-1 of the turntable 4; install the welding head 5 in the horizontal welding mode, adjust the turntable 4 of the track automatic welding machine so that the welding gun 5-9 points to the position M, and adjust the six-axis manipulator 6 to move vertically up and down so that the vertical distance between the tungsten tip of the welding gun 5-9 and the reference plane B of the support ring 8 is (H1+H 2) / 2+(0.3~0.5)mm, adjust the scissor-type adjustment table 5-3 of the orbital automatic welding machine so that the gun distance of the welding gun 5-9 is the set value, set the arc starting and ending points of the welding gun 5-9 and the welding parameters, and execute the welding program to complete the first weld cladding; set the arc starting and ending points of the second weld to be 30° clockwise relative to the arc starting and ending points of the first weld, adjust the scissor-type adjustment table 5-3 of the orbital automatic welding machine so that the gun distance of the welding gun 5-9 is the set value, and execute the welding program to complete the second weld cladding; and so on, until the first positioning The inner diameter of edge 8-1 is D2-(3~5)mm, and the first positioning edge 8-1 surfacing is completed; the six-axis manipulator 6 is adjusted to move vertically downward to make the support ring 8 away from the welding head 5, and the welding head 5 is installed in the vertical welding mode. The turntable 4 is adjusted to make the welding gun 5-9 point to the position M, and the scissor adjustment table 5-3 is adjusted to make the horizontal distance between the tungsten tip of the welding gun 5-9 and the outer surface A of the support ring 8 is (D1-(D3+D4) / 2) / 2, and the six-axis manipulator 6 is adjusted to move vertically up and down to make the welding gun 5-9 gun distance set to Set the starting and ending points of the welding gun 5-9 and the welding parameters, and then execute the welding procedure to complete the first weld buildup; set the starting and ending points of the second weld to be 30° clockwise relative to the starting and ending points of the first weld, adjust the vertical movement of the six-axis manipulator 6 up and down so that the gun distance of the welding gun 5-9 is the set value, and execute the welding procedure to complete the second weld buildup; and so on, until the vertical distance from the upper edge of the second positioning edge 8-2 to the reference plane B is H3+(1.5~2.5)mm, and the second positioning edge 8-2 buildup is completed.

[0058] Step 7: Heat treatment after support ring welding. Place the support ring on a flat high-temperature ceramic base plate to prevent deformation of the support ring due to the decrease in high-temperature strength during the heat treatment process. Place the support ring and the base plate together in a vacuum or argon atmosphere furnace. Heat to 850-1000°C for 30-100 minutes, cool to 700-800°C for 200-300 minutes, and take it out of the heat treatment furnace after cooling to room temperature.

[0059] Step 8: Cold calibration of the support ring shape, such as Fig. 9 , Fig.10As shown, the shaping tooling required for cold shaping of the support ring shape provided by the present invention is composed of a base 9, a first push rod 10, a second push rod 11, a third push rod 12, and a fourth push rod 13; the base 9 is a horizontal plate-like structure with regularly arranged through holes on it; the support ring 8 is located on the upper surface of the base 9; the first push rod 10, the second push rod 11, the third push rod 12, and the fourth support rod 13 are evenly distributed on the inner side of the support ring 8 and are installed and fixed through the through holes on the base 9; the first push rod 10, the second push rod 11, the third push rod 12, and the fourth push rod 13 are composed of a locking nut 10-1, a positioning pin 10-2, a screw push column 10-3, a thrust bearing 10-4, and a top The top plate 10-5 is composed of a threaded plate 10-2; the lower section of the locating pin 10-2 is threaded and fixed to the base 9 by a locking nut 10-1; the middle section is a cylinder, the outer diameter of which is the same as the inner diameter of the through hole on the base 9, and there is a threaded through hole in the middle of the upper section; the right section of the screw top column 10-3 is a lever arm, the middle section is threaded and cooperates with the thread of the threaded through hole in the upper section of the locking nut 10-1, and the left end is a cylinder; the inner diameter of the thrust bearing 10-4 is the same as the outer diameter of the cylinder at the left end of the screw top column 10-3; the top plate 10-5 is an arc-shaped plate, the outer surface diameter of which is the same as the inner diameter of the push surface E of the support ring 8, and there is a cylindrical groove on the inside, and the inner diameter of the groove is the same as the outer diameter of the thrust bearing 10-4.

