Preparation method of rod-like potassium titanium phosphate negative electrode material and potassium ion battery
By adding metal complex adsorbent and titanium phosphate to the carbon nanotubes, the rod-shaped titanium phosphate potassium material is solved, and the high magnification and cycling performance of potassium ion battery materials are achieved.
Patent Information
- Application Number
- CN202410721611.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-05
- Publication Date
- 2024-11-26
AI Technical Summary
It is difficult to develop a potassium ion battery material with a stable structure that can provide inlet and exit channels for potassium ions and has excellent longitudinal conductivity, resulting in poor magnification and cycling performance of the potassium ion battery.
Using the preparation method of rod-shaped potassium titanium phosphate negative electrode material, by adding metal complex adsorbent and titanium phosphate on the basis of carbon nanotubes, ultrasonic dispersion, spray drying and high-temperature sintering, forming rod-shaped potassium titanium phosphate material with excellent conductivity .
It achieves excellent magnification and cycling performance of potassium ion batteries, has stable material structure, strong longitudinal conductivity, short ion transmission distance in vertical direction, and no additional carbon source is required, which is low cost.
Smart Images

Figure CN119018868A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of potassium ion battery materials, and particularly relates to a preparation method of a rod-shaped potassium titanium phosphate negative electrode material and a potassium ion battery. Background Art
[0002] Energy issues have always been one of the focuses of global attention. With the rapid development of the economy and the continuous growth of the population, the demand for energy has also increased. Renewable energy such as solar energy and wind energy are unstable, so equipment that can store and release energy is needed, which has promoted the development of energy storage batteries.
[0003] Although lithium-ion batteries have been widely used, lithium resources are limited and expensive, far from meeting the growing energy demand of mankind. Therefore, exploring new resource energy storage technologies has become the focus and breakthrough direction of academic research. Compared with lithium, potassium is more abundant and is in the same main group with similar chemical properties. Potassium-ion batteries have application prospects as energy storage batteries.
[0004] In technological applications, due to the large radius of potassium ions, many traditional battery materials cannot embed and extract potassium ions in electrochemical reactions. Therefore, it is extremely important to develop a material that can provide entry and exit channels for potassium ions and has advantages such as stable structure and high specific capacity. Summary of the invention
[0005] In view of the problems existing in the prior art, the object of the present invention is to provide a preparation method of a rod-shaped potassium titanium phosphate negative electrode material and a potassium ion battery thereof. The rod-shaped potassium titanium phosphate negative electrode material of the present invention is a potassium ion superfast conductor structure, which can provide an entry and exit channel for potassium ions to embed and escape, has a stable structure, and its special rod-shaped structure has excellent longitudinal conductivity and strong ion conductivity in the vertical direction. It is applied to potassium ion batteries with excellent rate performance and cycle performance.
[0006] To achieve the above objectives, the present invention provides the following technical solutions:
[0007] A method for preparing a rod-shaped potassium titanium phosphate negative electrode material comprises the following steps:
[0008] 1) adding carbon nanotubes and metal complex adsorbent into deionized water and uniformly dispersing them by ultrasonication to obtain solution A;
[0009] 2) dispersing the titanium source in isopropanol and stirring uniformly to obtain solution B;
[0010] 3) Slowly add solution B into solution A and stir evenly to obtain solution C;
[0011] 4) adding a potassium source and phosphoric acid to solution C, stirring and dispersing them uniformly to obtain solution D, controlling the solid content to 40-60%, performing closed-loop spray drying to obtain a potassium titanium phosphate precursor, and sieving the powder;
[0012] 5) The precursor powder is heated at 750° C. in a N2 atmosphere for 8-12 h, and cooled to room temperature at a rate of 3° C. / min to obtain a rod-shaped potassium titanium phosphate material.
[0013] Preferably, the length of the rod-shaped potassium titanium phosphate is 1-10 μm, the diameter is 300-500 nm, and carbon nanotubes are distributed in the center of the rod-shaped material.
[0014] Preferably, the carbon nanotubes are multi-walled carbon nanotubes with a diameter of 2-50 nm, a length of 100-1000 nm, and a mass percentage of 5%-30%.
[0015] Preferably, the metal complex adsorbent is one or more of 2-phenylbenzimidazole, disodium phenyl dibenzimidazole tetrasulfonate, sodium ethylenediaminetetramethylenephosphate, and sodium ferric ethylenediaminetetraacetate, accounting for 2-10% by mass.
