Recycling method of fiber reinforced composite solid waste
By mixing and kneading waste fiber reinforced composite materials with wood chips and thermosetting resins, new composite materials are prepared, which solves the problems of high costs and environmental pollution in the existing technology, and achieves low-cost and low-energy reuse, and has stable product performance. The intensity meets the standard.
Patent Information
- Application Number
- CN202411286063.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-26
AI Technical Summary
The existing fiber reinforced composite recycling technology has high cost, great environmental impact and complex processing process, making it difficult to effectively reduce resource waste and environmental pollution.
The discarded fiber-reinforced resin-based composite is mixed with wood chips and thermosetting resin to prepare a new composite material, and the molding is prepared through a molding mechanism to control process conditions to reduce cost and environmental risks.
It realizes low-cost and low-energy reuse of fiber-reinforced composite materials, reduces resource dependence and environmental pollution, and has stable product performance and meets the strength standards.
Smart Images

Figure FT_1 
Figure FT_2 
Figure FT_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of resource recycling and environmental protection, and in particular relates to a method for recycling solid waste of fiber-reinforced composite materials. Background Art
[0002] Fiber reinforced composite materials are structural materials, usually composed of fibers and matrix. The fibers can be carbon fibers, glass fibers, aramid fibers, etc., while the matrix is usually resin or metal. This material is widely used in aerospace, automotive industry, construction industry, sports equipment and other fields due to its excellent properties such as high strength, light weight and corrosion resistance.
[0003] In actual application, fiber-reinforced composite materials often generate waste due to damage, aging or design changes. If these wastes are not effectively handled, they may lead to serious waste of resources and environmental pollution. Therefore, the recycling and reuse of composite materials has become particularly important.
[0004] At present, patent documents such as application publication numbers CN118325188A and CN118290816A have proposed different recycling methods. Among them, CN118325188A discloses the use of plasma high-temperature cracking technology to recover fiber reinforcement from waste carbon fiber composites, while CN118290816A introduces the use of a solubilizer to dissolve the resin in a polyaryletherketone resin-based composite material to recover and recycle polyaryletherketone and reinforcing fibers. However, the above two recycling technologies are usually costly, and the separation, treatment and reuse processes involved require special equipment and technology. In addition, these methods use chemical solvents or pyrolysis technology to decompose the resin matrix, which may have a negative impact on the environment, and the treatment process is often complicated and energy-intensive.
[0005] Therefore, there is an urgent need for an innovative recycling method that can reprocess discarded fiber-reinforced composites into new composites and apply them in the field of pallet load-bearing, etc.; this can not only reduce resource waste, but also reduce the production cost and energy consumption of new materials. In addition, effective recycling technology can also help reduce environmental pollution and protect the health of the ecosystem. Summary of the invention
[0006] The purpose of the present invention is to solve the problems existing in the prior art and provide a method for recycling solid waste of fiber-reinforced composite materials. By mixing and kneading waste powder with a certain humidity with wood chips and thermosetting resin to regenerate new composite materials, the cost of waste treatment and disposal is reduced, the dependence on natural resources is reduced, and the risk of environmental pollution is reduced, which has significant economic and environmental benefits.
[0007] To achieve the above object, the present invention adopts the following technical solution: A method for recycling fiber reinforced composite solid waste, comprising the following steps: S1. Preliminary screening of discarded fiber-reinforced resin-based composite solid waste, washing at an ambient temperature of 30°C for 0.5-1h, and then classifying and removing surface impurities and non-target substances; S2, drying the classified solid waste, and crushing the dried solid waste into waste powder with a length of 1 to 2.5 cm; S3, drying the crushed waste powder at an ambient temperature of 80-100°C for 1-2 hours, controlling its moisture content at 4-6%; S4, mixing the dried waste powder with sawdust, wherein the mixing ratio of the waste powder to the sawdust is 1:0~1; S5. Add thermosetting resin during the mixing of waste powder and wood chips and knead for 2 to 5 minutes, wherein the thermosetting resin accounts for 5 to 20% of the total weight of the kneaded mixture, and prepare the kneaded mixture into a new composite material using a molding machine.
[0008] In the step S1, clean water is used to remove surface stains, and solid waste is classified according to the preparation process, including FRP pultrusion waste, molding waste and winding waste.
[0009] In step S2, the moisture content of the solid waste after drying is between 10% and 15%.