[0060] Place the support ring 8 on the base 9 of the shape correction tool, and the reference surface A contacts the upper surface of the base 9; the first push rod 10, the second push rod 11, the third push rod 12, and the fourth push rod 13 of the shape correction tool are installed on the inner side of the support ring 8 and are evenly distributed, and the screw push rods 10-3 of the four push rods are screwed to drive the top plate 10-5 to move outward, so that the outer surface of the top plate 10-5 contacts the push surface E of the support ring 8; measure the outer diameter of the outer surface A of the support ring 8 at multiple positions, mark the position with the smallest outer diameter as position N1, adjust the support ring 8 so that position N1 is opposite to the first push rod 10, and screw the screw push rods 10-3 of the second push rod 11 and the fourth push rod 13 to drive the top plate 10-5 to move inward, so that the top plate 10- The distance between the outer surface of 5 and the pushing surface E of the support ring 8 is 0.1-1.0mm. The screw push column 10-3 of the first push rod 10 drives the push plate 10-5 to move outward to push the pushing surface E of the support ring 8, so that the support ring 8 is slightly deformed along the pushing direction; the screw push column 10-3 of the first push rod 10 drives the push plate 10-5 to move inward to unload the pushing force, and the outer diameter of the support ring 8 is measured in multiple directions. The position with the smallest outer diameter is marked as position N2, and the above pushing operation is repeated until the outer diameter of the support ring 8 meets the roundness requirement; the surface integrity of the first positioning edge 8-1 and the second positioning edge 8-2 is detected by penetrant testing. If a crack defect is displayed, repeat from step 3.

[0061] Step 9: The support ring positioning edge is machined and formed. The support ring 8 is installed on the processing table of the vertical lathe. Taking the reference plane B as the reference, the first positioning edge 8-1 and the second positioning edge 8-2 are machined and formed according to the characteristic dimensions measured in step 1).

[0062] Although the embodiments and drawings of the present invention are disclosed for illustrative purposes, those skilled in the art will appreciate that various substitutions, changes and modifications are possible without departing from the spirit and scope of the present invention and the appended claims. Therefore, the scope of the present invention is not limited to the contents disclosed in the embodiments and drawings.

Claims

1. A method for restoring the size of the positioning edge of a support ring of an aircraft engine sector, characterized in that: The repair method comprises the following steps: Step 1): Measuring characteristic dimensions of the support ring: measuring and determining the outer diameter of the outer surface A of the support ring, and measuring and determining the characteristic dimensions of the first positioning edge (8-1) and the second positioning edge (8-2); Step 2): machining the damaged positioning edge of the support ring: machining to remove the powdered and burned materials on the surface of the first positioning edge (8-1) and the second positioning edge (8-2); Step 3): Manually remove the remaining cracks on the support ring: Grind to remove the remaining cracks, and shape the grinding notch into a regular "V" shape, with the chamfer radius of the bottom notch not less than 2mm; Step 4): Heat treatment before support ring welding: The support ring is heated to 850-1000°C in a vacuum or argon atmosphere furnace for 30-100 minutes, and then taken out after cooling to room temperature. Step 5): Manual surfacing welding of the support ring: fill the V-shaped gap of the support ring by welding until no cracks are visible; Step 6): surfacing welding of the support ring positioning edge: on the track automatic welding machine, according to the characteristic dimensions measured in step 1), completing the surfacing welding of the first positioning edge (8-1) and the second positioning edge (8-2); Step 7): Heat treatment after support ring welding: in a vacuum or argon atmosphere furnace, heat up to 850-1000°C and keep warm for 30-100 minutes, cool down to 700-800°C and keep warm for 200-300 minutes, cool to room temperature with the furnace and take out from the heat treatment furnace; Step 8): Cold shaping of the support ring: placing the support ring on a shaping tool for cold shaping of the shape; Step 9): Machining of the support ring positioning edge: Based on the characteristic dimensions measured in step 1), the first positioning edge and the second positioning edge are machined and formed.

2. The method for restoring the size of the positioning edge of the support ring of an aircraft engine sector according to claim 1, characterized in that: The specific operation of measuring the characteristic dimensions of the support ring in step 1 is: ①Measure the outer diameter of the support ring outer surface A: Measure the outer diameter of the outer surface A of the support ring at multiple positions, calculate the average outer diameter D1 of the outer surface A of the support ring, and select the outer diameter of the outer surface corresponding to the position M equal to D1; ②Measure the characteristic dimensions of the first positioning edge (8-1) and the second positioning edge (8-2): Taking the lower surface of the support ring as the support ring reference plane B, measure the distance H1 between the upper surface of the first positioning edge (8-1) and the support ring reference plane B, the distance H2 between the lower surface of the first positioning edge (8-1) and the reference plane A, and the distance H3 between the upper surface of the second positioning edge (8-2) and the reference plane B; The inner diameters of multiple positions of the first positioning edge (8-1) are measured to obtain an average value D2, the inner diameters of multiple positions of the second positioning edge (8-2) are measured to obtain an average value D3, and the outer diameters of multiple positions of the second positioning edge (8-2) are measured to obtain an average value D4.