[0016] Preferably, the pH of the solution A is 3-5. Under such acidic conditions, the metal complex adsorbent has a stronger ability to complex metal ions and a larger complex stability constant.
[0017] Preferably, the titanium source is selected from one or more of titanium dioxide, titanium sulfate, tetrabutyl titanate, isopropyl titanate, and titanyl phosphate.
[0018] Preferably, the volume ratio of deionized water to isopropanol in steps 1) and 2) is 2:1.
[0019] Preferably, the potassium source is selected from one or more of potassium carbonate, potassium dihydrogen phosphate, potassium sulfate, potassium nitrate, potassium chloride and potassium acetate.
[0020] Preferably, the molar ratio of the potassium source:titanium source:phosphoric acid is 1:2:3.
[0021] Preferably, in step 4), the stirring time is 5-15 h, and the stirring speed is 500-800 r / min.
[0022] Preferably, in step 4), the inlet air temperature of the spray drying equipment is 200-220°C, the outlet air temperature is 100-115°C; the centrifugal speed is 15000-20000r / min; the tower is slightly positively pressurized, with a pressure of 50-200kPa.
[0023] The present invention also provides a potassium ion battery, wherein the rod-shaped potassium titanium phosphate negative electrode material is used as the negative electrode active material of the potassium ion battery.
[0024] Preferably, the electrolyte in the potassium ion battery includes an organic system, an aqueous system or an organic-aqueous mixed system.
[0025] The beneficial effects of the present invention are:
[0026] The potassium titanium phosphate negative electrode material prepared by the present invention is a potassium ion superfast conductor structure, which can provide channels for potassium ion insertion and extraction and has a stable structure. It has a rod-like structure, a long distance in the longitudinal direction, which is suitable for electron transmission, and can shorten the ion transmission distance in the vertical direction. It has both electronic conductivity and ionic conductivity, and has excellent rate performance and cycle performance when applied to potassium ion batteries.
[0027] The present invention uses tubular carbon nanotubes as a substrate. Under the action of a metal complexing adsorbent, a precursor material is orderly complexed and deposited around the carbon nanotubes. Under the control rate of isopropanol, a preliminary rod-shaped structure is formed. After spray drying and high-temperature sintering, a rod-shaped potassium titanium phosphate negative electrode material is prepared. In addition, the carbon nanotubes run through the interior of the material, and the material has excellent electrical conductivity without the need to add other carbon sources. The multi-walled carbon nanotubes used can increase the adhesion of the metal ion complex and are inexpensive.
[0028] The metal complexing agent used in the present invention has strong complexing and adsorption capacity of titanium and sodium metal ions, and can stably exist with carbon nanotubes. The components thereof can be removed by high-temperature calcination, so that the synthesized material is free of impurities. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is the XRD of the negative electrode material prepared in Example 1.
[0030] Figure 2 This is the SEM image of the negative electrode material prepared in Example 1.
[0031] Figure 3 This is the charge and discharge curve of the potassium ion battery prepared in Example 1.
[0032] Figure 4 The cycle performance of the potassium ion battery prepared in Example 1 (calculated based on the mass of the negative electrode active material).
[0033] Figure 5 This is the charge and discharge curve of the aqueous potassium ion battery prepared in Example 2 (calculated based on the mass of the negative electrode active material).
[0034] Figure 6 This is the cycle performance diagram of the potassium ion battery prepared in Comparative Example 1. DETAILED DESCRIPTION
[0035] In order to make the technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0036] Example 1
[0037] 20 g of multi-walled carbon nanotubes and 7 g of sodium ferric ethylenediaminetetraacetate were added into 200 ml of deionized water and uniformly dispersed by ultrasonication to obtain solution A;
[0038] Disperse 0.4 mol of nano-titanium dioxide in 100 ml of isopropanol and stir to obtain solution B;
[0039] Slowly add solution A into solution B and stir evenly to obtain solution C;
[0040] 0.1 mol potassium carbonate and 0.6 mol phosphoric acid were added to solution C, stirred and dispersed evenly, the stirring time was 10 h, the stirring speed was 600 r / min, and solution D was obtained. The solid content was controlled to be 50%, and closed spray drying was performed to obtain potassium titanium phosphate precursor. The inlet air temperature was set to 215°C, the outlet air temperature was set to 105°C, the centrifugal speed was set to 17000 r / min, the pressure in the tower was set to 100 kPa, and the powder was sieved;
[0041] The precursor powder was heated at 750° C. in a N2 atmosphere for 10 h and cooled to room temperature at a rate of 3° C. / min to obtain a rod-shaped potassium titanium phosphate material.