[0010] In step S4, the waste powder and the wood chips are mixed by a mixer, the mixer speed is 30-40 r / min, and the mixing time is 10-20 min.
[0011] In the step S5, the thermosetting resin is polyurethane resin.
[0012] In step S5, the preparation process of the new composite material is: the mixed material is pressed for 140-150 seconds under a 1600 t molding machine at a pressure of 20 MPa and a temperature of 145-155° C., and then allowed to cool naturally to solidify and form.
[0013] The beneficial effects of the present invention are as follows: in the method of the present invention, waste powder with a certain humidity is mixed and kneaded with wood chips and thermosetting resin to be remade into a new composite material, thereby reducing the cost of waste treatment and disposal, reducing dependence on natural resources, and reducing the risk of environmental pollution, thereby having significant economic and environmental benefits; and the fiber-reinforced composite material recycling method has a simple process, low production cost, stable product performance, and strength that meets standards, and can truly realize the reuse of composite materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 It is a schematic diagram of the process of the present invention; Figure 2 This is a graph showing the mechanical properties test results of a product prepared in Example 1 of the present invention with a mixing ratio of waste powder to sawdust of 1:0 and a resin content of 5%; Figure 3 This is a graph showing the mechanical properties test results of a product prepared in Example 2 of the present invention with a mixing ratio of waste powder to sawdust of 1:0 and a resin content of 10%; Figure 4 This is a graph showing the mechanical properties test results of a product prepared with a mixing ratio of waste powder to sawdust of 1:0 and a resin content of 20% in Example 3 of the present invention; Figure 5 This is a graph showing the mechanical properties test results of a product prepared in Example 4 of the present invention with a mixing ratio of waste powder to sawdust of 1:1 and a resin content of 5%; Figure 6 This is a graph showing the mechanical properties test results of a product prepared in Example 5 of the present invention with a mixing ratio of waste powder to sawdust of 1:1 and a resin content of 10%; Figure 7 This is a graph showing the mechanical properties test results of a product prepared in Example 6 of the present invention with a mixing ratio of waste powder to sawdust of 1:1 and a resin content of 20%; Figure 8 This is a graph showing the mechanical properties test results of a product prepared with a mixing ratio of waste powder to wood chips of 1:1 and a resin content of 25% in Comparative Example 1 of the present invention. DETAILED DESCRIPTION
[0015] The present invention is further explained below in conjunction with the accompanying drawings and specific embodiments.
[0016] Example 1: Figure 1 As shown, the present invention provides a method for recycling fiber reinforced composite solid waste, comprising the following steps: S1. Preliminary screening of discarded fiber-reinforced resin-based composite solid waste, washing at an ambient temperature of 30°C for 0.5h, and then classification, removal of surface impurities and non-target substances, and removal and standing; use clean water to remove surface stains, and classify solid waste according to the preparation process, including FRP pultrusion waste, molding waste and winding waste.
[0017] S2. Dry the classified solid waste, and crush the dried solid waste into waste powder with a length of 1.5 cm; wherein the moisture content of the dried solid waste is below 15%.
[0018] S3. Dry the crushed waste powder at an ambient temperature of 95°C for 1 hour and control its moisture content to 4%.
[0019] S4. Mix the dried waste powder with sawdust in a ratio of 1:0. The waste powder and sawdust are mixed by a mixer with a rotating speed of 40 r / min and a mixing time of 10 min.
[0020] S5. Add polyurethane resin during the mixing of the waste powder and the sawdust and knead for 5 minutes, wherein the polyurethane resin accounts for 5% of the total weight of the kneaded mixture, and prepare the kneaded mixture into a new composite material using a molding machine.
[0021] The preparation process of the new composite material is as follows: the mixed material is pressed for 150 seconds under a 1600 t molding machine at a pressure of 20 MPa and a temperature of 150°C, and then allowed to cool naturally to solidify and form.
[0022] The mechanical properties of the prepared new composite material 1 were tested, and the results are as follows: Figure 2 shown.
[0023] Embodiment 2: The present invention provides a method for recycling fiber-reinforced composite solid waste, comprising the following steps: S1. Preliminary screening of discarded fiber-reinforced resin-based composite solid waste, washing at an ambient temperature of 30°C for 0.5h, and then classification, removal of surface impurities and non-target substances, and removal and standing; use clean water to remove surface stains, and classify solid waste according to the preparation process, including FRP pultrusion waste, molding waste and winding waste.
