Prussian blue analogue as well as preparation method and application thereof

By introducing Co elements and using co-precipitation method and solvothermal reaction, a low-water content of cobalt-based Prussian blue analog was prepared, which solved the problem that the electrochemical properties of the existing Prussian blue analogues were affected by crystallization water, and achieved High-efficiency application of sodium ion battery positive electrode material.

CN119018911APending Publication Date: 2024-11-26WUYI UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411272272.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The high crystal water content of existing Prussian blue analogs hinders the improvement of their electrochemical properties, and the common face-centered cubic or monoclinic structures are not suitable for the migration and storage of sodium ions.

Method used

By introducing Co elements, a cobalt-based Prussian blue analog with rhombic phase structure and low moisture content was prepared. Co-precipitation method and solvothermal reaction were used to embed organic solvents into the crystal to replace water molecules, reduce crystallization water content and improve thermal stability sex.

Benefits of technology

Cobalt-based Prussian blue analogs with excellent electrochemical properties and good cycle performance were obtained, which exhibited a flat charge and discharge curve and a wide range of application potentials for sodium ion battery positive electrode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119018911A_ABST
    Figure CN119018911A_ABST
Patent Text Reader

Abstract

The invention discloses a Prussian blue analogue as well as a preparation method and application thereof, and belongs to the technical field of material preparation. The chemical formula of the Prussian blue analogue is NaxCoy [Fe (CN) 6] z, y is larger than or equal to 0.5 and smaller than or equal to 1.2, x / y is 1.0-4.0, and z / y is 0.8-2.0. The crystal structure of the Prussian blue analogue is a rhombohedral phase. The cobalt-based Prussian blue analogue is obtained by introducing Co element, has specific chemical composition and structural characteristics, is of a rhombohedral phase structure with good reversibility and low water content, has good cycle performance and deformability, and has wide application as a sodium ion battery positive electrode material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material preparation, and in particular relates to a Prussian blue analogue and a preparation method and application thereof. Background Art

[0002] The increasing depletion of fossil energy and the resulting environmental problems have made people urgently need to use sustainable energy, and the development of renewable energy is the focus of research today. Among them, sodium-ion batteries have attracted widespread attention due to their good electrochemical performance, abundant sodium resource reserves and wide availability. In sodium-ion batteries, the cathode material plays a decisive role in their performance. Prussian blue analogues (PBAs) have a unique open framework and three-dimensional macroporous structure, which is particularly suitable for the migration and storage of sodium ions. They also have the advantages of low cost, easy synthesis and high theoretical specific capacity. They are a very promising cathode material for sodium-ion batteries. However, the current Prussian blue analogues are usually prepared by coprecipitation. The obtained Prussian blue analogues are generally face-centered cubic or monoclinic structures, which contain a large amount of crystal water. The higher the content of crystal water, the worse its electrochemical performance. The presence of crystal water seriously hinders the improvement of the performance of Prussian blue analogues. Summary of the invention

[0003] In order to overcome at least one of the problems existing in the above-mentioned prior art, one of the objects of the present invention is to provide a Prussian blue analogue, wherein the Prussian blue has a specific composition, a rhombohedral phase structure, and a low content of crystalline water.

[0004] A second object of the present invention is to provide a method for preparing the above-mentioned Prussian blue analogue.

[0005] A third object of the present invention is to provide an application of the above-mentioned Prussian blue analogue as a positive electrode material for a sodium ion battery.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] The first aspect of the present invention provides a Prussian blue analogue, wherein the chemical formula of the Prussian blue analogue is Na x Co y [Fe(CN) 6 ] z , wherein 0.5≤y≤1.2, x / y=1.0~4.0, z / y=0.8~2.0; the crystal structure of the Prussian blue analogue is a rhombohedral phase.

[0008] The present invention obtains a cobalt-based Prussian blue analogue by introducing Co element. The material has a specific chemical composition and a rhombohedral phase structure, has strong deformability, low water content and is quasi-anhydrous. The quasi-anhydrous, rhombohedral phase structure cobalt-based Prussian blue material has excellent electrochemical performance and cycle performance.

[0009] Preferably, in the chemical formula of the Prussian blue analogue, x / y=1.0-3.0; more preferably, x / y=1.5-2.5.

[0010] Preferably, in the chemical formula of the Prussian blue analogue, z / y=0.8-1.5; more preferably, z / y=0.9-1.1.

[0011] In some specific embodiments of the present invention, in the chemical formula of the Prussian blue analog, 0.8≤y≤1.2; in some more specific embodiments of the present invention, 0.9≤y≤1.1. Non-limiting specific examples include, for example, the value of y is 0.92, 0.95, 1, 1.02, 1.05, etc.

[0012] In some specific embodiments of the present invention, in the chemical formula of the Prussian blue analog, 1.0≤x≤2.5; in some more specific embodiments of the present invention, 1.5≤x≤2.1. Non-limiting specific examples include, for example, the value of x is 1.6, 1.7, 1.8, 1.9, 2, 2.05, etc.