3. The method for restoring the size of the positioning edge of the support ring of an aircraft engine sector according to claim 1, characterized in that: The specific operation of machining the damaged positioning edge in the step 2) is as follows: the damaged support ring is mounted on the processing table of the vertical lathe, and the powdered and burned materials on the surface of the first positioning edge (8-1) and the second positioning edge (8-2) are removed by machining with reference plane B and position M as reference, until the machined surfaces all present a continuous metallic luster, and the surface defects are detected by penetrant testing. If clustered cracks appear, the positioning edge surface is further processed, and then the penetrant testing is performed again until no clustered cracks are displayed.

4. The method for restoring the size of the positioning edge of the support ring of an aircraft engine sector according to claim 1, characterized in that: The specific operation of manually removing the residual cracks in the support ring in the step 3) is as follows: manually grind and remove the residual cracks on the positioning edge with an electric grinder and a small-diameter electric grinder head, and perform penetrant testing to detect surface defects on the positioning edge. If crack defects are displayed, continue to use the electric grinder to remove them and then perform penetrant testing until no crack defects are displayed on the surface; the grinding notch is reshaped into a regular "V" shape, and the chamfer radius of the bottom notch is not less than 2mm.

5. The method for restoring the size of the positioning edge of the support ring of an aircraft engine sector according to claim 1, characterized in that: The specific operation of the heat treatment before the support ring welding in the step 4) is: placing the support ring on a high-temperature ceramic base plate with a flat surface to prevent the support ring from being deformed due to the decrease in high-temperature strength during the heat treatment process, placing the support ring and the base plate together in a vacuum or argon atmosphere furnace, heating to 850-1000°C and keeping warm for 30-100 minutes, and taking it out of the heat treatment furnace after cooling to room temperature.

6. The method for restoring the size of the positioning edge of the support ring of an aircraft engine sector according to claim 1, characterized in that: The specific operation of manual surfacing welding repair in the step 5) is as follows: use sandpaper to grind and remove the oxide scale of the first positioning edge (8-1), the second positioning edge (8-2) and the surrounding area, wipe and clean them with a non-woven cloth dipped in a cleaning agent, use manual tungsten inert gas arc welding with welding wire, use a small current, a small wire feed amount, and an intermittent repair welding method to fill the V-shaped gap; use an electric grinder to grind away excess material in the repair welding area, and use penetrant testing to detect surface defects in the repair welding area. If a crack defect is displayed, continue to grind with an electric grinder and then continue to weld and grind and perform penetrant testing until no crack defect is displayed.

7. The method for restoring the size of the positioning edge of the support ring of an aircraft engine sector according to claim 1, characterized in that: The specific operation of the surfacing welding of the positioning edge of the support ring in step 6) is as follows: the surfacing welding is performed on the orbital automatic welding machine, and the spatial posture of the six-axis manipulator (6) of the orbital automatic welding machine is adjusted so that the axis C of the inner surface processed by the first positioning edge (8-1) of the support ring (8) coincides with the rotation axis of the turntable (4), and the upper surface D processed by the second positioning edge (8-2) is parallel to the first connecting plate (5-1) of the turntable (4); the welding machine head (5) is installed in a horizontal welding mode, the turntable (4) of the orbital automatic welding machine is adjusted so that the welding gun (5-9) points to the position M, and the six-axis manipulator (6) is adjusted to move vertically up and down so that the vertical distance between the tungsten electrode tip of the welding gun (5-9) and the reference surface B of the support ring (8) is The scissor-type adjustment table (5-3) of the track automatic welding machine is adjusted so that the gun distance of the welding gun (5-9) is the set value, the arc starting and ending points of the welding gun (5-9) and the welding parameters are set, and the welding program is executed to complete the first weld cladding; the arc starting and ending points of the second weld are set to deviate 30 degrees clockwise relative to the arc starting and ending points of the first weld, and the scissor-type adjustment table (5-3) of the track automatic welding machine is adjusted so that the gun distance of the welding gun (5-9) is the set value, and the welding program is executed to complete the second weld cladding; and so on. Until the inner diameter of the first positioning edge (8-1) is D2-(3-5) mm, the first positioning edge (8-1) is built-up; the six-axis manipulator (6) is adjusted to move vertically downward so that the support ring (8) is away from the welding head (5), the welding head (5) is installed in a vertical welding mode, the turntable (4) is adjusted so that the welding gun (5-9) points to the position M, and the scissor adjustment table (5-3) is adjusted so that the horizontal distance between the tungsten electrode tip of the welding gun (5-9) and the outer surface A of the support ring (8) is The six-axis manipulator (6) is adjusted to move vertically up and down so that the gun distance of the welding gun (5-9) is the set value, and the welding program is executed after the arc starting and ending points of the welding gun (5-9) and welding parameters are set to complete the first weld surfacing; the arc starting and ending points of the second weld are set to deviate 30 degrees clockwise relative to the arc starting and ending points of the first weld, and the six-axis manipulator (6) is adjusted to move vertically up and down so that the gun distance of the welding gun (5-9) is the set value, and the welding program is executed to complete the second weld surfacing; and so on, until the vertical distance between the upper edge of the second positioning edge (8-2) and the reference plane B is H3+(1.5-2.5) mm, and the second positioning edge (8-2) is completed.

