Preparation method of high-capacity shell of water-based lithium battery

Through the preparation method of aqueous lithium battery shell, the stress characteristics and welding technology of iron sheets are used to solve the problems of lithium battery shell in environmental protection and use, and the efficient sealing and thermal performance of the shell is achieved, ensuring the battery Safety and reliability.

CN119017019APending Publication Date: 2024-11-26ORIENTAL SMART LION ENERGY STORAGE BATTERY LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411174406.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The lithium battery case has high environmental requirements during processing, storage and use, and the prior art is difficult to ensure its protective effect, especially under the chemical properties of highly reactive lithium metal.

Method used

The large-capacity shell preparation method of aqueous lithium batteries includes bending the iron sheet into a cylindrical structure, forming a square cylinder structure through the inner support and the outer clamp, and conducting welding, grinding, sealing, sealing and thermal performance testing, and Coat the insulating corrosion-resistant coating on the surface.

Benefits of technology

The stress of the iron sheet is better, weld cracks are avoided, heat dissipation effect is enhanced, the sealing and thermal performance of the shell are ensured, and the safety and reliability of the battery are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119017019A_ABST
    Figure CN119017019A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-capacity shell of a water-based lithium battery, and the preparation method comprises the steps of shell preparation, shell welding seam detection, shell polishing and cleaning, shell leakproofness detection, shell thermal performance detection and shell coating, an inner supporting piece is matched with an outer clamping piece to support the iron sheet of the cylindrical structure into a square cylinder structure, a plurality of strip-shaped ribs arranged at intervals are arranged on the surface of the inner supporting piece, the inner supporting piece supports the iron sheet of the cylindrical structure into the square cylinder structure with rib grooves in the outer surface through two times of inner supporting, and then the connector of the square cylinder structure is welded. According to the invention, the iron sheet is used as a material for forming the shell instead of a cast iron shell because the stress of the iron sheet is better; the iron sheet is firstly internally supported and then is welded, so that the iron sheet can be better prevented from having better deformation quantity in the internal supporting process, and the condition that a weld seam is easy to crack when the internal support is firstly welded is further avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of aqueous lithium batteries, and in particular relates to a method for preparing a large-capacity shell of an aqueous lithium battery. Background Art

[0002] Lithium batteries are a type of battery that uses lithium metal or lithium alloy as the positive (negative) electrode material and a non-aqueous electrolyte solution. Lithium-ion batteries have been widely used in various scenarios in our lives, such as smartphones, laptops, electric vehicles, electric bicycles, medical fields and other fields. The development of lithium-ion battery technology has made various devices so integrated into people's lives. It not only facilitates people's lives, but is also a tool with a significant impact on changing the state of society.

[0003] However, due to the very active chemical properties of lithium metal, the processing, storage and use of lithium metal have very high environmental requirements. Among them, the shell of the lithium battery is an important part of protecting the lithium battery. Therefore, this application proposes a method for preparing the shell of an aqueous lithium battery to ensure that the produced shell has a strong protective effect. Summary of the invention

[0004] The present invention provides a method for preparing a large-capacity shell of an aqueous lithium battery, which can effectively solve the above problems.

[0005] The present invention is achieved in that:

[0006] A method for preparing a large-capacity shell of an aqueous lithium battery comprises the following steps:

[0007] S1. Preparation of the shell: firstly, the iron sheet is bent into a cylindrical structure, and then the iron sheet with the cylindrical structure is supported into a square cylindrical structure by an inner support member and an outer clamp member, wherein the surface of the inner support member is provided with a plurality of strip ribs arranged at intervals, and the inner support member supports the iron sheet with the cylindrical structure into a square cylindrical structure with rib grooves on the outer surface through two inner supports, and then the interface of the square cylindrical structure is welded;

[0008] S2. Shell weld inspection: Take photos and analyze whether the shell weld is qualified through the visual component;

[0009] S3, shell grinding and cleaning: grinding and cleaning the inner and outer surfaces of the shell by a grinder;

[0010] S4, shell sealing: insert the polished shell into the top cover and the bottom plate, and perform internal welding on the top cover and the bottom plate to seal the shell;

[0011] S5. Shell tightness test: put the sealed shell into the tightness test tank for tightness test;

[0012] S6. Shell thermal performance test: dry the shell that has passed the airtightness test and then put it into the temperature control box for thermal performance test;

[0013] S7. Shell coating: The inner and outer surfaces of the shell that has passed the thermal performance test will be coated with an insulating corrosion-resistant coating.