[0013] In some specific embodiments of the present invention, in the chemical formula of the Prussian blue analog, 0.8≤z≤1.5; in some more specific embodiments of the present invention, 0.9≤z≤1.2. Non-limiting specific examples include, for example, the value of z is 0.95, 1, 1.05, 1.1, 1.05, etc.

[0014] Preferably, the charge-discharge curve of the Prussian blue analog has only one charge-discharge platform.

[0015] The charge-discharge curve of the Prussian blue analogue of the present invention has only one charge-discharge platform, which is because the change of the spin state of the Prussian blue analogue Co-C and N-Fe affects the chemical environment of the active site, thereby changing the charge-discharge platform of the material. This new electrochemical feature improves the electrochemical performance and cycle characteristics of the cobalt-based Prussian blue analogue, so that the capacity of its entire charge-discharge platform can be utilized in practical applications, broadening its application field in positive electrode materials, especially as positive electrode materials for sodium ion batteries.

[0016] The charge-discharge platform described in the present invention refers to a period during which the voltage changes relatively steadily during the charge-discharge process of the battery. In this period, the voltage of the battery changes slightly, showing a certain stability.

[0017] Preferably, the voltage range of the charge-discharge platform is 3-3.4V vs.Na / Na + ; Further preferably, the voltage range of the charge and discharge platform is 3 to 3.3 V vs. Na / Na + .

[0018] The second aspect of the present invention provides a method for preparing the Prussian blue analogue described in the first aspect of the present invention, comprising the following steps: mixing a cobalt salt solution and a ferrocyanide salt solution for coprecipitation reaction to obtain a mixed system, and subjecting the mixed system to a solvothermal reaction to obtain the Prussian blue analogue; the cobalt salt solution and / or the ferrocyanide salt solution contain an organic solvent.

[0019] In the existing coprecipitation method, a rapid coprecipitation reaction will occur after the ferrocyanide salt solution and the cobalt salt solution are mixed to form a Prussian blue analog crystal containing a large amount of crystal water. However, the present invention allows the coprecipitation reaction to be carried out in an organic solvent, and the organic solvent can reduce the rate of the coprecipitation reaction to a certain extent, thereby reducing the defects in the obtained Prussian blue analog crystal; and in the subsequent solvent thermal reaction, the organic solvent will be embedded in the crystal of the Prussian blue analog, replacing the water molecules in the original position, thereby reducing the water content; and after the organic solvent is embedded in the lattice of the Prussian blue analog, the thermal stability of the Prussian blue analog crystal can also be improved. Through the preparation method provided by the present invention, a cobalt-based Prussian blue analog with low water content and a rhombohedral phase structure can be obtained, which has a flat charge and discharge curve and good electrochemical performance.

[0020] Preferably, the organic solvent is selected from organic solvents miscible with water; further preferably, the organic solvent includes at least one of alcohols, ketones, esters, amides, furans, nitriles or ether solvents.

[0021] The organic solvent used in the present invention is miscible with water and does not affect the solubility of ferrocyanide and cobalt salt. It can be embedded in the crystal of Prussian blue analog during its formation process, change the crystal structure of Prussian blue analog, reduce its water content, and improve its electrochemical performance.

[0022] Preferably, the organic solvent includes at least one of methanol, ethanol, glycerol, acetone, butanone, methyl formate, ethyl acetate, dimethylformamide, dimethylacetamide, tetrahydrofuran, 2-furan methanol, acetonitrile, propionitrile, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether or ethylene glycol dimethyl ether; further preferably, the organic solvent includes at least one of dimethylformamide, dimethylacetamide, tetrahydrofuran, 2-furan methanol, acetonitrile, propionitrile, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether or ethylene glycol dimethyl ether; further preferably, the organic solvent includes at least one of tetrahydrofuran, acetonitrile, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether or ethylene glycol dimethyl ether. In some specific embodiments of the present invention, the organic solvent is selected from tetrahydrofuran.

[0023] Preferably, the weight average molecular weight of the organic solvent is 10 to 1000; more preferably 20 to 500; and even more preferably 30 to 200.

[0024] The use of small molecule organic solvents is more conducive to embedding them into the crystals of Prussian blue analogs, replacing water molecules in their original positions, thereby reducing the water content and improving the thermal stability of the Prussian blue analogs.

[0025] Preferably, the ferrocyanide salt comprises at least one of lithium ferrocyanide, sodium ferrocyanide, potassium ferrocyanide, magnesium ferrocyanide, calcium ferrocyanide, zinc ferrocyanide or aluminum ferrocyanide; further preferably, the ferrocyanide salt comprises sodium ferrocyanide, potassium ferrocyanide or a combination thereof. In some specific embodiments of the present invention, the ferrocyanide salt is selected from sodium ferrocyanide.