[0042] The materials prepared in this example were tested using relevant instruments to obtain XRD and SEM data. Figure 1 The XRD peak position corresponds perfectly to the standard card, and there is no impurity peak, which proves that the material prepared in this example is KTi2(PO4)3. Figure 2 Scanning electron microscopy test proves that the material prepared in this embodiment has a rod-like morphology and a length of 1-10 μm.
[0043] The materials prepared in the embodiment are assembled into a potassium ion battery, and the specific preparation steps are as follows: the prepared rod-shaped potassium titanium phosphate negative electrode material, conductive carbon black, and binder (SBR) are mixed in a ratio of 80:15:5, and the slurry is evenly coated on an aluminum foil as a negative electrode plate; 0.88 Mn8O 16 , conductive carbon black, and binder (PVDF) were mixed in a ratio of 80:15:5, and the slurry was coated on aluminum foil as the positive electrode. Potassium hexafluorophosphate was used as the electrolyte to prepare button cells for testing. The test current density was 100 mA / g. Figure 3 As shown in the charge and discharge curve, it can be seen that the discharge specific capacity of KTi2(PO4)3 reaches 100mAh / g, showing a relatively high specific capacity; the capacity retention rate of the battery after 100 cycles is 95.8%, and the coulombic efficiency is greater than 99%, which has excellent long-life performance. Figure 4 described.
[0044] Example 2
[0045] The preparation method of potassium titanium phosphate is consistent with that of Example 1, except that the positive electrode of the potassium ion battery adopts K2Mn(Fe(CN)6) material, the electrolyte is a 0.5M potassium sulfate aqueous solution, and the aqueous potassium ion battery is assembled for testing. The test current density is 100mA / g; the battery has a capacity retention rate of 89.6% after 100 cycles, and the coulomb efficiency is greater than 99.5%, which has excellent life performance. Figure 5 shown.
[0046] Example 3
[0047] 40 g of multi-walled carbon nanotubes and 10 g of disodium phenyl dibenzimidazole tetrasulfonate were added to 200 ml of deionized water and uniformly dispersed by ultrasonication to obtain solution A;
[0048] Disperse 0.4 mol of titanium sulfate in 100 ml of isopropanol and stir to obtain solution B;
[0049] Slowly add solution A into solution B and stir evenly to obtain solution C;
[0050] 0.1 mol of potassium dihydrogen phosphate and 0.6 mol of phosphoric acid were added to solution C, stirred and dispersed evenly, the stirring time was 8 hours, the stirring speed was 800 r / min, and solution D was obtained. The solid content was controlled to be 60%, and closed spray drying was performed to obtain potassium titanium phosphate precursor. The inlet air temperature was set to 220°C, the outlet air temperature was set to 100°C, the centrifugal speed was set to 15000 r / min, the pressure in the tower was set to 150 kPa, and the powder was sieved;
[0051] The precursor powder was heated at 750° C. in a N2 atmosphere for 10 h and cooled to room temperature at a rate of 3° C. / min to obtain a rod-shaped potassium titanium phosphate material.
[0052] Example 4
[0053] 10 g of multi-walled carbon nanotubes and 5 g of 2-phenylbenzimidazole were added into 200 ml of deionized water and uniformly dispersed by ultrasonication to obtain solution A;
[0054] Disperse 0.4 mol of tetrabutyl titanate in 100 ml of isopropanol and stir to obtain solution B;
[0055] Slowly add solution A into solution B and stir evenly to obtain solution C;
[0056] 0.1 mol potassium nitrate and 0.6 mol phosphoric acid were added to solution C, stirred and dispersed evenly, the stirring time was 15 h, the stirring speed was 500 r / min, and solution D was obtained. The solid content was controlled to be 40%, and closed spray drying was performed to obtain potassium titanium phosphate precursor. The inlet air temperature was set to 200°C, the outlet air temperature was set to 115°C, the centrifugal speed was set to 18000 r / min, the pressure in the tower was set to 50 kPa, and the powder was sieved;
[0057] The precursor powder was heated at 750° C. in a N2 atmosphere for 10 h and cooled to room temperature at a rate of 3° C. / min to obtain a rod-shaped potassium titanium phosphate material.
