Preparation method of negative Poisson's ratio geotechnical reinforced material

By using thermoplastic polyurethane elastomers, spiral fibers and honeycomb microstructures in georeinforced materials, and combining 3D printing technology to prepare negative Poisson's ratio materials, the problem of insufficient cushioning performance of existing georeinforced materials has been solved, and significantly improved The seismic performance and structural stability of the embankment have improved the energy absorption and dissipation capabilities.

CN119017702AActive Publication Date: 2024-11-26HOHAI UNIV

Patent Information

Application Number
CN202410880952.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-11-26
Estimated Expiration
2044-07-02

AI Technical Summary

Technical Problem

The existing georeinforced materials have insufficient cushioning performance when facing strong dynamic loads such as earthquakes, resulting in damage to the embankment structure, especially in lateral deformation, which increases the instability and damage risk of the structure.

Method used

Thermoplastic polyurethane elastomer is used as the basic material, spiral fibers and honeycomb microstructure are added, hourglass structure is formed through foaming process, negative Poisson's ratio georectile material is prepared in combination with 3D printing technology, and water-based polyurethane protective coating is applied to the surface. , optimize the mechanical properties of the material.

Benefits of technology

It significantly improves the seismic performance and structural stability of the embankment, enhances energy absorption and dissipation capabilities through the negative Poisson ratio effect, improves the tensile strength and engineering quality of the material, and provides an efficient, durable and environmentally friendly solution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119017702A_ABST
    Figure CN119017702A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a negative Poisson's ratio geotechnical reinforced material. The preparation method comprises the following steps: S1, uniformly mixing a thermoplastic polyurethane elastomer and an additive; s2; adding two reinforcing structure units of a spiral fiber and a honeycomb micro-structure, uniformly mixing, and cooling into a solid state by adopting a foaming process; s3, preparing and forming by using a 3D printer; and S4, a protective coating is applied to the surface of the solid object, and the spraying thickness ranges from 0.5 mm to 1 mm. According to the preparation method of the material, the anti-seismic property and the structural stability of an embankment are remarkably improved, the negative Poisson's ratio effect is effectively induced, and the energy absorption and dissipation capacity is enhanced. The material performance is maximized, the construction efficiency and the engineering quality are improved, and the method is suitable for various complex terrains.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing a building material, in particular to a method for preparing a negative Poisson's ratio geotechnical reinforcement material, and belongs to the field of civil engineering material science and technology. Background Art

[0002] In current traditional embankment construction, geotechnical reinforcement materials are mainly used to improve soil stability and enhance the bearing capacity of the structure. However, when faced with strong dynamic loads such as earthquakes, the seismic absorption performance of existing materials is often not sufficient to effectively resist lateral deformation, resulting in damage to the embankment structure.

[0003] Poisson's ratio refers to the ratio of the vertical strain to the principal strain when the material is stretched or compressed in one direction. The Poisson's ratio of most traditional materials is positive. When encountering strong dynamic loads such as earthquakes, materials with positive Poisson's ratio tend to produce significant lateral deformation in addition to the longitudinal force direction. This lateral expansion or contraction not only cannot effectively resist the lateral force caused by the earthquake, but may also increase the instability and damage risk of the structure. On the contrary, negative Poisson's ratio materials can exhibit unique lateral compression characteristics when subjected to force, which makes them show great potential in absorbing and dissipating seismic energy and reducing structural deformation. Therefore, there is an urgent need to prepare a special building buffer material with a negative Poisson's ratio. Summary of the invention

[0004] In view of the problems existing in the above-mentioned prior art, the purpose of the present invention is to provide a method for preparing a negative Poisson's ratio geotechnical reinforcement material to solve the problem of insufficient shock absorbing performance of the existing materials.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] A method for preparing a negative Poisson's ratio geotechnical reinforcement material comprises the following steps:

[0007] S1: Under the reaction conditions of temperature 180-230°C and pressure 0.3-2Mpa, thermoplastic polyurethane elastomer (TPU) is used as the basic polymer matrix material, and additives in a mass ratio of 2%-5% are added and mixed evenly;

[0008] S2: Add two reinforcing structural units, spiral fibers and honeycomb microstructures, to the mixture obtained in S1 and mix them evenly, wherein the mass proportion of thermoplastic polyurethane elastomer is 70%-80%, and the mass proportions of the spiral fibers and honeycomb microstructures are 10%-15% respectively, and a foaming process is adopted to form a honeycomb structure with cavities inside the mixture, and the mixture becomes solid when cooled to room temperature, and the internal spaces of the material are designed to be an hourglass structure, with wider ends and a narrower middle connecting part;

[0009] S3: Preparation and molding using a 3D printer;

[0010] S4: After cooling and curing, a protective coating is applied on the surface of the solid object. A water-based polyurethane protective coating is selected and a high-pressure airless spraying method is adopted. After coating, it is dried under natural conditions or heated in an oven to accelerate the curing process. The spraying thickness is between 0.5-1mm.

[0011] Preferably, the mass ratio of the spiral fibers and the honeycomb microstructure is 1:1.