[0026] Preferably, the cobalt salt comprises at least one of cobalt chloride, cobalt nitrate or cobalt sulfate. In some embodiments of the present invention, the cobalt salt is selected from cobalt chloride.

[0027] Preferably, the molar ratio of the ferrocyanide salt to the cobalt salt is (0.5-10):1; more preferably (0.8-6):1; and even more preferably (1-5):1.

[0028] Preferably, the ferrocyanide salt solution contains an organic solvent, and the organic solvent in the ferrocyanide salt solution accounts for 50% or more of the total volume of the organic solvent; further preferably, the organic solvent in the ferrocyanide salt solution accounts for 80-100% of the total volume of the organic solvent; even more preferably, the organic solvent in the ferrocyanide salt solution accounts for 100% of the total volume of the organic solvent, that is, the ferrocyanide salt solution contains an organic solvent, and the cobalt salt solution does not contain an organic solvent.

[0029] An organic solvent accounting for more than half of the total volume is added to the ferrocyanide salt solution, so that during the coprecipitation reaction, the organic solvent can better reduce the rate of the coprecipitation reaction, thereby reducing the defects in the obtained Prussian blue analog crystal, and is conducive to the subsequent solvothermal reaction to improve its crystal structure and electrochemical properties.

[0030] In addition, since the mutual solubility of the cobalt salt solution and the organic solvent is relatively weak, if the cobalt salt solution contains a large amount of organic solvent, obvious stratification will occur. Therefore, it is preferred to reduce the organic solvent content in the cobalt salt solution and increase the organic solvent content in the ferrocyanide salt solution.

[0031] Preferably, the cobalt salt solution and the ferrocyanide salt solution further contain water.

[0032] In some specific embodiments of the present invention, the amount of water in the cobalt salt solution and the amount of water in the ferrocyanide salt solution is not specifically limited, as long as the solute can be completely dissolved.

[0033] Preferably, in the mixed system, the volume ratio of water to the organic solvent is 1:(1-30); more preferably 1:(5-25); and even more preferably 1:(10-20).

[0034] Preferably, in the method for preparing the Prussian blue analog, the cobalt salt and the ferrocyanide salt are first dissolved in water respectively, and then an organic solvent is added to obtain the cobalt salt solution and the ferrocyanide salt solution. It is understood that when the cobalt salt solution does not contain an organic solvent, the step of adding an organic solvent is not included accordingly.

[0035] Preferably, the rate of adding the organic solution is 0.1 to 10 mL / min; more preferably, it is 0.5 to 8 mL / min; and even more preferably, it is 1 to 5 mL / min.

[0036] Ensuring a moderate rate of adding the organic solvent can allow the organic solvent to be more fully dispersed in the system.

[0037] Preferably, the cobalt salt solution and the ferrocyanide salt solution are mixed in a specific manner as follows: the cobalt salt solution is added into the ferrocyanide salt solution.

[0038] In order to avoid stratification due to the presence of too much organic solvent in the cobalt salt solution, the cobalt salt solution is preferably added to the ferrocyanide salt solution to reduce the organic solvent content in the cobalt salt solution system and ensure that the reaction raw materials are fully dispersed and the reaction proceeds fully.

[0039] Preferably, the addition rate of the cobalt salt solution is 0.01 to 1 mL / min; more preferably 0.05 to 0.8 mL / min; and even more preferably 0.1 to 0.5 mL / min.

[0040] Since the coprecipitation reaction between the cobalt salt and the ferrocyanide salt is relatively rapid, when the cobalt salt solution is added to the ferrocyanide salt solution for reaction, controlling the addition rate can make the reaction more uniform and the obtained crystals have fewer defects.

[0041] Preferably, the temperature of the solvothermal reaction is 80 to 180°C; more preferably 90 to 170°C; and even more preferably 100 to 150°C.

[0042] Preferably, the solvent thermal reaction time is 3 to 20 hours; more preferably 5 to 15 hours; further preferably 6 to 12 hours.

[0043] Preferably, a drying step is further included after the solvothermal reaction.

[0044] Preferably, the drying temperature is 80-220°C; more preferably 100-200°C; further preferably 120-180°C.

[0045] Since in the preparation method of the present invention, the thermal stability of the Prussian blue analog crystal can be improved after the organic solvent small molecules are embedded in the lattice of the Prussian blue analog, a drying step can be included after the solvent thermal reaction, and a higher drying temperature can be used to further reduce the water content without causing crystal decomposition.

[0046] Preferably, the drying time is 5 to 48 hours; more preferably 10 to 36 hours; and even more preferably 12 to 24 hours.

[0047] Preferably, after the solvothermal reaction and before the drying, at least one step of solid-liquid separation, washing, pre-drying or grinding is further included. In some specific embodiments of the present invention, after the solvothermal reaction and before the drying, at least one step of solid-liquid separation, washing, pre-drying and grinding is further included.

[0048] Preferably, the solid-liquid separation method includes filtration, centrifugation or a combination thereof.

