Aluminum extraction method and system capable of realizing carbon utilization
Through the three-level cooling system and CO2 concentration preheating and pre-decomposition system, the problems of large liquid phasing of clinker and low CO2 concentration in limestone sintering method are solved, the operation rate and dissolution rate are improved, and low energy consumption and carbon emission reduction are achieved. It meets the needs of carbonation separation and improves the preparation efficiency and quality of alumina.
Patent Information
- Application Number
- CN202411057183.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-26
AI Technical Summary
In the existing limestone sintering process, the liquid phasing of the kiln clinker is large and easy to slab cleavage, resulting in low operation rate and low CO2 concentration, which cannot meet the needs of subsequent carbonation and separation processes, increasing production costs and carbon emissions. quantity.
Adopt three-stage cooling system and corresponding equipment, including mechanically driven compressed air spray cooling, single-cylinder cooler and grate cooler to ensure the optimal phase composition and spontaneous powdering of clinker, and preheating through CO2 enrichment The decomposition system increases the CO2 concentration and meets the needs of the carbonation separation process.
The clinker operation rate and dissolution rate are improved, energy consumption and cost are reduced, carbon emission reduction and carbon utilization are achieved, and the preparation efficiency and quality of alumina are improved.
Smart Images

Figure CN119018918A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aluminum extraction by limestone sintering, and in particular to a method and system for aluminum extraction by limestone sintering capable of realizing carbon utilization. Background Art
[0002] At present, the world produces more than 700,000 tons of alumina each year. China is the world's largest alumina producer, with an annual output of about 300,000 tons of alumina, accounting for about 40% of the world's total output. However, my country's bauxite resources are relatively scarce, with bauxite reserves accounting for only about 6% of the world's total reserves, and the ore grade is low. The ore type is mainly refractory water-insulating stone, the processing process is complex, the energy consumption is high, and the production cost is also high. Due to the serious shortage of bauxite resources in my country, it can only rely on importing ore from abroad to solve the problem of raw materials. China imports about 300,000 tons of bauxite each year, accounting for about 50% of the domestic bauxite usage. The lack of ore resources has seriously restricted the development of my country's alumina industry. Therefore, finding new alternative non-bauxite resources as raw materials for the alumina industry and studying new process technologies for alumina production have become the top priority of China's aluminum industry.
[0003] Bauxite, alum, kaolin, bauxite, nepheline, clay, fly ash, coal gangue, aluminum ash, Bayer red mud, etc. are high-aluminum minerals or solid wastes of aluminum, which can be used as raw materials for aluminum extraction. The main processes for aluminum extraction are alkali method, acid method and electric thermal method, in addition to limestone sintering method, acid-base combined method, ammonium salt roasting method, etc. The limestone sintering method can extract alumina from aluminum-containing raw materials. Compared with the soda-lime sintering method, the limestone sintering method has a wide range of applicability to raw materials. It is not necessary to add alkalinity when sintering clinker, and the clinker will self-powderize. It does not require wet grinding during dissolution, and the dissolved mud can be used to make cement.
[0004] The conventional production process of aluminum extraction by limestone sintering is as follows: limestone and aluminum-containing raw materials are mixed in a certain proportion, and the mixed raw materials are fed into the raw material grinding system to prepare raw material powder with particle size meeting the requirements; the raw material powder is fed into the preheating and pre-decomposition system through the feeding point, and then enters the decomposition furnace for calcination and decomposition after gas-solid heat exchange in the multi-stage cyclone preheater, and then enters the kiln tail smoke chamber after gas-solid separation in the bottom cyclone separator, and then enters the rotary kiln for solid phase reaction calcination to produce clinker. The main product of the sintering reaction is calcium dodecaaluminate (Ca 12 Al 14 O 33 , abbreviated as C 12A7) and dicalcium silicate (Ca2SiO4, abbreviated as C2S), and then the high-temperature clinker is cooled by a cooler. During the cooling process of the sintered clinker, the dicalcium silicate undergoes a phase change, that is, from β-C2S to γ-C2S, and the volume expands by 10%, and the clinker is pulverized into fine powder by itself; after the fine powder clinker is mixed with alkali solution, the separation of alumina and solid impurities can be achieved by utilizing the characteristics of calcium heptaaluminate decomposing in sodium carbonate solution to generate sodium aluminate solution. The dissolution slurry is obtained through the clinker dissolution process, and after separation through the calcium silicate slag separation process, a sodium aluminate crude liquid and a byproduct calcium silicate slag (i.e., active calcium silicate, which can be used as a raw material for calcining cement) are obtained. A medium concentration of CO2 gas is introduced into the sodium aluminate crude liquid to obtain an aluminum hydroxide slurry, and then alumina products are obtained through multiple processes such as filter pressing, re-dissolution, separation, and roasting. In addition, the low-temperature flue gas (flue gas containing low concentration of CO2) discharged from the outlet of the top cyclone separator of the preheating and predecomposition system recovers part of the heat through the waste heat recovery system and then enters the flue gas treatment system. After the flue gas treatment, it enters the chimney and is discharged into the atmosphere.