[0014] As a further improvement, the S1 specifically includes the following steps:

[0015] S101, performing first internal support by using internal support members, that is, internally supporting the cylindrical structure into a square cylindrical structure;

[0016] S102, performing a second internal support through an internal support member, and ensuring that the offset angle at the interface of the square tube structure is less than plus or minus 3°;

[0017] S103, when the offset angle at the interface of the square tube structure meets the conditions, welding is performed on the interface of the square tube structure.

[0018] As a further improvement, the S2 comprises the following steps:

[0019] S201, acquiring an image of a weld of a shell;

[0020] S202, segmenting the acquired weld image into units to obtain a plurality of first images;

[0021] S203, performing image definition enhancement processing on a plurality of first images respectively, and obtaining second images;

[0022] S204: Perform weld detection according to the acquired second image.

[0023] As a further improvement, the weld detection specifically includes:

[0024] Performing surface defect detection on the weld according to the second image, wherein the surface defects include holes, cracks, cavitation, etc. If the surface defects are detected in the second image, the weld needs to be removed and welded again;

[0025] The vertical bending angle of the weld is analyzed according to the second image. If the vertical bending angle of the weld is greater than 5°, the weld needs to be repaired.

[0026] As a further improvement, the S5 specifically includes the following steps:

[0027] The sealed shell is placed in an airtightness detection tank, wherein an aqueous solution is contained in the airtightness detection tank, that is, a visual monitor is used to observe whether bubbles appear when the shell is slowly placed in the airtightness detection tank. If bubbles appear, the positions of the bubbles on the shell are marked. After the overall inspection of the shell is completed, the welds can be repaired according to the positions marked by the visual monitor. After the repair is completed, the shell is subjected to a second airtightness inspection.

[0028] As a further improvement, the S6 specifically includes the following steps:

[0029] First, the shell that has passed the airtightness test is dried in a drying box, and then the dried shell is placed in a temperature control box. The temperature of the temperature control box is adjusted to simulate the external high temperature situation, and then the real-time temperature inside the shell is fed back through the temperature detector inside the shell and transmitted to the processor. After receiving the feedback temperature, the processor punctuates the temperature and time, and connects each time and temperature punctuation to form a time and temperature change curve.

[0030] As a further improvement, the obtained time and temperature change curve is analyzed, the slope of each time period in the change curve is calculated, and then each group of slopes is compared with the standard value to ensure that each group of slopes is not greater than the standard value. If any group of slopes is greater than the standard value, the shell is tested multiple times in the temperature range. If the slope is still greater than the standard value, the shell is unqualified.

[0031] As a further improvement, the S7 specifically includes the following steps:

[0032] S701, placing the entire housing in an oven at a temperature of 80°C-100°C for 20min-30min;

[0033] S702, coating the inside of the shell with an insulating corrosion-resistant coating having a thickness of 40um-60um;

[0034] S703, coating the bottom plate of the housing with an insulating corrosion-resistant coating having a thickness of 80 um to 120 um;

[0035] S704, coating the top cover of the shell with an insulating corrosion-resistant coating having a thickness of 100um-140um;

[0036] S705, then place the shell in an oven at a temperature of 100°C-130°C for 2h-4h.

[0037] As a further improvement, the coating material of the insulating corrosion-resistant coating comprises 70%-80% of insulating material and 20%-30% of binder in terms of mass percentage.

[0038] As a further improvement, the insulating corrosion-resistant coating is sprayed on the shell body by thermal spraying.

[0039] The beneficial effects of the present invention are as follows: by using iron sheets as the material for shell molding instead of using cast iron shells, the stress of the iron sheets is better; secondly, by first supporting the iron sheets internally and then welding them, it is possible to better avoid the iron sheets having a greater amount of deformation during the internal support process, thereby avoiding the situation where cracks in the welds are easily caused when welding on the internal support first. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0041] Figure 1 It is a schematic diagram of the overall structure of the present invention in which the iron sheet is bent and formed into a square tube structure through internal support;

[0042] Figure 2 It is a schematic flow chart of the method of the present invention;

[0043] Reference numerals:

[0044] 1- iron sheet, 2- strip ribs, 3- interface. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the invention claimed for protection, but merely represents the selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0046] In the description of the present invention, the orientations or positional relationships indicated by terms such as "upper", "lower", "above", "both ends", etc. are based on the orientations or positional relationships shown in the accompanying drawings and are only for the convenience of describing the present invention and simplifying the description. They do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0047] Reference Figure 1-2 As shown, this embodiment provides a method for preparing a large-capacity shell of an aqueous lithium battery, comprising the following steps:

[0048] S1. Preparation of the shell: firstly, the iron sheet 1 is bent into a cylindrical structure, and then the iron sheet 1 with the cylindrical structure is supported into a square cylindrical structure by an inner support member and an outer clamp member, wherein the surface of the inner support member is provided with a plurality of strip ribs 2 arranged at intervals, and the inner support member supports the iron sheet 1 with the cylindrical structure into a square cylindrical structure with rib grooves on the outer surface through two inner supports, and then the interface 3 of the square cylindrical structure is welded;

[0049] S2. Shell weld inspection: Take photos and analyze whether the shell weld is qualified through the visual component;

[0050] S3, shell grinding and cleaning: grinding and cleaning the inner and outer surfaces of the shell by a grinder;

[0051] S4, shell sealing: insert the polished shell into the top cover and the bottom plate, and perform internal welding on the top cover and the bottom plate to seal the shell;

[0052] S5. Shell tightness test: put the sealed shell into the tightness test tank for tightness test;

[0053] S6. Shell thermal performance test: dry the shell that has passed the airtightness test and then put it into the temperature control box for thermal performance test;

[0054] S7. Shell coating: The inner and outer surfaces of the shell that has passed the thermal performance test will be coated with an insulating corrosion-resistant coating.

[0055] The reason why the iron sheet 1 is used as the material for forming the shell instead of a cast iron shell is that the stress of the iron sheet 1 is better; secondly, by first supporting the iron sheet 1 internally and then welding it, it is possible to better avoid the iron sheet 1 having a greater deformation amount during the internal support process, thereby avoiding the situation where cracks in the weld are easily caused when welding on the internal support first; and by arranging strip ribs 2 on the internal support parts, the surface of the shell after forming has a plurality of strip convex grooves, which can enhance the heat dissipation effect of the shell and ensure the heat dissipation efficiency of the shell.

[0056] Furthermore, the S1 specifically includes the following steps:

[0057] S101, performing first internal support by using internal support members, that is, internally supporting the cylindrical structure into a square cylindrical structure;

[0058] S102, performing a second internal support through the internal support member, and ensuring that the offset angle of the interface 3 of the square tube structure is less than plus or minus 3°;

[0059] S103, when the offset angle of the interface 3 of the square tube structure meets the conditions, the interface 3 of the square tube structure is welded.

[0060] By ensuring that the offset angle of the interface 3 of the square tube structure is less than plus or minus 3°, the overall forming effect of the square tube structure during welding is better, and there will be no misalignment, and the occurrence of leaks or holes in the weld is reduced.

[0061] Further, the S2 comprises the following steps:

[0062] S201, acquiring an image of a weld of a shell;

[0063] S202, segmenting the acquired weld image into units to obtain a plurality of first images;

[0064] S203, performing image definition enhancement processing on a plurality of first images respectively, and obtaining second images;

[0065] S204: Perform weld detection according to the acquired second image.

[0066] Furthermore, the weld detection specifically includes:

[0067] Performing surface defect detection on the weld according to the second image, wherein the surface defects include holes, cracks, cavitation, etc. If the surface defects are detected in the second image, the weld needs to be removed and welded again;

[0068] The vertical bending angle of the weld is analyzed according to the second image. If the vertical bending angle of the weld is greater than 5°, the weld needs to be repaired.

[0069] By performing unit segmentation on the acquired weld image, that is, dividing the entire weld image into several small parts, and then performing image clarity enhancement processing, the monitoring component can more accurately and clearly detect whether there are surface defects in the weld, avoiding the problem of missed detection or fuzzy detection by the monitoring component; by ensuring that the vertical bending angle of the weld is not greater than 5°, the aesthetic appearance of the weld can be guaranteed, that is, the overall aesthetics of the shell.

[0070] Furthermore, the S5 specifically includes the following steps:

[0071] The sealed shell is placed in an airtightness detection tank, wherein an aqueous solution is contained in the airtightness detection tank, that is, a visual monitor is used to observe whether bubbles appear when the shell is slowly placed in the airtightness detection tank. If bubbles appear, the positions of the bubbles on the shell are marked. After the overall inspection of the shell is completed, the welds can be repaired according to the positions marked by the visual monitor. After the repair is completed, the shell is subjected to a second airtightness inspection.