[0012] Preferably, the two reinforcing structural units of the spiral fiber and the honeycomb microstructure use one or more of polylactic acid (PLA), thermoplastic liquid crystal polymer (TLCP), carbon nanotubes (CNTs), polyurethane foam (PU), and bio-based fibers.

[0013] Preferably, the additives include one or more of a coupling agent, an antioxidant, a plasticizer, an antibacterial agent and an antifungal agent.

[0014] Preferably, the components of the waterborne polyurethane protective coating in S4 include 50% waterborne polyurethane resin, 8% film-forming aid, 7% hydrolyzed isocyanate cross-linking agent, 5% auxiliary additives, and the rest is distilled water.

[0015] The beneficial effects of the preparation method of the present invention are:

[0016] The material preparation method of the present invention significantly improves the seismic performance and structural stability of the embankment. The hourglass-shaped space design of the material optimizes the stress distribution, effectively induces the negative Poisson's ratio effect, and enhances the energy absorption and dissipation capacity. Environmentally friendly TPU is used as the substrate, and multiple reinforcement units are integrated to ensure material performance and environmental protection. The precise molding using 3D printing technology and the method of fine construction ensure that the material performance is maximized, the construction efficiency and engineering quality are improved, and it is suitable for a variety of complex terrains. It provides an efficient, durable and environmentally friendly solution for embankment construction and promotes technological progress in the field of civil engineering. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a three-dimensional image of negative Poisson's ratio geotechnical reinforcement material;

[0018] Figure 2 It is the plane dimension diagram of negative Poisson's ratio geotechnical reinforcement material;

[0019] Figure 3 , 4 This is the test data diagram of the proportion of negative Poisson's ratio geotechnical reinforcement materials;

[0020] Figure 5 This is the negative Poisson's ratio effect curve of this negative Poisson's ratio geotechnical reinforcement material. DETAILED DESCRIPTION

[0021] The present invention will be further described in detail below in conjunction with the accompanying drawings.

[0022] A method for preparing a negative Poisson's ratio geotechnical reinforcement material comprises the following steps:

[0023] S1: Under the reaction conditions of temperature 180-230°C and pressure 0.3-2Mpa, thermoplastic polyurethane elastomer (TPU) is used as the basic polymer matrix material, and additives in a mass ratio of 2%-5% are added and mixed evenly. In order to improve the toughness of the mixture and improve the compressive performance, the additives can be selected from one or more of coupling agents, antioxidants, plasticizers, antibacterial agents and antifungal agents.

[0024] S2: Add two reinforcing structural units, spiral fibers and honeycomb microstructures, to the mixture obtained in S1 and mix them evenly. As the most preferred solution, the two reinforcing structural units, spiral fibers and honeycomb microstructures, use one or more of polylactic acid (PLA), thermoplastic liquid crystal polymer (TLCP), carbon nanotubes (CNTs), polyurethane foam (PU), and bio-based fibers. The mass proportion of thermoplastic polyurethane elastomer is 70%-80%, and the mass proportion of the spiral fibers and honeycomb microstructures is 10%-15% respectively. The foaming process is used to form a honeycomb structure with cavities inside the mixture, and it becomes solid when cooled to room temperature. The space inside the material is designed to be an hourglass structure, with wider ends and a narrower middle connecting part, such as Figure 1 , 2 shown.

[0025] S3: Preparation and molding using a 3D printer;

[0026] S4: After cooling and curing, a protective coating is applied to the surface of the solid object. A water-based polyurethane protective coating is selected and a high-pressure airless spray method is adopted. After coating, it is dried under natural conditions or heated in an oven to accelerate the curing process. The spraying thickness is between 0.5-1mm. At the same time, from the perspective of improving the mechanical properties of the coating surface, the weight proportion of each component of the water-based polyurethane protective coating includes 50% water-based polyurethane resin, 8% film-forming aid, 7% hydrolyzed isocyanate cross-linking agent, 5% auxiliary additives, and the rest is distilled water.

[0027] The process of high-pressure airless spraying generally includes:

[0028] 1. Surface pretreatment: Use a suitable detergent to clean the grille surface to remove all dirt, grease and loose particles. If necessary, light grinding can be performed to increase the surface roughness and improve the adhesion of the paint.

[0029] 2. Primer coating: Apply a layer of primer before formally applying TPU-compatible waterborne polyurethane protective coating to further enhance the bonding between the coating and the substrate and provide additional anti-corrosion protection.

[0030] 3. Multi-layer spraying: Use two or more coating systems to increase the protective performance. After each layer of spraying, wait for the prescribed drying time before spraying the next layer.

[0031] 4. Check the coating: After spraying, check whether the coating has defects such as missing coating, sagging, orange peel, etc., and repair them in time.

[0032] 5. Drying and curing: After coating, the coating needs to be allowed to dry naturally under natural conditions or heated in an oven to accelerate the curing process. The full curing time of TPU-compatible waterborne polyurethane protective coatings varies depending on the specific product and thickness, generally ranging from a few hours to a few days.