8. The method for restoring the size of the positioning edge of the support ring of an aircraft engine sector according to claim 1, characterized in that: The specific operation of the post-weld heat treatment in the step 7) is as follows: placing the support ring on a high-temperature ceramic base plate with a flat surface to prevent the support ring from being deformed due to the decrease in high-temperature strength during the heat treatment process, placing the support ring and the base plate together in a vacuum or argon atmosphere furnace, heating to 850-1000°C and keeping it for 30-100 minutes, cooling to 700-800°C and keeping it for 200-300 minutes, and taking it out of the heat treatment furnace after cooling to room temperature.

9. The method for restoring the size of the positioning edge of the support ring of an aircraft engine sector according to claim 1, characterized in that: The specific operation of the cold shaping of the outer shape in the step 8) is as follows: placing the support ring (8) on the base (9) of the shaping tool, with the reference surface A in contact with the upper surface of the base (9); installing the first push rod (10), the second push rod (11), the third push rod (12), and the fourth push rod (13) of the shaping tool evenly distributed on the inner side of the support ring (8), screwing the screw push rods (10-3) of the four push rods to drive the top plate (10-5) to move outward, so that the outer surface of the top plate (10-5) contacts the push surface E of the support ring (8); measuring the outer diameter of the outer surface A of the support ring (8) at multiple positions, marking the position with the smallest outer diameter as position N1, adjusting the support ring (8) so that position N1 is directly opposite to the first push rod (10), screwing the screw push rods (10-3) of the second push rod (11) and the fourth push rod (13) to drive the top plate (10-5) to move outward, so that the outer surface of the top plate (10-5) contacts the push surface E of the support ring (8). 0-5) moves inwards, so that the outer surface of the top plate (10-5) and the push surface E of the support ring (8) are spaced 0.1 to 1.0 mm apart, the screw push column (10-3) of the first push rod (10) is screwed to drive the top plate (10-5) to move outwards to push the push surface E of the support ring (8), so that the support ring (8) is slightly deformed along the push direction; the screw push column (10-3) of the first push rod (10) is screwed to drive the top plate (10-5) to move inwards to unload the push force, the outer diameter of the support ring (8) is measured in multiple directions, and the position with the smallest outer diameter is marked as position N2, and the above push operation is repeated until the outer diameter of the support ring (8) meets the roundness requirement; the surface integrity of the first positioning edge (8-1) and the second positioning edge (8-2) is detected by penetrant flaw detection, and if crack defects are displayed, the process is repeated from step 3.

10. The method for restoring the size of the positioning edge of the support ring of an aircraft engine sector according to claim 1, characterized in that: The specific operation of machining the positioning edges in step 9) is: installing the support ring (8) on the processing table of the vertical lathe, taking the reference plane B as the reference, and machining the first positioning edge (8-1) and the second positioning edge (8-2) according to the characteristic dimensions measured in step 1).

Citation Information

Patent Citations

  • Intermediate casing ring repairing method

    CN104476096A

  • Maintenance method for stator supporting ring of aeronautical auxiliary power unit

    CN107617851A

  • Repair method for installation edge cracks of bearing frame of inclined support plate

    CN111940993A

  • Argon arc welding repair deformation control method for thin-wall casing assembly

    CN115555687A

  • Gas turbine engine transition liner assembly and repair

    US20040088988A1