Graphite crystallization and growth method of carbon material and application of graphite crystallization and growth method
By using molten salt medium under the protection of inert gas, contact between carbon materials and activated materials or electronic paths are formed, the problems of high temperature and high energy consumption and catalysts of graphite preparation are solved, and high crystallinity and low cost graphite preparation are achieved, which is suitable for multiple Domain application.
Patent Information
- Application Number
- CN202310591812.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-26
AI Technical Summary
The existing graphite preparation technology has problems such as high temperature and high energy consumption, difficult to reuse catalysts, large product sizes and unsuitable for catalytic energy storage applications, and traditional methods are difficult to effectively convert hard carbon materials.
Under the protection of inert gas, molten salts are used as a medium to form a contact between the carbon material and the activated material or an electronic pathway to perform graphite crystallization and growth of the carbon material, and control temperature and time to regulate the crystallinity and size of the product.
It has achieved graphite preparation with low energy consumption, low cost and high product crystallinity. It is suitable for structural materials, energy storage, catalysis and adsorption, and can realize continuous preparation and multi-structure selection of graphite materials.
Smart Images

Figure CN119018886A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of graphite preparation, and in particular to a graphite crystallization and growth method of a carbon material and application thereof. Background Art
[0002] Graphite materials are widely used due to their excellent physical and chemical properties. Due to the resource limitations and insufficient performance of natural graphite, people have an increasing demand for artificial graphite. At present, artificial graphite is prepared by converting amorphous carbon into graphite at high temperature, but this method requires a high temperature of up to 3000°C, a long cycle, and high energy consumption. Moreover, this method is only applicable to soft carbon raw materials, but most amorphous carbon, including renewable amorphous carbon, belongs to hard carbon materials, and it is difficult to convert it into graphite even if the heat treatment temperature continues to increase. In addition, the graphite carbon material prepared by this method is large in size, and its application in the fields of catalysis and energy storage is limited. In addition to the high temperature and high pressure method, amorphous carbon can also be catalytically converted into graphite at a lower temperature (about 1100°C) in the presence of a catalyst, such as patents US2005 / 0008562A1, CN102745677A, CN102807212A, etc. The catalytic conversion temperature is greatly reduced compared with the traditional method, but in the above method, graphite often grows around the catalyst, and the product is spiral graphite rather than flake graphite, which has a wider application demand. Moreover, the catalyst is confined in the spiral graphite, which makes it difficult to reuse the catalyst and requires cumbersome subsequent processing steps to remove it. Patent CN103510103A reports the conversion of amorphous carbon into flake graphite by electrochemical means, which has attracted widespread attention because it does not require the use of a catalyst and can operate at a lower temperature, but this method consumes a large amount of electrolysis electricity, and the electrolysis potential and electrolysis time need to be strictly controlled to take into account the crystallinity and yield of graphite. Summary of the invention
[0003] In view of the above-mentioned defects of the prior art, in the first aspect of the present invention, a method for graphite crystallization and growth of carbon materials is provided, which has the advantages of simple process, low cost and high product crystallinity, and comprises the following steps: under the protection of an inert gas, using a molten salt as a medium, contacting the carbon material with an activated material or forming an electron path, and completing the graphite crystallization and growth of the carbon material after treatment.
[0004] Preferably, the elemental composition of the salt is denoted by MX, where M represents at least one of Li, Na, K, Rb, Cs, Be, Mg, Ca, Sr, and Ba, and X represents at least one of the halogens.
[0005] Further preferably, the salt includes a halogen salt whose elemental composition is MX, and a mixture formed by the halogen salt.
[0006] Preferably, the elemental composition of the activation material is represented by M1-Y, where M1 represents at least one of Li, Na, K, Rb, Cs, Be, Mg, Ca, Sr, and Ba, and Y represents at least one of Zn, Cd, B, Al, Ga, In, Tl, C, Si, Ge, Sn, Pb, N, P, As, Sb, and Bi.
[0007] Further preferably, the activation material includes a compound with an elemental composition of M1-Y, a mixture formed by the compound, and a metal alloy with an elemental composition of M1-Y.
[0008] Preferably, the carbon material includes non-graphite structural carbon material, graphite structural carbon material, non-graphite structural carbon composite material, and graphite structural carbon composite material; the non-graphite structural carbon composite material and graphite structural carbon composite material are respectively composited by non-graphite structural carbon material, graphite structural carbon material and substance to be dispersed or precursor of substance to be dispersed.