[0072] The tightness test ensures the tightness of the shell, thus avoiding subsequent leakage of the product.

[0073] The visual monitor mentioned in this embodiment is an existing product, wherein the visual detector can be a camera, a video camera, etc. The above-mentioned visual monitor only plays the role of bubble monitoring. When bubbles appear, the visual monitor sends a signal to the position marker located in the airtightness detection groove. The position marker can mark the position where the bubbles appear in the shell detected by the visual monitor and record it, and finally feed back the recorded data to the display screen, thereby providing workers with the ability to inspect and repair the shell according to the punctuation displayed on the display screen.

[0074] Furthermore, the S6 specifically includes the following steps:

[0075] First, the shell that has passed the airtightness test is dried in a drying box, and then the dried shell is placed in a temperature control box. The temperature of the temperature control box is adjusted to simulate the external high temperature situation, and then the real-time temperature inside the shell is fed back through the temperature detector inside the shell and transmitted to the processor. After receiving the feedback temperature, the processor punctuates the temperature and time, and connects each time and temperature punctuation to form a time and temperature change curve.

[0076] Furthermore, based on the obtained time and temperature change curve, the slope of each time period in the change curve is calculated, and then each group of slopes is compared with the standard value to ensure that each group of slopes is not greater than the standard value. If any group of slopes is greater than the standard value, the shell is tested multiple times in the temperature range. If the slope is still greater than the standard value, the shell is unqualified.

[0077] By using a temperature control box to simulate the external ambient temperature and recording the shell temperature change curve within a certain period of time in temperature control boxes with different temperatures, we can know the temperature change of the shell as a whole at different temperatures, ensure that the shell will not suddenly heat up or cool down under the influence of the external temperature, and ensure the stability of the temperature change inside the shell, that is, ensure that the solution inside the shell will not change rapidly due to the influence of the external temperature.

[0078] Furthermore, the S7 specifically includes the following steps:

[0079] S701, placing the entire housing in an oven at a temperature of 80°C-100°C for 20min-30min;

[0080] S702, coating the inside of the shell with an insulating corrosion-resistant coating having a thickness of 40um-60um;

[0081] S703, coating the bottom plate of the housing with an insulating corrosion-resistant coating having a thickness of 80 um to 120 um;

[0082] S704, coating the top cover of the shell with an insulating corrosion-resistant coating having a thickness of 100um-140um;

[0083] S705, then place the shell in an oven at a temperature of 100°C-130°C for 2h-4h.

[0084] The insulating corrosion-resistant coating comprises 70%-80% of insulating material and 20%-30% of adhesive in terms of mass percentage, and the insulating corrosion-resistant coating is sprayed on the shell body by thermal spraying.

[0085] By coating the inside of the shell with an insulating corrosion-resistant coating, that is, the insulating corrosion-resistant coating can isolate the ion path between the shell and the electrode, preventing corrosion from occurring when the negative electrode and the shell are accidentally connected, thereby effectively improving the safety and reliability of the battery cell.

[0086] In this embodiment, the coating of the insulating corrosion-resistant coating includes 70%-80% of insulating material and 20%-30% of binder in terms of mass percentage. The insulating material is one or more of PET, polyamide epoxy resin, phenol-formaldehyde resin, alkyd resin, chlorinated rubber, vinyl resin, polyaniline, and polyurethane; the binder is one of PTFE emulsion and PVDF emulsion.

[0087] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing a large-capacity shell of an aqueous lithium battery, characterized in that: The following steps are involved: S1. Preparation of the shell: firstly, the iron sheet is bent into a cylindrical structure, and then the iron sheet with the cylindrical structure is supported into a square cylindrical structure by an inner support member and an outer clamp member, wherein the surface of the inner support member is provided with a plurality of strip ribs arranged at intervals, and the inner support member supports the iron sheet with the cylindrical structure into a square cylindrical structure with rib grooves on the outer surface through two inner supports, and then the interface of the square cylindrical structure is welded; S2. Shell weld inspection: Take photos and analyze whether the shell weld is qualified through the visual component; S3, shell grinding and cleaning: grinding and cleaning the inner and outer surfaces of the shell by a grinder; S4, shell sealing: insert the polished shell into the top cover and the bottom plate, and perform internal welding on the top cover and the bottom plate to seal the shell; S5. Shell tightness test: put the sealed shell into the tightness test tank for tightness test; S6. Shell thermal performance test: dry the shell that has passed the airtightness test and then put it into the temperature control box for thermal performance test; S7. Shell coating: The inner and outer surfaces of the shell that has passed the thermal performance test will be coated with an insulating corrosion-resistant coating.