[0049] Preferably, the centrifugal rotation speed is 8000-12000 r / min; more preferably, it is 9000-11000 r / min.

[0050] Preferably, the reagent used for washing is water; centrifugation is also performed after washing, and the centrifugal speed is preferably 8000-12000 r / min.

[0051] Preferably, the pre-drying temperature is 20-30°C; more preferably 22-28°C.

[0052] Preferably, the pre-drying time is 0.1 to 1 h; more preferably, it is 0.3 to 0.7 h.

[0053] The third aspect of the present invention provides a use of the Prussian blue analogue described in the first aspect of the present invention, or the Prussian blue analogue prepared by the preparation method described in the second aspect of the present invention as a positive electrode material for a sodium ion battery.

[0054] The beneficial effects of the present invention are as follows: the present invention obtains a cobalt-based Prussian blue analogue by introducing the Co element, which has a specific chemical composition and structural characteristics, presents a rhombohedral phase structure with good reversibility and low water content, has good cycle performance and deformability, and has a wide range of applications as a positive electrode material for sodium ion batteries.

[0055] Specifically, compared with the prior art, the present invention has the following advantages:

[0056] 1. The present invention reduces the reaction rate between ferrocyanide and cobalt salt by coprecipitating cobalt salt with ferrocyanide in an organic solvent, thereby reducing defects in the obtained Prussian blue analog crystals. In addition, small organic solvent molecules will be embedded in the interior of the Prussian blue analog crystals in the subsequent solvothermal reaction to replace the water molecules at the original position, so that a cobalt-based Prussian blue analog with good thermal stability, low water content and rhombohedral phase structure can be obtained. The cobalt-based Prussian blue analog has a flat charge and discharge curve and good electrochemical performance, and is widely used as a positive electrode material for sodium ion batteries.

[0057] 2. The preparation method provided by the present invention is simple, and a Prussian blue analogue with low water content can be obtained by coprecipitation and solvothermal method. In addition, since the obtained Prussian blue analogue has good thermal stability, the water content can be reduced by further high-temperature drying.

[0058] 3. Since the change of the spin state of Co-C and N-Fe affects the chemical environment of the active site, the cobalt-based Prussian blue analogue of the present invention has a specific crystal structure and electrochemical properties, and the charge-discharge curve has only one charge-discharge platform. Conventional Prussian blue analogues have two charge-discharge platforms, but in practical applications, only the energy of one of the platforms is generally used. The Prussian blue analogue prepared by the present invention only exhibits one charge-discharge platform, which is different from lithium iron phosphate (LiFePO 4 ), and in the Prussian blue analogue of the present invention, the capacity of the entire charge-discharge platform can be utilized in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0059] Figure 1 1 is a flow chart for the preparation of Prussian blue analogs in an embodiment of the present invention.

[0060] Figure 2 The infrared spectra of the Prussian blue analogs obtained in Example 1 and Comparative Example 1 are shown.

[0061] Figure 3 It is the infrared spectra of the Prussian blue analogs of Examples 2-3.

[0062] Figure 4 1 and 2 are XRD patterns of the Prussian blue analogs obtained in Example 1 and Comparative Example 1.

[0063] Figure 5 : XRD diagram of the Prussian blue analogues of Examples 2-3.

[0064] Figure 6 The charge and discharge curves of the Prussian blue analogues obtained in Example 1 and Comparative Example 1 are used as positive electrode materials.

[0065] Figure 7 The charge and discharge curves of the Prussian blue analogs of Examples 2 to 3 are used as the positive electrode material.

[0066] Figure 8 The electrochemical performance diagram of the Prussian blue analogues obtained in Example 1 and Comparative Example 1 when used as positive electrode materials.

[0067] Fig. 9 The electrochemical performance diagram of the Prussian blue analogues of Examples 2 to 3 when used as positive electrode materials. DETAILED DESCRIPTION

[0068] The content of the present invention is further described in detail below through specific examples. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the principles set forth in the present invention all belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific data exemplified below. The raw materials, reagents or devices used in the following examples and comparative examples, unless otherwise specified, can all be obtained from conventional commercial sources, or can be obtained by existing known methods.

[0069] The present invention provides a method for preparing a Prussian blue analogue. The preparation flow chart is as follows: Figure 1 As shown, the specific steps include:

[0070] A) Change Na 4 Fe(CN) 6 and CoCl 2 Dissolved in a certain amount of pure water, Na 4 Fe(CN) 6and CoCl 2 The molar ratio of the substance is (1-5): 1, and a certain amount of organic solvent (at least one of tetrahydrofuran, acetonitrile, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether and ethylene glycol dimethyl ether) is added dropwise. There is no strict restriction here, and it can be miscible with water and does not affect Na 4 Fe(CN) 6 and CoCl 2 Any organic solvent that can dissolve Na can be used. 4 Fe(CN) 6 or CoCl 2 In the system, but it is necessary to ensure that Na 4 Fe(CN) 6 The system contains more than half of the organic solvent. In the overall mixed system of water and organic solvent, the volume ratio of water to organic solvent is controlled at 1: (10-20), and the dripping speed of the organic solvent is 1-5 mL / min. In this step, a coprecipitation reaction occurs in the organic solvent system, and a subsequent solvent thermal reaction is carried out; in this way, the small molecules of the organic solvent can be embedded in the interior of the Prussian blue analog crystal, replacing the water molecules in the original position, which can reduce the water content; the organic solvent can also reduce the rate of the coprecipitation reaction to a certain extent, and reduce the defects in the obtained Prussian blue analog; on the other hand, after the small molecules of the organic solvent are embedded in the crystal lattice, the thermal stability of the Prussian blue analog crystal can be improved.

[0071] B) CoCl 2 The solution containing Na 4 Fe(CN) 6 ) was added to the solution (the dropping speed was 0.1-0.5 mL / min) to obtain a mixed solution.

[0072] C) The mixed solution is transferred to a reaction kettle, and kept at a certain temperature for a certain time (the holding temperature is 100-150° C., and the holding time is 6-12 hours) to obtain a solid-liquid mixture.

[0073] D) After the reactor is fully cooled, the solid-liquid mixture is centrifuged (at a speed of 5000 to 10000 r / min), the liquid is poured off to obtain a centrifugal product, and the centrifugal product is then washed with pure water for multiple times and centrifuged (at a speed of 5000 to 10000 r / min).

[0074] E) vacuum drying the washed solid (vacuum drying temperature is 100-200° C., and drying time is 12-24 h).

[0075] The present invention is further described below in conjunction with more specific embodiments and comparative examples.

[0076] Example 1

[0077] A method for preparing a Prussian blue analogue comprises the following steps:

[0078] Take 0.0003 mol Na 4 Fe(CN) 6 and 0.0003 mol CoCl 2 Dissolve them in 1 mL of pure water and stir at 400 r / min to 4 Fe(CN) 6 34 mL of tetrahydrofuran (THF) was added dropwise to the system (the addition rate was 1 mL / min), and then the CoCl 2 The solution containing Na 4 Fe(CN) 6 The solid-liquid mixture was then transferred to a 50mL reactor and kept at 120°C for 6 hours. After the reactor was cooled to room temperature, the solid-liquid mixture was taken out and centrifuged (at a speed of 10,000 r / min). The liquid was poured out to obtain a centrifuged product. The centrifuged product was then washed and centrifuged with pure water (at a speed of 10,000 r / min) and repeated three times. The obtained solid powder was then vacuum dried at 25°C for half an hour, and then fully ground, and then vacuum dried at 150°C for 24 hours to obtain the final product, named Na 2 CoFe(CN) 6 -THF.

[0079] Comparative Example 1

[0080] A method for preparing a Prussian blue analogue comprises the following steps:

[0081] 0.0003 mol Na 4 Fe(CN) 6 and 0.0003 mol CoCl 2 Dissolve them in 1 mL of pure water respectively, and stir them at 400 r / min. 2 The solution containing Na 4 Fe(CN) 6 The solution was added (the dropping speed was 0.1 mL / min), and then centrifuged (the speed was 10000 r / min), and the liquid was poured off to obtain the centrifugal product. The centrifugal product was washed and centrifuged with pure water (the speed was 10000 r / min), and repeated three times. The obtained solid powder was vacuum dried at 25°C for half an hour, and then fully ground, and then vacuum dried at 60°C for 24 hours (if dried above 60 degrees, the sample will decompose and is no longer Na 2 CoFe(CN) 6), the sample obtained in this example is named Na 2 CoFe(CN) 6 -H 2 O.

[0082] Example 2

[0083] A method for preparing a Prussian blue analogue comprises the following steps:

[0084] Take 0.0003 mol Na 4 Fe(CN) 6 and 0.0003 mol CoCl 2 Dissolve them in 1 mL of pure water and stir at 400 r / min to 4 Fe(CN) 6 34 mL of acetonitrile (ACN) was added dropwise to the system (the addition rate was 1 mL / min), and then the CoCl 2 The solution containing Na 4 Fe(CN) 6 The solid-liquid mixture was then transferred to a 50mL reactor and kept at 120°C for 6 hours. After the reactor was cooled to room temperature, the solid-liquid mixture was taken out and centrifuged (at a speed of 10,000 r / min). The liquid was poured out to obtain a centrifuged product. The centrifuged product was then washed and centrifuged with pure water (at a speed of 10,000 r / min) and repeated three times. The obtained solid powder was then vacuum dried at 25°C for half an hour, and then fully ground, and then vacuum dried at 150°C for 24 hours to obtain the final product, named Na 2 CoFe(CN) 6 -ACN.