[0009] The substance to be dispersed or the precursor of the substance to be dispersed can play a role in inducing graphite growth, thereby obtaining a one-dimensional graphite structure carbon material, such as graphite fiber, or a porous material constructed of graphite structure carbon, providing richer structural options based on the preparation of flake graphite.
[0010] Further preferably, the non-graphite structural carbon material includes at least one of biomass carbon, organic carbon, amorphous carbon, fullerene, and diamond.
[0011] The raw materials of the non-graphite structure carbon material of the present invention are widely available, among which amorphous carbon can be activated carbon, carbon black, charcoal, coke, bone char, carbon fiber, carbon tube, and amorphous carbon materials obtained by carbonization of organic matter and other preparation methods. The organic matter used for carbonization includes various agricultural and forestry crops, sediments such as petroleum and coal, artificially synthesized organic matter, and various organic solid and liquid wastes. In the present invention, the carbon material is not limited to pure substances composed of carbon elements. Carbon materials containing heteroatoms can also be converted into graphite structure carbon materials containing heteroatoms using the method provided in the first aspect of the present invention.
[0012] Further preferably, when the carbon material adopts a non-graphite structure carbon composite material or a graphite structure carbon composite material, the substance to be dispersed is at least one of a metal element, a metal alloy, and a metal carbide; the precursor of the substance to be dispersed is at least one of a metal sulfide, a metal oxide, and a metal salt.
[0013] Furthermore, when the carbon material adopts a non-graphite structure carbon composite material or a graphite structure carbon composite material, impurities formed by the substance to be dispersed or the precursor of the substance to be dispersed are removed after graphite crystallization and growth to obtain a graphite-based material; or impurities formed by the substance to be dispersed or the precursor of the substance to be dispersed are retained after graphite crystallization and growth to obtain a graphite-based composite material.
[0014] Furthermore, the metal element is at least one of Mn, Fe, Co, Ni, Cu, and Zn.
[0015] Preferably, the carbon material is contacted with the activation material in at least one of the following ways: the carbon material is contacted with the activation material dispersed in a molten salt, and the carbon material is mixed with the activation material and then immersed in a molten salt; the carbon material and the activation material form an electron path in the following way: the carbon material and the activation material are connected through a conductor and immersed in a molten salt.
[0016] Preferably, the treatment temperature is 400-1400° C., and the treatment time is 0.5-50 h.
[0017] The product with graphite structure obtained by the present invention has a size between 10nm and 100μm. The graphite crystallinity, graphite sheet thickness and lateral size of the product can be regulated by controlling the treatment temperature and time, so that non-graphite structure carbon materials can be converted into graphite structure carbon, or the size of graphite structure carbon can be grown. The dimensional size is adjustable and has broad application prospects in the fields of structural materials, energy storage, catalysis, adsorption, separation and the like.
[0018] In a second aspect of the present invention, there is provided an application of a graphite crystallization and growth method of a carbon material in the continuous preparation of a graphite material.
[0019] The specific application method includes the following steps:
[0020] After the graphite crystallization and growth of the carbon material are completed, a product with a graphite structure is recovered from the molten salt, and then a new round of carbon material is prepared and graphite crystallization and growth are carried out using the same method.
[0021] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0022] The method adopted by the invention has low energy consumption cost, simple and flexible operation, and is suitable for preparing graphite materials with high crystallinity.
[0023] The invention provides an application method for continuously preparing graphite materials, which has high yield and good application prospect of large-scale preparation. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1X-ray diffraction (XRD) test patterns of amorphous carbon XC-72 and the product obtained in Example 3;
[0025] Figure 2 This is the scanning electron microscope (SEM) test map of amorphous carbon XC-72;
[0026] Figure 3 The scanning electron microscope (SEM) test spectrum of the product obtained in Example 3;
[0027] Figure 4 The scanning electron microscope (SEM) test spectrum of the product obtained in Example 4;
[0028] Figure 5 This is a scanning electron microscope (SEM) test spectrum of the product obtained in Example 9. DETAILED DESCRIPTION
[0029] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0030] The carbon material used in the embodiment is amorphous carbon XC-72 (Carbot Corp.); the molar concentration of hydrochloric acid is 1 mol / L.