2. The method for preparing a large-capacity shell of an aqueous lithium battery according to claim 1, characterized in that: The S1 specifically includes the following steps: S101, performing first internal support by using internal support members, that is, internally supporting the cylindrical structure into a square cylindrical structure; S102, performing a second internal support through an internal support member, and ensuring that the offset angle at the interface of the square tube structure is less than plus or minus 3°; S103, when the offset angle at the interface of the square tube structure meets the conditions, welding is performed on the interface of the square tube structure.

3. The method for preparing a large-capacity shell of an aqueous lithium battery according to claim 1, characterized in that: The S2 comprises the following steps: S201, acquiring an image of a weld of a shell; S202, segmenting the acquired weld image into units to obtain a plurality of first images; S203, performing image definition enhancement processing on a plurality of first images respectively, and obtaining second images; S204: Perform weld detection according to the acquired second image.

4. The method for preparing a large-capacity shell of an aqueous lithium battery according to claim 1, characterized in that: The weld detection specifically includes: Performing surface defect detection on the weld according to the second image, wherein the surface defects include holes, cracks, cavitation, etc. If the surface defects are detected in the second image, the weld needs to be removed and welded again; The vertical bending angle of the weld is analyzed according to the second image. If the vertical bending angle of the weld is greater than 5°, the weld needs to be repaired.

5. The method for preparing a large-capacity shell of an aqueous lithium battery according to claim 1, characterized in that: The S5 specifically includes the following steps: The sealed shell is placed in an airtightness detection tank, wherein an aqueous solution is contained in the airtightness detection tank, that is, a visual monitor is used to observe whether bubbles appear when the shell is slowly placed in the airtightness detection tank. If bubbles appear, the positions of the bubbles on the shell are marked. After the overall inspection of the shell is completed, the welds can be repaired according to the positions marked by the visual monitor. After the repair is completed, the shell is subjected to a second airtightness inspection.

6. The method for preparing a large-capacity shell of an aqueous lithium battery according to claim 1, characterized in that: The S6 specifically comprises the following steps: First, the shell that has passed the airtightness test is dried in a drying box, and then the dried shell is placed in a temperature control box. The temperature of the temperature control box is adjusted to simulate the external high temperature situation, and then the real-time temperature inside the shell is fed back through the temperature detector inside the shell and transmitted to the processor. After receiving the feedback temperature, the processor punctuates the temperature and time, and connects each time and temperature punctuation to form a time and temperature change curve.

7. The method for preparing a large-capacity shell of an aqueous lithium battery according to claim 6, characterized in that: According to the obtained time and temperature change curve, the slope of each time period in the change curve is analyzed, and then each group of slopes is compared with the standard value to ensure that each group of slopes is not greater than the standard value. If any group of slopes is greater than the standard value, the shell is tested in the temperature section multiple times. If the slope is still greater than the standard value, the shell is unqualified.

8. The method for preparing a large-capacity shell of an aqueous lithium battery according to claim 1, characterized in that: The S7 specifically comprises the following steps: S701, placing the entire housing in an oven at a temperature of 80°C-100°C for 20min-30min; S702, coating the inside of the shell with an insulating corrosion-resistant coating having a thickness of 40um-60um; S703, coating the bottom plate of the housing with an insulating corrosion-resistant coating having a thickness of 80 um to 120 um; S704, coating the top cover of the shell with an insulating corrosion-resistant coating having a thickness of 100um-140um; S705, then place the shell in an oven at a temperature of 100°C-130°C for 2h-4h.

9. The method for preparing a large-capacity shell of an aqueous lithium battery according to claim 8, characterized in that: The coating material of the insulating corrosion-resistant coating comprises 70%-80% of insulating material and 20%-30% of adhesive according to mass percentage.

10. The method for preparing a large-capacity shell of an aqueous lithium battery according to claim 8, characterized in that: The insulating corrosion-resistant paint is sprayed on the shell body by thermal spraying.

Citation Information

Patent Citations

  • Tubular plate-type compound perfusion forming method

    CN102172811A

  • A device for separating rice field boundary concrete block from mold

    KR1020230141263A

  • Catheter device comprising a balloon catheter

    KR102466237B1