[0024] S2. Dry the classified solid waste, and crush the dried solid waste into waste powder with a length of 1.5 cm; wherein the moisture content of the dried solid waste is below 15%.
[0025] S3. Dry the crushed waste powder at an ambient temperature of 95°C for 1 hour and control its moisture content to 4%.
[0026] S4. Mix the dried waste powder with sawdust in a ratio of 1:0. The waste powder and sawdust are mixed by a mixer with a rotating speed of 40 r / min and a mixing time of 10 min.
[0027] S5. Add polyurethane resin during the mixing of the waste powder and the sawdust and knead for 5 minutes, wherein the polyurethane resin accounts for 10% of the total weight of the kneaded mixture, and prepare the kneaded mixture into a new composite material using a molding machine.
[0028] The preparation process of the new composite material is as follows: the mixed material is pressed for 150 seconds under a 1600 t molding machine at a pressure of 20 MPa and a temperature of 150°C, and then allowed to cool naturally to solidify and form.
[0029] The mechanical properties of the prepared new composite material 2 were tested, and the results are as follows: Figure 3 shown.
[0030] Embodiment 3: The present invention provides a method for recycling fiber-reinforced composite solid waste, comprising the following steps: S1. Preliminary screening of discarded fiber-reinforced resin-based composite solid waste, washing at an ambient temperature of 30°C for 0.5h, and then classification, removal of surface impurities and non-target substances, and removal and standing; use clean water to remove surface stains, and classify solid waste according to the preparation process, including FRP pultrusion waste, molding waste and winding waste.
[0031] S2. Dry the classified solid waste, and crush the dried solid waste into waste powder with a length of 1.5 cm; wherein the moisture content of the dried solid waste is below 15%.
[0032] S3. Dry the crushed waste powder at an ambient temperature of 95°C for 1 hour and control its moisture content to 4%.
[0033] S4. Mix the dried waste powder with sawdust in a ratio of 1:0. The waste powder and sawdust are mixed by a mixer with a rotating speed of 40 r / min and a mixing time of 10 min.
[0034] S5. Add polyurethane resin during the mixing of the waste powder and the sawdust and knead for 5 minutes, wherein the polyurethane resin accounts for 20% of the total weight of the kneaded mixture, and prepare the kneaded mixture into a new composite material using a molding machine.
[0035] The preparation process of the new composite material is as follows: the mixed material is pressed for 150 seconds under a 1600 t molding machine at a pressure of 20 MPa and a temperature of 150°C, and then allowed to cool naturally to solidify and form.
[0036] The mechanical properties of the prepared new composite material 3 were tested, and the results are as follows: Figure 4 shown.
[0037] contrast Figure 2~Figure 4 , under the condition that the mixing ratio of waste powder and sawdust is 1:0, as the polyurethane resin content increases from 5% to 20%, the tensile strength of the composite material increases from 13.74 MPa to 35.3 MPa, the flexural strength increases from 30.76 MPa to 69.12 MPa, and the flexural modulus increases from 3.43 GPa to 9.63 GPa. Therefore, it can be seen from the above experimental results that within a certain range, the resin content has a positive effect on the mechanical properties of the composite material.
[0038] Embodiment 4: The present invention provides a method for recycling fiber-reinforced composite solid waste, comprising the following steps: S1. Preliminary screening of discarded fiber-reinforced resin-based composite solid waste, washing at an ambient temperature of 30°C for 0.5h, and then classification, removal of surface impurities and non-target substances, and removal and standing; use clean water to remove surface stains, and classify solid waste according to the preparation process, including FRP pultrusion waste, molding waste and winding waste.
[0039] S2. Dry the classified solid waste, and crush the dried solid waste into waste powder with a length of 1.5 cm; wherein the moisture content of the dried solid waste is below 15%.
[0040] S3. Dry the crushed waste powder at an ambient temperature of 95°C for 1 hour and control its moisture content to 4%.
[0041] S4. Mix the dried waste powder with sawdust in a ratio of 1:1. The waste powder and sawdust are mixed by a mixer with a rotating speed of 40 r / min and a mixing time of 10 min.
[0042] S5. Add polyurethane resin during the mixing of the waste powder and the sawdust and knead for 5 minutes, wherein the polyurethane resin accounts for 5% of the total weight of the kneaded mixture, and prepare the kneaded mixture into a new composite material using a molding machine.