[0031] Example 1
[0032] Graphite crystallization and growth method of carbon materials:
[0033] At 950°C and under argon protection, 0.5g of calcium boride and 1.5g of amorphous carbon XC-72 were mixed and pressed into tablets, which were then wrapped with a porous metal mesh and then immersed in molten calcium chloride and kept at this temperature for 2 hours to complete the graphite crystallization and growth of the carbon material. The product was taken out and cooled to room temperature in an argon atmosphere, and the finished product was obtained after washing and drying. The finished product was characterized by X-ray diffraction. In the obtained XRD spectrum, the characteristic peaks of the finished product and Figure 1 The product spectrum is similar to that in, confirming that a product with a graphite structure is obtained.
[0034] Example 2
[0035] Graphite crystallization and growth method of carbon materials:
[0036] At 950°C and under argon protection, 0.5g of calcium carbide and 1.5g of amorphous carbon XC-72 were mixed and pressed into tablets, which were then wrapped with a porous metal mesh and then immersed in molten calcium chloride and kept at this temperature for 2 hours to complete the graphite crystallization and growth of the carbon material. The product was taken out and cooled to room temperature in an argon atmosphere, and the finished product was obtained after washing and drying. The finished product was characterized by X-ray diffraction. In the obtained XRD spectrum, the characteristic peaks of the finished product and Figure 1 The product spectrum is similar to that in, confirming that a product with a graphite structure is obtained.
[0037] Example 3
[0038] Graphite crystallization and growth method of carbon materials:
[0039] At 950°C and under argon protection, 1.5 g of calcium carbide was uniformly dispersed in 10.0 g of molten calcium chloride, and then 1.0 g of amorphous carbon XC-72 was pressed into a tablet and wrapped with a porous metal mesh and immersed in molten calcium chloride containing calcium carbide, and then heat-treated at this temperature for 2 hours to complete the graphite crystallization and growth of the carbon material. The product was taken out and cooled to room temperature in an argon atmosphere, and the finished product was obtained after washing and drying. The finished product and the amorphous carbon XC-72 raw material were characterized by X-ray diffraction. The XRD spectra of the obtained finished product and amorphous carbon XC-72 are shown in Figure 1 , Figure 1 The characteristic peaks of the finished product are consistent with those of graphite. The XRD spectrum of amorphous carbon only shows a wide and short peak package near 2θ of 25° and 44°, while the XRD spectrum of highly crystalline graphitized carbon shows a very sharp peak near 2θ of 26.4°. Figure 1 It is confirmed that after treatment, the amorphous carbon XC-72 changes from an amorphous structure to highly crystalline graphite. The microscopic morphology of the finished product and the amorphous carbon XC-72 raw material is observed by scanning electron microscopy (SEM). Figure 2 , Figure 3 As shown, amorphous carbon XC-72 particles with a particle size of about 50 nm are transformed into flake graphite after treatment.
[0040] Example 4
[0041] Graphite crystallization and growth method of carbon materials:
[0042] At 1100°C and under argon protection, 1.0g of barium carbide was uniformly dispersed in 10.0g of molten barium chloride, and then 1.0g of amorphous carbon XC-72 was pressed into a tablet and wrapped with a porous metal mesh and immersed in the molten barium chloride containing barium carbide. The tablet was kept at this temperature for 2h to complete the graphite crystallization and growth of the carbon material. The product was taken out and cooled to room temperature in an argon atmosphere. The finished product was obtained by washing and drying. The finished product was characterized by X-ray diffraction. In the obtained XRD spectrum, the characteristic peaks of the finished product and Figure 1 The product spectra are similar to those in the above, confirming that a product with a graphite structure is obtained. The microscopic morphology of the finished product was observed by scanning electron microscopy (SEM). Figure 4 It can be seen that the present embodiment obtains micrometer-sized graphite blocks.
[0043] Example 5
[0044] Graphite crystallization and growth method of carbon materials:
[0045] In the experimental group of this embodiment, under the set temperature and argon protection, 0.5 g of lithium carbide was dispersed in 10.0 g of a molten salt formed by 35% calcium chloride and 65% lithium chloride by mass, and then 1.0 g of amorphous carbon XC-72 was pressed into a tablet and wrapped with a porous metal mesh and immersed in the molten salt containing lithium carbide. The product was kept warm at the set temperature for a predetermined time to complete the graphite crystallization and growth of the carbon material. The product was taken out and cooled to room temperature in an argon atmosphere. The finished product was obtained by washing and drying. The finished product was characterized by X-ray diffraction. In the obtained XRD spectrum, the characteristic peaks of the finished product and Figure 1 The product spectrum is similar to that in, confirming that a product with a graphite structure is obtained.