[0085] Example 3

[0086] A method for preparing a Prussian blue analogue comprises the following steps:

[0087] Take 0.0015 mol Na 4 Fe(CN) 6 Dissolve in 5 mL of pure water and take 0.0003 mol CoCl 2 Dissolve in 1 mL pure water and stir at 400 r / min to 4 Fe(CN) 6 30 mL of tetrahydrofuran (THF) was added dropwise to the system (the addition rate was 1 mL / min), and then the CoCl 2 The solution containing Na 4 Fe(CN) 6The solid-liquid mixture was then transferred to a 50mL reactor and kept at 120°C for 6 hours. After the reactor was cooled to room temperature, the solid-liquid mixture was taken out and centrifuged (at a speed of 10,000 r / min). The liquid was poured out to obtain a centrifuged product. The centrifuged product was then washed and centrifuged with pure water (at a speed of 10,000 r / min) and repeated three times. The obtained solid powder was then vacuum dried at 25°C for half an hour, and then fully ground, and then vacuum dried at 150°C for 24 hours to obtain the final product, named Na 2 CoFe(CN) 6 -THF-5:1.

[0088] Performance Testing

[0089] 1) The Prussian blue analogs obtained in Examples 1 to 3 and Comparative Example 1 were characterized by infrared spectroscopy.

[0090] Figure 2 The infrared spectra of the Prussian blue analogs obtained in Example 1 and Comparative Example 1 are shown in FIG. 2 CoFe(CN) 6 -H 2 O at 3400cm -1 and 1620cm -1 Strong absorption peaks appeared at , corresponding to the adsorbed water and coordinated water of the Prussian blue analogue; while the Na 2 CoFe(CN) 6 -THF at 3400cm -1 The adsorption water peak at 20° is significantly weakened, indicating that the Na 2 CoFe(CN) 6 -THF has low adsorbed water content; at the same time, 1620cm -1 The coordinated water peak at almost completely disappeared, indicating that Na 2 CoFe(CN) 6 The content of crystal water inside the THF lattice is close to 0. Figure 2 Visible Na 2 CoFe(CN) 6 -H 2 The strongest peak of O is located at 2088 cm -1 At, it corresponds to the stretching vibration of Co-C≡N-Fe, while Na 2 CoFe(CN) 6 The strongest peak of -THF is at 2062cm -1There is a certain shift at the point, indicating that the stretching vibration state of Co-C≡N-Fe has changed, reflecting the change of the spin state of Co-C and N-Fe in the material, which also makes Na 2 CoFe(CN) 6 -THF has a unique flat charge and discharge curve.

[0091] Figure 3 is the infrared spectra of the Prussian blue analogs of Examples 2-3. It can be seen that the Na 2 CoFe(CN) 6 -CAN and Na of Example 3 2 CoFe(CN) 6 -THF-5:1, with Na 2 CoFe(CN) 6 -THF has similar structure and properties, Na 2 CoFe(CN) 6 -ACN and Na 2 CoFe(CN) 6 -The infrared spectrum of THF-5:1 is at 3400cm -1 The adsorption peak of water at 1620 cm -1 The coordinated water peaks at 2062 cm-1 are very weak, indicating that the content of crystalline water inside the crystal lattice is close to 0. -1 The position of the characteristic peak is basically consistent with that in Example 1.

[0092] 2) The Prussian blue analogs obtained in Examples 1 to 3 and Comparative Example 1 were characterized by X-ray diffraction.

[0093] Figure 4 The XRD patterns of the Prussian blue analogs obtained in Example 1 and Comparative Example 1 are shown in Table 1. 2 CoFe(CN) 6 -H 2 O has diffraction peaks at 17.2°, 24.1°, 38.7°, and 34.7°, corresponding to the (200), (220), (400), and (420) crystal planes, respectively, and is a monoclinic phase (space group is p21 / n). 2 CoFe(CN) 6 -THF has diffraction peaks at 18.4°, 24.7°, 37.6°, 31.1°, 37.3°, and 40.0°, corresponding to the crystal planes (012), (104), (110), (113), (107), and (116), respectively, and is a rhombohedral phase (space group is R-3). This indicates that the Na prepared by the method of Example 1 2 CoFe(CN) 6In the -THF crystals, the main peak of the monoclinic phase at 17.2° disappeared, and the main peak of the rhombohedral phase at 18.4° appeared instead, resulting in a rhombohedral phase structure, indicating that the crystalline water in the material has been almost completely removed.

[0094] Figure 5 2 is the XRD diagram of the Prussian blue analogue of Examples 2-3. It can be seen that the diffraction peak positions of the Prussian blue analogues of Examples 2-3 are substantially the same as those of Example 1, indicating that the crystal structures of the Prussian blue analogues obtained in Examples 2-3 are the same as those in Example 1, both of which are rhombohedral phase structures, and the materials contain almost no crystalline water.