[0043] The preparation process of the new composite material is as follows: the mixed material is pressed for 150 seconds under a 1600 t molding machine at a pressure of 20 MPa and a temperature of 150°C, and then allowed to cool naturally to solidify and form.
[0044] The mechanical properties of the prepared new composite material 4 were tested, and the results are as follows: Figure 5 shown.
[0045] Embodiment 5: The present invention provides a method for recycling fiber-reinforced composite solid waste, comprising the following steps: S1. Preliminary screening of discarded fiber-reinforced resin-based composite solid waste, washing at an ambient temperature of 30°C for 0.5h, and then classification, removal of surface impurities and non-target substances, and removal and standing; use clean water to remove surface stains, and classify solid waste according to the preparation process, including FRP pultrusion waste, molding waste and winding waste.
[0046] S2. Dry the classified solid waste, and crush the dried solid waste into waste powder with a length of 1.5 cm; wherein the moisture content of the dried solid waste is below 15%.
[0047] S3. Dry the crushed waste powder at an ambient temperature of 95°C for 1 hour and control its moisture content to 4%.
[0048] S4. Mix the dried waste powder with sawdust in a ratio of 1:1. The waste powder and sawdust are mixed by a mixer with a rotating speed of 40 r / min and a mixing time of 10 min.
[0049] S5. Add polyurethane resin during the mixing of the waste powder and the sawdust and knead for 5 minutes, wherein the polyurethane resin accounts for 10% of the total weight of the kneaded mixture, and prepare the kneaded mixture into a new composite material using a molding machine.
[0050] The preparation process of the new composite material is as follows: the mixed material is pressed for 150 seconds under a 1600 t molding machine at a pressure of 20 MPa and a temperature of 150°C, and then allowed to cool naturally to solidify and form.
[0051] The mechanical properties of the prepared new composite material 5 were tested, and the results are as follows: Figure 6 shown.
[0052] Embodiment 6: The present invention provides a method for recycling fiber-reinforced composite solid waste, comprising the following steps: S1. Preliminary screening of discarded fiber-reinforced resin-based composite solid waste, washing at an ambient temperature of 30°C for 0.5h, and then classification, removal of surface impurities and non-target substances, and removal and standing; use clean water to remove surface stains, and classify solid waste according to the preparation process, including FRP pultrusion waste, molding waste and winding waste.
[0053] S2. Dry the classified solid waste, and crush the dried solid waste into waste powder with a length of 1.5 cm; wherein the moisture content of the dried solid waste is below 15%.
[0054] S3. Dry the crushed waste powder at an ambient temperature of 95°C for 1 hour and control its moisture content to 4%.
[0055] S4. Mix the dried waste powder with sawdust in a ratio of 1:1. The waste powder and sawdust are mixed by a mixer with a rotating speed of 40 r / min and a mixing time of 10 min.
[0056] S5. Add polyurethane resin during the mixing of the waste powder and the sawdust and knead for 5 minutes, wherein the polyurethane resin accounts for 20% of the total weight of the kneaded mixture, and prepare the kneaded mixture into a new composite material using a molding machine.
[0057] The preparation process of the new composite material is as follows: the mixed material is pressed for 150 seconds under a 1600 t molding machine at a pressure of 20 MPa and a temperature of 150°C, and then allowed to cool naturally to solidify and form.
[0058] The mechanical properties of the prepared new composite material 6 were tested, and the results are as follows: Figure 7 shown.
[0059] Comparative Example 1: A method for recycling fiber-reinforced composite solid waste, comprising the following steps: S1. Preliminary screening of discarded fiber-reinforced resin-based composite solid waste, washing at an ambient temperature of 30°C for 0.5h, and then classification, removal of surface impurities and non-target substances, and removal and standing; use clean water to remove surface stains, and classify solid waste according to the preparation process, including FRP pultrusion waste, molding waste and winding waste.
[0060] S2. Dry the classified solid waste, and crush the dried solid waste into waste powder with a length of 1.5 cm; wherein the moisture content of the dried solid waste is below 15%.
[0061] S3. Dry the crushed waste powder at an ambient temperature of 95°C for 1 hour and control its moisture content to 4%.
[0062] S4. Mix the dried waste powder with sawdust in a ratio of 1:1. The waste powder and sawdust are mixed by a mixer with a rotating speed of 40 r / min and a mixing time of 10 min.