[0005] The main reaction equations involved in the conventional production process of aluminum extraction by limestone sintering are:
[0006] CaCO3=CaO+CO2 (1)
[0007] 12CaO + 7Al2O3 = Ca 12 Al 14 O 33 (2)
[0008] CaO + Al2O3 = CaAl2O4 (3)
[0009] 2CaO + SiO2 = Ca2SiO4 (4)
[0010] Ca 12 Al 14 O 33 + 12Na2CO3 + 5H2O = 14NaAlO2 +12CaCO3 + 10NaOH (5)
[0011] 2NaAlO2 + CO2 + 3H2O = Na2CO3 + 2Al(OH)3 (6)
[0012] 2Al(OH)3 = Al2O3 + 3H2O (7)
[0013] During the sintering process, the aluminum oxide in the aluminum resource reacts with lime to form calcium aluminate which is soluble in sodium carbonate solution, and the silicon dioxide reacts with lime to form dicalcium silicate which is insoluble in sodium carbonate solution. The calcium aluminate clinker is then leached with sodium carbonate solution to achieve efficient separation of aluminum and silicon. The theoretical optimal phase composition of clinker is C 12 A7 and γ-C2S, and when the clinker is cooled to about 650℃, dicalcium silicate is transformed from β-C2S to γ-C2S, accompanied by a volume expansion of about 10%. The calcium aluminate clinker undergoes spontaneous pulverization and can be leached without crushing or grinding. In addition, since it is relatively stable in the sodium aluminate solution, there is basically no secondary reaction in the leaching process of calcium aluminate that causes the loss of aluminum oxide and sodium oxide.
[0014] Chinese invention patent CN103712462A discloses an indirect cooling device for fly ash, limestone, calcined alumina self-pulverizing clinker, which realizes the slow movement of clinker in the cooler, and the crystal transformation occurs during the cooling process to form self-pulverizing clinker. However, the cooling device has a complex structure and is composed of many ventilation ducts. The clinker moves slowly between the ventilation ducts, which easily causes the equipment to be blocked, making it inconvenient to repair, resulting in a low system operation rate. Once the clinker wears the air duct, the damaged duct is difficult to repair.
[0015] In summary, the main problems of aluminum production by limestone sintering are:
[0016] 1) The aluminum-containing clinker out of the kiln has a high liquid phase (about 40-60%, and the cement clinker liquid phase is about 25-30%), and has high viscosity. It is very easy to adhere to the connecting equipment between the rotary kiln and the cooler, forming a crust and blockage, resulting in the inability to continuously operate the production line, extremely low operating rate, and low production capacity.
[0017] 2) Due to the narrow firing temperature range, the clinker out of the kiln tends to form large lumps, and the theoretically optimal phase composition of the clinker is C 12 A7 and γ-C2S, so how to achieve the best phase composition of clinker, spontaneous pulverization of clinker and heat recovery through appropriate cooling system and equipment has become a key issue of this technology.
[0018] 3) The carbonation separation process of sodium aluminate crude liquid (reaction equation (6)) requires the provision of flue gas containing medium-concentration CO2, and the CO2 concentration needs to be ≥30%. However, the conventional limestone sintering method for aluminum extraction uses air combustion, resulting in a large amount of flue gas and a low CO2 concentration (CO2 concentration is about 10-20%), which cannot meet the requirements of the crude liquid carbonation separation process. Therefore, a large amount of medium- and high-concentration CO2 gas needs to be purchased, resulting in a significant increase in production costs; at the same time, a large amount of flue gas containing CO2 is discharged, resulting in a significant increase in carbon emission reduction pressure.
[0019] Based on the above background, this study optimizes and improves the existing limestone sintering aluminum extraction process to solve the problems of large liquid phase volume of clinker out of the kiln, easy compaction, inability to transport and cool, and affecting the system operation rate, so as to achieve the optimal phase composition of clinker, spontaneous pulverization of clinker and heat recovery, and enable the sintering system to normally produce aluminum-based compounds. At the same time, without purchasing additional CO2 gas, the flue gas containing medium concentration of CO2 required for the carbonation separation link is prepared, further reducing the system CO2 emissions, thereby preparing alumina with higher efficiency and lower cost, which will become the key to large-scale preparation of alumina by limestone sintering. Summary of the invention
[0020] In order to solve the problems existing in the prior art, the present invention provides an aluminum extraction method and system that can realize carbon utilization. The present invention solves the problem that the amount of liquid phase of the kiln clinker is large and easy to harden, which cannot be transported and cooled, affecting the system operation rate. The three-stage cooling system and corresponding equipment are used to achieve the optimal phase composition of the clinker, spontaneous pulverization of the clinker and heat recovery; and without purchasing additional CO2 gas, the carbonation separation in the alumina preparation link meets the demand for medium-concentration CO2, and solves the problem that the CO2 concentration of the flue gas generated by the existing limestone sintering method for aluminum extraction is low, resulting in the inability to utilize carbon in the subsequent carbonation separation process, resulting in a significant increase in production costs, and the existing limestone sintering method for aluminum extraction The system has high energy consumption, low clinker dissolution rate and large carbon emissions, resulting in a significant increase in carbon emission reduction pressure. The entire production system of the present invention has a high operation rate, low energy consumption, low cost, and realizes carbon emission reduction, carbon utilization and waste heat utilization functions, which has important practical significance.