[0046] Table 1: Treatment temperature and corresponding treatment time of Example 5
[0047] name Processing temperature (℃) Processing time (h) 5-1 500 10 5-2 600 5 5-3 700 2 5-4 800 1 5-5 900 0.5
[0048] The microscopic morphology of the finished product was observed by scanning electron microscopy (SEM). From the SEM spectrum, it was observed that with the increase of treatment temperature, the product grew from a few-layer graphene sheet to a nanographite sheet, confirming that the thickness of the graphite layer increased with the increase of treatment temperature.
[0049] Example 6
[0050] Graphite crystallization and growth method of carbon materials:
[0051] At 850°C and under argon protection, 1.5g of lithium nitride was uniformly dispersed in 10.0g of a molten salt formed by 35% by mass of calcium chloride and 65% by mass of lithium chloride, and then 1.0g of amorphous carbon XC-72 was pressed into a tablet and wrapped with a porous metal mesh and immersed in molten calcium chloride containing lithium nitride, and kept at this temperature for 2h to complete the graphite crystallization and growth of the carbon material, the product was taken out and cooled to room temperature in an argon atmosphere, and the finished product was obtained by washing and drying. The finished product was characterized by X-ray diffraction. In the obtained XRD spectrum, the characteristic peaks of the finished product and Figure 1 The product spectrum is similar to that in, confirming that a product with a graphite structure is obtained.
[0052] Example 7
[0053] Graphite crystallization and growth method of carbon materials:
[0054] At 850°C and under argon protection, 1.0g of calcium carbide was uniformly dispersed in 10.0g of molten salt formed by 35% calcium chloride and 65% lithium chloride by mass, and then 1.0g of sycamore charcoal, phenolic resin charcoal, and petroleum coke were pressed into tablets and wrapped with a porous metal mesh, and then immersed in the molten salt containing calcium carbide, and kept at this temperature for 2h to complete the graphite crystallization and growth of the corresponding carbon material. The product was taken out and cooled to room temperature in an argon atmosphere, and the finished product was obtained after washing and drying. The finished product was characterized by X-ray diffraction, and the characteristic peaks of different finished products in the obtained XRD spectrum were consistent with Figure 1 The product spectra are similar to those in the examples, confirming that products with graphite structures are obtained in all the examples.
[0055] Example 8
[0056] Graphite crystallization and growth method of carbon materials:
[0057] At 850°C and under argon protection, 1.0g of calcium carbide was uniformly dispersed in 10.0g of molten salt of a set ratio, and then 1.0g of amorphous carbon XC-72 was pressed into tablets and wrapped with a porous metal mesh and immersed in various molten salts containing calcium carbide. The tablets were kept at this temperature for 2h to complete the graphite crystallization and growth of the carbon material. The product was taken out and cooled to room temperature in an argon atmosphere, and the finished product was obtained after washing and drying.
[0058] Table 2: Types of molten salts used in Example 8 and their corresponding mass percentages
[0059] name Molten salt 8-1 Calcium Bromide 8-2 80% calcium fluoride + 20% lithium fluoride 8-3 75% calcium chloride + 25% potassium chloride 8-4 50% calcium chloride + 50% sodium chloride
[0060] The finished products were characterized by X-ray diffraction, and the characteristic peaks of different finished products in the obtained XRD patterns were consistent with Figure 1 The product spectra are similar to those in the examples, confirming that products with graphite structures are obtained in all the examples.
[0061] Example 9
[0062] Graphite crystallization and growth method of carbon materials:
[0063] At 850°C and under argon protection, 1.0g of calcium carbide is evenly dispersed in 10.0g of molten calcium chloride, and then 1.0g of amorphous carbon XC-72 is mixed with ferrous sulfide, iron, and nickel oxide to obtain a mixture, in which the mass of ferrous sulfide accounts for 5% of the mass of the mixture, the mass of iron accounts for 7% of the mass of the mixture, and the mass of nickel oxide accounts for 3% of the mass of the mixture; the mixture is pressed into tablets and wrapped with porous metal mesh, and then immersed in molten calcium chloride containing calcium carbide, and kept at this temperature for 2h to complete the graphite crystallization and growth of the carbon material, the product is taken out and cooled to room temperature in an argon atmosphere, and washed with water and hydrochloric acid and dried to obtain the finished product. The finished product is characterized by X-ray diffraction. In the obtained XRD spectrum, the characteristic peaks of the finished product are consistent with Figure 1 The product spectrum is similar to that in the above, confirming that a product with a graphite structure is obtained. The microscopic morphology of the finished product with 5% ferrous sulfide added was observed by scanning electron microscopy (SEM). Figure 5 It can be seen that the graphite product is in the form of fibers. In this embodiment, the product is not washed with hydrochloric acid to obtain a fiber-shaped graphite-based composite material containing iron or nickel.