[0095] 3) Testing the charge and discharge performance of the Prussian blue analogues obtained in Examples 1 to 3 and Comparative Example 1, the specific steps are as follows: The Prussian blue analogues obtained in Examples 1 to 3 and Comparative Example 1 are used as positive electrode materials, metallic sodium is used as negative electrode, 1 mol / L NaClO 4 The solution (the solvent is ethylene carbonate EC and dimethyl carbonate DMC in a volume ratio of 1:1) is used as the electrolyte, and the glass fiber is used as the separator. They are assembled into a sodium ion battery and the charge and discharge test is carried out at 30mA / g.

[0096] Figure 6 The charge-discharge curves of the Prussian blue analogs obtained in Example 1 and Comparative Example 1 are as positive electrode materials. It can be seen that the charge-discharge curves of the two Prussian blue analogs are significantly different, wherein Na 2 CoFe(CN) 6 -H 2 The charge-discharge curve of O has two charge-discharge platforms, while Na 2 CoFe(CN) 6 -THF's charge-discharge curve shows only one charge-discharge platform, and the voltage range of the charge-discharge platform is 3.0-3.4V vs.Na / Na + This is due to Na 2 CoFe(CN) 6 -THF changes the spin states of Co-C and N-Fe, affecting the chemical environment of the active sites and thus changing the charge and discharge platform of the material. Figure 6 It can also be seen that compared with Na 2 CoFe(CN) 6 -H 2 O,Na 2 CoFe(CN) 6 The discharge capacity of -THF increased from 123 mAh / g to 145 mAh / g. This was due to the fact that the material obtained by the method of Example 1 had fewer internal defects and a high capacity utilization rate. 2 CoFe(CN)6 -Reduction of the content of crystal water and adsorbed water in THF.

[0097] Figure 7 The charge and discharge curves of the Prussian blue analogs of Examples 2 to 3 as the positive electrode material show that Na 2 CoFe(CN) 6 -CAN and Na 2 CoFe(CN) 6 -THF-5:1 have flat charge-discharge curves, which are similar to those of Example 1, with only one charge-discharge platform appearing, and the voltage range of the charge-discharge platform is 3.0-3.4 V vs. Na / Na + .

[0098] 4) Testing the electrochemical performance of the Prussian blue analogs obtained in Examples 1 to 3 and Comparative Example 1, the specific steps are as follows: The Prussian blue analogs obtained in Examples 1 to 3 and Comparative Example 1 are used as the positive electrode material, metallic sodium is used as the negative electrode, and 1 mol / L NaClO 4 The solution (the solvent is ethylene carbonate EC and dimethyl carbonate DMC in a volume ratio of 1:1) was used as the electrolyte and the glass fiber was used as the separator to assemble a sodium ion battery, and a constant current charge and discharge test was carried out at 30 mA / g.

[0099] Figure 8 The electrochemical performance diagram of the Prussian blue analogue obtained in Example 1 and Comparative Example 1 when used as the positive electrode material. 2 CoFe(CN) 6 -H 2 The content of crystal water in O is high and occupies a part of the space for sodium ion deintercalation, resulting in an initial discharge capacity of only 123 mAh / g. After 100 charge and discharge cycles, the original sample Na 2 CoFe(CN) 6 The capacity retention rate of the Na 2 CoFe(CN) 6 -THF, its initial discharge capacity can reach 145mAh / g, which is significantly better than Na 2 CoFe(CN) 6 -H 2 O. At the same time, after 100 charge and discharge cycles, Na 2 CoFe(CN) 6 -THF capacity retention rate is 91%, and the cycle stability is significantly improved.

[0100] Fig. 9 The electrochemical performance diagram of the Prussian blue analogues of Examples 2 to 3 as the positive electrode material shows that the Na2 CoFe(CN) 6 -CAN and Na of Example 3 2 CoFe(CN) 6 -THF-5:1 capacity retention rates were 90.94% and 89.69%, respectively, both higher than that of Na 2 CoFe(CN) 6 -H 2 O, the Prussian blue analogs of Examples 2-3 also have good cycle stability.

[0101] The preparation method provided in the embodiment of the present invention is simple, and a Prussian blue analogue with low water content can be obtained by coprecipitation and solvothermal method. In addition, since the obtained Prussian blue analogue has good thermal stability, the water content can be reduced by further high-temperature drying. x CoFe(CN) 6 ) has two charge-discharge platforms (such as comparative example 1), but in practical applications, generally only one of the platforms is used. The Prussian blue analogue prepared in the embodiment of the present invention only exhibits one charge-discharge platform, and lithium iron phosphate (LiFePO 4 ), and in the Prussian blue analogue of the embodiment of the present invention, the capacity of the entire charge and discharge platform can be utilized in practical applications.

[0102] The Prussian blue analogue (Na x Co y [Fe(CN) 6 ] z , wherein 0.5≤y≤1.2, x / y=1.0~4.0, z / y=0.8~2.0; more specifically Na 2 CoFe(CN) 6 ) is a quasi-anhydrous, rhombohedral phase material. Due to its low water content and better reversibility, it has good cycle performance and deformability, and has a flat charge and discharge curve. The voltage range of the charge and discharge platform is 3.0~3.4V vs.Na / Na + , has good electrochemical properties and is widely used in the preparation of battery positive electrode materials, especially sodium ion battery positive electrode materials.