[0063] S5. Add polyurethane resin during the mixing of the waste powder and the sawdust and knead for 5 minutes, wherein the polyurethane resin accounts for 25% of the total weight of the kneaded mixture, and prepare the kneaded mixture into a new composite material using a molding machine.
[0064] The preparation process of the new composite material is as follows: the mixed material is pressed for 150 seconds under a 1600 t molding machine at a pressure of 20 MPa and a temperature of 150°C, and then allowed to cool naturally to solidify and form.
[0065] The mechanical properties of the prepared comparative composite material 1 were tested, and the results are as follows: Figure 8 shown.
[0066] As described in Examples 4-6 and Comparative Example 1, under the condition that the mixing ratio of waste powder and sawdust is 1:1, as the polyurethane resin content increases from 5% to 20%, the tensile strength of the composite material increases from 17.1 MPa to 60.2 MPa, the flexural strength increases from 39.18 MPa to 104.03 MPa, and the flexural modulus increases from 4.07 GPa to 10.34 GPa. Therefore, it can be seen from the above experimental results that the resin content has a positive promoting effect on the mechanical properties within a certain range, and the strength of the composite material does not simply depend on the resin content, but is also affected by multiple factors such as fiber type, fiber to resin ratio, fiber arrangement and manufacturing process. Too high a resin content may lead to an insufficient fiber ratio, thereby reducing the overall strength of the material.
[0067] Finally, a composite material pallet was prepared using the waste composite material recycling process of the present invention. As shown in Figure 1, compared with the existing plastic pallets, the performance of the new composite material pallet and the existing plastic pallet standards can meet the use requirements.
[0068] Table 1 Performance comparison between plastic pallets and composite pallets In the method of the present invention, waste powder with a certain humidity is mixed and kneaded with wood chips and thermosetting resin to be remade into a new composite material, thereby reducing the cost of waste treatment and disposal, reducing dependence on natural resources, and reducing the risk of environmental pollution, thereby having significant economic and environmental benefits; and the fiber-reinforced composite material recycling method has simple process, low production cost, stable product performance, and strength that meets standards, and can truly realize the reuse of composite materials.
[0069] The above description is only used to illustrate the technical solution of the present invention rather than to limit it. Other modifications or equivalent substitutions made to the technical solution of the present invention by ordinary technicians in this field should be included in the scope of the claims of the present invention as long as they do not depart from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for recycling fiber-reinforced composite solid waste, characterized in that: The following steps are involved: S1. Preliminary screening of discarded fiber-reinforced resin-based composite solid waste, washing at an ambient temperature of 30°C for 0.5-1h, and then classifying and removing surface impurities and non-target substances; S2, drying the classified solid waste, and crushing the dried solid waste into waste powder with a length of 1 to 2.5 cm; S3, drying the crushed waste powder at an ambient temperature of 80-100°C for 1-2 hours, controlling its moisture content at 4-6%; S4, mixing the dried waste powder with sawdust, wherein the mixing ratio of the waste powder to the sawdust is 1:0~1; S5. Add thermosetting resin during the mixing of waste powder and wood chips and knead for 2 to 5 minutes, wherein the thermosetting resin accounts for 5 to 20% of the total weight of the kneaded mixture, and prepare the kneaded mixture into a new composite material using a molding machine.
2. The method for recycling fiber-reinforced composite solid waste according to claim 1, characterized in that: In the step S1, clean water is used to remove surface stains, and solid waste is classified according to the preparation process, including FRP pultrusion waste, molding waste and winding waste.
3. The method for recycling fiber-reinforced composite solid waste according to claim 1, characterized in that: In step S2, the moisture content of the solid waste after drying is between 10% and 15%.
4. The method for recycling fiber-reinforced composite solid waste according to claim 1, characterized in that: In step S4, the waste powder and the wood chips are mixed by a mixer, the mixer speed is 30-40 r / min, and the mixing time is 10-20 min.
5. The method for recycling fiber-reinforced composite solid waste according to claim 1, characterized in that: In the step S5, the thermosetting resin is polyurethane resin.
6. The method for recycling fiber-reinforced composite solid waste according to claim 1, characterized in that: In step S5, the preparation process of the new composite material is: the mixed material is pressed for 140-150 seconds under a 1600 t molding machine at a pressure of 20 MPa and a temperature of 145-155° C., and then allowed to cool naturally to solidify and form.