[0064] Example 10
[0065] Graphite crystallization and growth methods of carbon materials:
[0066] At 850°C and under argon protection, 1.0g of calcium carbide is uniformly dispersed in 10.0g of molten calcium chloride, and then 1.0g of amorphous carbon XC-72 is mixed with nano-TiS to obtain a mixture, in which the mass of TiS accounts for 4% of the total mass of the mixture. After tableting, it is wrapped with a porous metal mesh and immersed in molten calcium chloride containing calcium carbide, and heat-treated at this temperature for 2.0h to complete the graphite crystallization and growth of amorphous carbon and the conversion of TiS to TiC. The product is taken out and cooled to room temperature in an argon atmosphere, and washed with water and dilute hydrochloric acid and dried to obtain a finished product. The dried product is tested by XRD, and the results show that the finished product is a composite material of graphite and TiC.
[0067] Embodiment 11
[0068] At 850°C and under argon protection, 1.0g of calcium carbide is uniformly dispersed in 10.0g of molten calcium chloride, and then 1.0g of amorphous carbon XC-72 is mixed with Co-Cu alloy nanopowder to obtain a mixture, in which the mass of Co-Cu alloy accounts for 8% of the total mass of the mixture. After tableting, it is wrapped with a porous metal mesh and immersed in molten calcium chloride containing calcium carbide, and heat-treated at this temperature for 2.0h to complete the graphite crystallization and growth of amorphous carbon. The product is taken out and cooled to room temperature in an argon atmosphere, and the finished product is obtained after washing with water and drying. The dried product is tested by XRD, and the results show that the finished product is a composite material of graphite and Co-Cu alloy.
[0069] Example 12
[0070] Graphite crystallization and growth method of carbon materials:
[0071] Ammonium chloroplatinate and glucose are mixed together in an atomic ratio of 1:100 between platinum and carbon, and water is added to form a solution, which is then dried at 70°C to obtain a colloid, and then the colloid is carbonized at 500°C to obtain a complex of amorphous carbon and platinum; at 850°C and under argon protection, lithium carbide is uniformly dispersed in a molten salt formed by 35% calcium chloride and 65% lithium chloride by mass, with lithium carbide accounting for 10% of the total mass of lithium carbide and the molten salt, and then the above-mentioned complex is pressed into a sheet and wrapped with a porous metal mesh, immersed in the molten salt, and kept at this temperature for 2 hours to complete the graphite crystallization and growth of the carbon material, and the product is taken out and cooled to room temperature in an argon atmosphere, and then washed with water and hydrochloric acid and dried to obtain the finished product. The finished product is characterized by X-ray diffraction, and in the obtained XRD spectrum, the characteristic peaks of the finished product are consistent with Figure 1 The product spectrum is similar to that in the above, confirming that a product with a graphite structure is obtained. The microscopic morphology of the added product was observed by scanning electron microscopy (SEM), and the SEM spectrum results showed that the product was a porous composite material constructed of platinum and graphite sheets.
[0072] Embodiment 13
[0073] Graphite crystallization and growth method of carbon materials:
[0074] At 900°C and under argon protection, 1.0g of amorphous carbon XC-72 and 1.0g of calcium chloride were mixed with 0.5g of calcium-tin alloy powder, calcium-zinc alloy powder, lithium-tin alloy powder, barium-zinc alloy powder, and sodium-tin alloy powder, respectively, and then pressed into tablets. The mixture was then kept at this temperature for 2 hours to complete the graphite crystallization and growth of the carbon material. The product was taken out and cooled to room temperature in an argon atmosphere, and the finished product was obtained after washing and drying. The finished product was characterized by X-ray diffraction. In the obtained XRD spectrum, the characteristic peaks of the finished product were consistent with Figure 1 The product spectra are similar to those in the above, confirming that products with graphite structures are obtained.