[0033] like Figure 3 As shown in the figure, under the conditions of mixing temperature of 200°C and pressure of 0.5MkPa, the tensile performance curve of the mixed material when the ratio of the two reinforcing unit materials is 1:1 is taken as the unit tensile strength. When the content of the reinforcing unit material gradually increases, the tensile properties of the composite material first increase and then decrease. When the content of the reinforcing unit material is within 30%, the tensile strength of the material is better, which is greater than that of the raw material.

[0034] like Figure 4 As shown in the figure, under the conditions of mixing temperature of 200°C and pressure of 0.5MkPa, the tensile performance curve of the material is when the content of the base material TPU is 80%. The tensile strength when the two reinforcing unit materials are added in a ratio of 1:1 is taken as the unit tensile strength. When the spiral fiber content is higher, the tensile strength of the material is higher.

[0035] like Figure 5 As shown in the figure, under the conditions of mixing temperature of 200°C and pressure of 0.5MkPa, the negative Poisson's ratio effect curve of the material is when the addition amount of the base material TPU is 80%. The negative Poisson's ratio effect when the addition ratio of the two reinforcing unit materials is 1:1 is taken as the unit negative Poisson's ratio effect. When the dosage of the honeycomb microstructure is large, the negative Poisson's ratio effect is better.

[0036] In order to achieve a balance between tensile strength and negative Poisson's ratio effect, the content of the two reinforcing structural units should be 1:1. The content of various materials can be adjusted under different mixing conditions and different applicable requirements.

[0037] When seismic waves are transmitted to the structure, negative Poisson's ratio materials can effectively limit the lateral displacement of the structure through their lateral compression characteristics, reduce the lateral deformation caused by the earthquake, and thus protect the main structure from serious damage. This ability not only reduces the risk of immediate structural damage, but also improves the long-term structural stability and durability. In addition, negative Poisson's ratio materials can help disperse and relieve stress concentration, further enhancing the toughness of the entire structural system. Through its unique mechanical response mechanism, negative Poisson's ratio materials overcome some fundamental defects of positive Poisson's ratio materials in dealing with complex dynamic loads, and provide new solutions for improving the safety and reliability of infrastructure such as embankments and bridges under extreme conditions.

Claims

1. A method for preparing a negative Poisson's ratio geotechnical reinforcement material, characterized in that: The following steps are involved: S1: Under the reaction conditions of temperature 180-230°C and pressure 0.3-2Mpa, thermoplastic polyurethane elastomer (TPU) is used as the basic polymer matrix material, and additives in a mass ratio of 2%-5% are added and mixed evenly; S2: Add two reinforcing structural units, spiral fibers and honeycomb microstructures, to the mixture obtained in S1 and mix them evenly, wherein the mass proportion of thermoplastic polyurethane elastomer is 70%-80%, and the mass proportions of the spiral fibers and honeycomb microstructures are 10%-15% respectively, and a foaming process is adopted to form a honeycomb structure with cavities inside the mixture, and the mixture becomes solid when cooled to room temperature, and the internal spaces of the material are designed to be an hourglass structure, with wider ends and a narrower middle connecting part; S3: Preparation and molding using a 3D printer; S4: After cooling and curing, a protective coating is applied on the surface of the solid object. A water-based polyurethane protective coating is selected and a high-pressure airless spraying method is adopted. After coating, it is dried under natural conditions or heated in an oven to accelerate the curing process. The spraying thickness is between 0.5-1mm.

2. The method for preparing a negative Poisson's ratio geotechnical reinforcement material according to claim 1, characterized in that: The mass ratio of the spiral fiber and the honeycomb microstructure is 1:

1.

3. The method for preparing a negative Poisson's ratio geotechnical reinforcement material according to claim 1, characterized in that: The two reinforcing structural units of spiral fiber and honeycomb microstructure use one or more of polylactic acid (PLA), thermoplastic liquid crystal polymer (TLCP), carbon nanotubes (CNTs), polyurethane foam (PU), and bio-based fibers.

4. The method for preparing a negative Poisson's ratio geotechnical reinforcement material according to claim 1 or 2, characterized in that: The additives include one or more of coupling agents, antioxidants, plasticizers, antibacterial agents and antifungal agents.

5. The method for preparing a negative Poisson's ratio geotechnical reinforcement material according to claim 1 or 2, characterized in that: The components of the waterborne polyurethane protective coating described in S4 include 50% waterborne polyurethane resin, 8% film-forming aid, 7% hydrolyzed isocyanate cross-linking agent, 5% auxiliary additives, and the rest is distilled water.

Citation Information

Patent Citations

  • Preparation method of polyurethane elastomer composite material with negative Poisson's ratio property

    CN115584120A

  • Aseismatic reinforcing material, its manufacturing method and aseismatic structure

    JP2007277886A

Cited By

  • Negative Poisson's ratio geotechnical metamaterial structure of bionic muscle fiber and preparation method of negative Poisson's ratio geotechnical metamaterial structure

    CN120206901A