[0103] In the preparation method of the embodiment of the present invention, a cobalt salt and a ferrocyanide salt are subjected to a coprecipitation reaction in an organic solvent, which reduces the reaction rate between the ferrocyanide salt and the cobalt salt, reduces the defects in the obtained Prussian blue analog crystal, and the small molecules of the organic solvent are embedded in the interior of the Prussian blue analog crystal in the subsequent solvothermal reaction, replacing the water molecules at the original position, so that a cobalt-based Prussian blue analog with good thermal stability, low water content and a rhombohedral phase structure can be obtained.

[0104] In summary, the present invention obtains a cobalt-based Prussian blue analogue by introducing the Co element, which has a specific chemical composition and structural characteristics, presents a rhombohedral phase structure with good reversibility and low water content, has good cycle performance and deformability, and has a wide range of applications as a positive electrode material for sodium ion batteries.

Claims

1. A Prussian blue analogue, It is characterized in that The chemical formula of the Prussian blue analog is Na x Co y [Fe(CN) 6 ] z , wherein 0.5≤y≤1.2, x / y=1.0~4.0, z / y=0.8~2.0; the crystal structure of the Prussian blue analogue is a rhombohedral phase.

2. The Prussian blue analogue according to claim 1, It is characterized in that The charge-discharge curve of the Prussian blue analog has only one charge-discharge platform; preferably, the voltage of the charge-discharge platform is 3-3.4V vs.Na / Na + .

3. A method for preparing the Prussian blue analogue according to claim 1 or 2, It is characterized in that The following steps are involved: The cobalt salt solution and the ferrocyanide salt solution are mixed for coprecipitation reaction to obtain a mixed system, and the mixed system is subjected to solvent thermal reaction to obtain the Prussian blue analogue; the cobalt salt solution and / or the ferrocyanide salt solution contain an organic solvent.

4. The preparation method according to claim 3, It is characterized in that The organic solvent is selected from organic solvents miscible with water; preferably, the organic solvent includes at least one of alcohols, ketones, esters, amides, furans, nitriles or ether solvents; Preferably, the organic solvent comprises at least one of methanol, ethanol, glycerol, acetone, butanone, methyl formate, ethyl acetate, dimethylformamide, dimethylacetamide, tetrahydrofuran, 2-furanmethanol, acetonitrile, propionitrile, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether or ethylene glycol dimethyl ether; Preferably, the weight average molecular weight of the organic solvent is 10-1000.

5. The preparation method according to claim 3, It is characterized in that The ferrocyanide salt includes at least one of lithium ferrocyanide, sodium ferrocyanide, potassium ferrocyanide, magnesium ferrocyanide, calcium ferrocyanide, zinc ferrocyanide or aluminum ferrocyanide; and / or, the cobalt salt comprises at least one of cobalt chloride, cobalt nitrate or cobalt sulfate; And / or, the molar ratio of the ferrocyanide salt to the cobalt salt is (0.5-10):

1.

6. The preparation method according to claim 3, It is characterized in that The ferrocyanide salt solution contains an organic solvent, and the organic solvent in the ferrocyanide salt solution accounts for 50% or more of the total volume of the organic solvent; Preferably, the cobalt salt solution and the ferrocyanide salt solution further contain water; Preferably, in the mixed system, the volume ratio of water to organic solvent is 1:(1-30); Preferably, the cobalt salt and the ferrocyanide salt are first dissolved in water respectively, and then an organic solvent is added to obtain the cobalt salt solution and the ferrocyanide salt solution; the speed of adding the organic solvent is preferably 0.1-10 mL / min.

7. The preparation method according to claim 3, It is characterized in that The method of mixing the cobalt salt solution and the ferrocyanide salt solution is specifically: adding the cobalt salt solution into the ferrocyanide salt solution; preferably, the adding speed of the cobalt salt solution is 0.01-1 mL / min.

8. The preparation method according to claim 3, It is characterized in that The temperature of the solvent thermal reaction is 80 to 180°C; And / or, the solvent thermal reaction time is 3 to 20 hours.

9. The preparation method according to claim 3, It is characterized in that The method further comprises a drying step after the solvent thermal reaction; Preferably, the drying temperature is 80 to 220° C.; and / or the drying time is 5 to 48 hours.

10. Use of the Prussian blue analogue according to claim 1 or 2, or the Prussian blue analogue obtained by the preparation method according to any one of claims 3 to 9 as a positive electrode material for a sodium ion battery.

Citation Information

Cited By

  • An iron-based Prussian blue positive electrode material and its preparation method and application

    CN119774638A

  • An iron-based Prussian blue cathode material, its preparation method and application

    CN119774638B