[0075] Embodiment 14
[0076] Graphite crystallization and growth method of carbon materials:
[0077] At 900℃ and under argon protection, 2.0g of calcium boride and 1.5g of amorphous carbon XC-72 were pressed into tablets, and then wrapped with porous metal mesh to obtain calcium boride test pieces and amorphous carbon test pieces. The two test pieces were then immersed in molten calcium chloride; the two test pieces were contacted by direct contact and by metal wire contact, respectively, and then kept at this temperature for 2 hours to complete the graphite crystallization and growth of the carbon material. The product was taken out and cooled to room temperature in an argon atmosphere, and the finished product was obtained after washing and drying. The finished product was characterized by X-ray diffraction. In the obtained XRD spectrum, the characteristic peaks of the finished product were consistent with Figure 1 The product spectra are similar to those in the results, confirming that products with graphite structures are obtained under different contact modes.
[0078] By simply replacing calcium boride with an equal amount of calcium carbide and using the same method to carry out graphite crystallization and growth of carbon materials, products with graphite structures can still be obtained under different contact modes.
[0079] Embodiment 15
[0080] Graphite crystallization and growth method of carbon materials:
[0081] At 1200°C and under argon protection, 1.0g of barium carbide was uniformly dispersed in 10.0g of molten barium chloride, and then 2.0g of nano-graphite was wrapped with a porous metal mesh and immersed in the molten barium chloride containing barium carbide. The temperature was kept at this temperature for 10 hours to complete the graphite crystallization and growth of the carbon material. The product was taken out and cooled to room temperature in an argon atmosphere, and the finished product was obtained by washing and drying. The microscopic morphology of the raw nano-graphite and the finished product was observed by scanning electron microscopy (SEM), and the SEM map results showed that the size of the nano-graphite increased to the micron level.
[0082] Example 16
[0083] Application of graphite crystallization and growth methods of carbon materials in continuous preparation of graphite materials:
[0084] At 850°C and under argon protection, 5.0g of calcium carbide was evenly dispersed in 50.0g of molten calcium chloride, 2.0g of amorphous carbon XC-72 was pressed into a tablet and wrapped with a porous metal mesh, and then placed in the molten calcium chloride containing calcium carbide, and kept at this temperature for 2 hours to complete the graphite crystallization and growth of the carbon material. The product was taken out and then another 2.0g of amorphous carbon XC-72 was pressed into a tablet and kept at this temperature for 2 hours. This cycle was repeated for a total of 10 batches. The products were all cooled to room temperature in an argon atmosphere, and the finished products were obtained after washing and drying. All 20.0g of amorphous carbon XC-72 can be converted into graphite products. The finished products were characterized by X-ray diffraction. In the obtained XRD spectrum, the characteristic peaks of the finished products were consistent with Figure 1The product spectrum is similar to that in the above, confirming that a product with a graphite structure is obtained. The test shows that there is still a large amount of calcium carbide left in the molten salt, indicating that amorphous carbon can continue to be converted into graphite, realizing the continuous preparation of graphite materials.
[0085] Embodiment 17
[0086] Graphite crystallization and growth method of carbon materials:
[0087] At 950°C and under argon protection, 1.0g of diamond powder and 1.0g of calcium boride were mixed evenly, pressed into tablets and wrapped with porous metal mesh, then immersed in a molten salt formed by 15% calcium fluoride and 85% potassium fluoride by mass, and kept at this temperature for 5 hours to complete the graphite crystallization and growth of the carbon material. The product was taken out and cooled to room temperature in an argon atmosphere, and the finished product was obtained after washing and drying. The finished product was characterized by X-ray diffraction. In the obtained XRD spectrum, the characteristic peaks of the finished product were consistent with Figure 1 The product spectrum is similar to that in , confirming that the diamond powder is converted into a product with a graphite structure.