[0058] Comparative Example 1:
[0059] Disperse 0.4 mol of titanium dioxide in 100 ml of isopropanol and stir to obtain solution A;
[0060] 0.1 mol potassium carbonate and 0.6 mol phosphoric acid were added to solution A, stirred and dispersed evenly, the stirring time was 10 h, the stirring speed was 600 r / min, and solution B was obtained. The solid content was controlled to be 50%, and closed spray drying was performed to obtain potassium titanium phosphate precursor. The inlet air temperature was set to 215°C, the outlet air temperature was set to 105°C, the centrifugal speed was set to 17000 r / min, the pressure in the tower was set to 100 kPa, and the powder was sieved;
[0061] The precursor powder was heated at 750°C in a N2 atmosphere for 10 h and cooled to room temperature at a rate of 3°C / min to obtain a potassium titanium phosphate material having a non-rod-like morphology.
[0062] The material prepared in Comparative Example 1 was used to assemble a potassium ion battery. The specific preparation steps were as follows: the prepared rod-shaped potassium titanium phosphate negative electrode material, conductive carbon black, and binder (SBR) were mixed in a ratio of 80:15:5, and the slurry was evenly coated on an aluminum foil as a negative electrode sheet; 0.88 Mn8O 16 , conductive carbon black, and binder (PVDF) were mixed in a ratio of 80:15:5, and the slurry was coated on aluminum foil as the positive electrode. Potassium hexafluorophosphate was used as the electrolyte to prepare button batteries for testing. The test current density was 100 mA / g. The battery had a capacity retention rate of only 80.1% after 100 cycles, and a coulombic efficiency of 98%. Figure 6 As described above, the performance is worse than that of the rod-shaped potassium titanium phosphate material prepared in Example 1.
Claims
1. A method for preparing a rod-shaped potassium titanium phosphate negative electrode material, It is characterized in that The steps include: 1) adding carbon nanotubes and metal complex adsorbent into deionized water and uniformly dispersing them by ultrasonication to obtain solution A; 2) dispersing the titanium source in isopropanol and stirring uniformly to obtain solution B; 3) Slowly add solution B into solution A and stir evenly to obtain solution C; 4) adding a potassium source and phosphoric acid to solution C, stirring and dispersing them uniformly to obtain solution D, controlling the solid content to 40-60%, performing closed-loop spray drying to obtain a potassium titanium phosphate precursor, and sieving the powder; 5) Precursor powder is heated in N 2 The temperature was kept at 750°C in an atmosphere for 8-12 hours and then cooled to room temperature at a rate of 3°C / min to obtain a rod-shaped potassium titanium phosphate material.
2. The preparation method according to claim 1, It is characterized in that The length of the rod-shaped potassium titanium phosphate is 1-10 μm, the diameter is 300-500 nm, and carbon nanotubes are distributed in the center of the rod-shaped potassium titanium phosphate.
3. The preparation method according to claim 1, It is characterized in that The carbon nanotubes are multi-walled carbon nanotubes with a diameter of 2-50 nm, a length of 100-1000 nm, and a mass proportion of 5%-30%.
4. The preparation method according to claim 1, It is characterized in that The metal complex adsorbent is one or more of 2-phenylbenzimidazole, disodium phenyl dibenzimidazole tetrasulfonate, sodium ethylenediaminetetramethylenephosphate, and sodium ferric ethylenediaminetetraacetate, accounting for 2-10% by weight.
5. The preparation method according to claim 1, It is characterized in that The titanium source is selected from one or more of titanium dioxide, titanium sulfate, tetrabutyl titanate, isopropyl titanate, and titanyl phosphate; the potassium source is selected from one or more of potassium carbonate, potassium dihydrogen phosphate, potassium sulfate, potassium nitrate, potassium chloride, and potassium acetate.
6. The preparation method according to claim 1, It is characterized in that The volume ratio of deionized water to isopropanol in steps 1) and 2) is 2:1; the molar ratio of the potassium source:titanium source:phosphoric acid is 1:2:
3.
7. The preparation method according to claim 1, It is characterized in that In the step 4), the stirring time is 5-15 hours, and the stirring speed is 500-800 r / min.
8. The preparation method according to claim 1, It is characterized in that In step 4), the inlet air temperature of the spray drying equipment is 200-220° C., the outlet air temperature is 100-115° C.; the centrifugal speed is 15000-20000 r / min; and the tower is slightly positively pressurized, with a pressure of 50-200 kPa.
9. A potassium ion battery, using the rod-shaped potassium titanium phosphate negative electrode material according to any one of claims 1 to 8 as a negative electrode active material for the potassium ion battery.
10. A potassium ion battery according to claim 9, wherein the electrolyte in the potassium ion battery comprises an organic system, an aqueous system or an organic-aqueous mixed system.