[0088] Embodiment 18
[0089] Graphite crystallization and growth method of carbon materials:
[0090] At 820℃ and under argon protection, 1.0g of activated carbon and nano cobalt oxide were mixed evenly, and the atomic ratio of carbon to cobalt in the mixture was 20:1; the mixture was pressed into a sheet and wrapped with a porous metal mesh to obtain a carbon cobalt test piece, and 2.0g of calcium boride was pressed into a sheet and wrapped with a porous metal mesh to obtain a calcium boride test piece. The two test pieces were fixed in contact with the same molybdenum wire and immersed in molten calcium chloride. The temperature was kept for 2 hours to complete the graphite crystallization and growth of the carbon material. The product was taken out and cooled to room temperature in an argon atmosphere, and washed with water and hydrochloric acid and dried to obtain the finished product. The finished product was characterized by X-ray diffraction. In the obtained XRD spectrum, the characteristic peaks of the finished product were consistent with Figure 1 The product spectrum is similar to that in the above, confirming that the product has a graphite structure. The microscopic morphology of the product was observed by transmission electron microscopy (TEM), and the TEM spectrum proved that the product was in the shape of nanotubes.
[0091] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A method for crystallizing and growing graphite of a carbon material, characterized in that: The method comprises the following steps: under the protection of an inert gas, using molten salt as a medium, contacting the carbon material with the activated material or forming an electron path, and completing the graphite crystallization and growth of the carbon material after treatment.
2. The method according to claim 1, characterized in that: The elemental composition of the salt is MX, where M represents at least one of Li, Na, K, Rb, Cs, Be, Mg, Ca, Sr, and Ba, and X represents at least one of the halogens; the salt includes a halogen salt having an elemental composition of MX and a mixture formed by the halogen salt.
3. The method according to claim 1, characterized in that: The elemental composition of the activation material is denoted by M1-Y, where M1 represents at least one of Li, Na, K, Rb, Cs, Be, Mg, Ca, Sr, and Ba, and Y represents at least one of Zn, Cd, B, Al, Ga, In, Tl, C, Si, Ge, Sn, Pb, N, P, As, Sb, and Bi; the activation material includes a compound with an elemental composition of M1-Y, a mixture formed by the compound, and a metal alloy with an elemental composition of M1-Y.
4. The method according to claim 1, characterized in that: The carbon material includes non-graphite structural carbon material, graphite structural carbon material, non-graphite structural carbon composite material, and graphite structural carbon composite material; the non-graphite structural carbon composite material and graphite structural carbon composite material are respectively composited by non-graphite structural carbon material, graphite structural carbon material and a substance to be dispersed or a precursor of a substance to be dispersed.
5. The method according to claim 4, characterized in that: The non-graphite structure carbon material includes at least one of biomass carbon, organic carbon, amorphous carbon, fullerene, and diamond; when the carbon material adopts a non-graphite structure carbon composite material or a graphite structure carbon composite material, the substance to be dispersed is at least one of a metal element, a metal alloy, and a metal carbide; the precursor of the substance to be dispersed is at least one of a metal sulfide, a metal oxide, and a metal salt.
6. The method according to claim 5, characterized in that: When the carbon material adopts a non-graphite structure carbon composite material or a graphite structure carbon composite material, impurities formed by the substance to be dispersed or the precursor of the substance to be dispersed are removed after graphite crystallization and growth to obtain a graphite-based material; or impurities formed by the substance to be dispersed or the precursor of the substance to be dispersed are retained after graphite crystallization and growth to obtain a graphite-based composite material.
7. The method according to claim 5, characterized in that: The metal element is at least one of Mn, Fe, Co, Ni, Cu and Zn.
8. The method according to claim 1, characterized in that: The method of contacting the carbon material with the activation material comprises at least one of contacting the carbon material with the activation material dispersed in a molten salt and immersing the carbon material and the activation material in a molten salt after mixing; the method of forming an electron path between the carbon material and the activation material comprises connecting the carbon material and the activation material through a conductor and immersing them in a molten salt; the treatment temperature is 400 to 1400°C and the treatment time is 0.5 to 50 hours.
9. Use of the method according to any one of claims 1 to 8 in the continuous preparation of graphite materials.
10. The use according to claim 9, characterized in that: The specific method comprises the following steps: after the graphite crystallization and growth of the carbon material are completed, a product having a graphite structure is recovered from the molten salt, and then a new round of carbon material is prepared, and graphite crystallization and growth are performed using the same method.
Citation Information
Patent Citations
Collaborative graphitization method for amorphous carbon material
CN102745677A
Method for preparing graphene at low temperature
CN102807212A
Electrochemical method for converting amorphous carbon into graphite
CN103510103A
Nanostructured carbon materials having excellent crystallinity and large surface area suitable for fuel cell electrodes and method for synthesizing the same
US20050008562A1