[0021] The present invention is implemented as follows: a method for extracting aluminum that can realize carbon utilization comprises the following steps:
[0022] Raw material preparation:
[0023] The aluminum-containing raw materials and limestone are mixed in a certain proportion, and the mixed raw materials are ground to prepare raw meal powder with a particle size that meets the requirements;
[0024] Clinker preparation and medium CO2 concentration flue gas preparation:
[0025] The raw meal powder is fed into the CO2 concentration preheating and predecomposition system and the energy-saving preheating and predecomposition system of different equipment specifications at a predetermined feeding ratio, and is respectively fed into the corresponding multi-stage cyclone preheaters of the two preheating and predecomposition systems for gas-solid heat exchange, and then is respectively fed into the corresponding decomposition furnaces of the two preheating and predecomposition systems for calcination and decomposition;
[0026] The mixed flue gas after high-purity O2 and part of high-temperature tertiary air are mixed into the decomposition furnace of the CO2 concentration preheating and predecomposition system. The mixed flue gas contains 30-50% O2 and 50-70% N2. The high-concentration O2 causes the fuel in the decomposition furnace of the CO2 concentration preheating and predecomposition system to burn and decompose the limestone to produce medium-concentration CO2. The flue gas discharged from the top outlet of the CO2 concentration preheating and predecomposition system is low-temperature medium-concentration CO2 flue gas. The temperature range of the low-temperature medium-concentration CO2 flue gas is 200-350°C. The wet-base CO2 concentration of the low-temperature medium-concentration CO2 flue gas is 30-50%, the O2 concentration is 2-4%, the N2 concentration is 28-50%, and the H2O concentration is 8-20%.
[0027] The kiln gas and part of the high-temperature tertiary air enter the decomposition furnace of the energy-saving preheating and predecomposition system. The flue gas discharged from the top outlet of the energy-saving preheating and predecomposition system is low-temperature and low-CO2 concentration flue gas. The temperature range of the low-temperature and low-CO2 concentration flue gas is 240-450°C, and the wet-based CO2 concentration in the low-temperature and low-CO2 concentration flue gas is 10-20%;
[0028] All the hot raw materials after decomposition enter the rotary kiln through the kiln tail smoke chamber for calcination. Kiln gas and high-temperature aluminum-based compound clinker are generated in the rotary kiln. The high-temperature aluminum-based compound clinker is cooled in three stages to obtain aluminum-based clinker products.
[0029] First stage cooling: mechanical pushing and compressed air blowing are used to transform the liquid phase on the surface of high-temperature aluminum-based compound clinker particles into a solid state;
[0030] Second stage cooling: Use a single-drum cooler to slowly cool the clinker from 1200-1300℃ to 700-900℃ after primary cooling. The cooling time is 30-60min, so that the phase composition of the clinker is 1200-1300℃, 700-900℃, 700-13 ... 12 A7 is the main one;
[0031] Third stage cooling: Use a grate cooler to cool the clinker after secondary cooling from 700-900℃ to 400-500℃ for 10-20min; then slowly cool from 400-500℃ to 70-100℃ for 40-80min;
[0032] Clinker Carbonation Separation:
[0033] The aluminum-based clinker product is dissolved with alkaline solution, separated and washed to obtain crude sodium aluminate liquid and waste residue; the crude sodium aluminate liquid fully reacts with the medium-concentration CO2 flue gas produced by the CO2 concentration preheating and predecomposition system to obtain sodium carbonate solution and aluminum hydroxide, and the aluminum hydroxide is roasted to obtain alumina finished product.
[0034] In the above technical solution, preferably, the cooling residual air after the third stage cooling has a temperature of 80-120°C after cyclone dust collection and bag dust collection, and part of it returns to the middle air supply of the grate cooler of the third stage cooling.
[0035] In the above technical solution, preferably, the raw meal powder feeding ratio of the CO2 concentration preheating and predecomposition system and the energy-saving preheating and predecomposition system is 1:1 to 1:6.
[0036] In the above technical solution, preferably, the O2 concentration in the high-purity O2 is 50-99%.
[0037] In the above technical scheme, preferably, the low-temperature and low-CO2 concentration flue gas discharged from the outlet of the energy-saving preheating and predecomposition system is partially recovered by the waste heat recovery system and then enters the flue gas treatment system, and after the flue gas treatment, it enters the chimney and is discharged into the atmosphere.
[0038] An aluminum extraction system capable of realizing carbon utilization, comprising a CO2 concentration preheating and predecomposition system, an energy-saving preheating and predecomposition system, a kiln tail smoke chamber, a rotary kiln, a three-stage cooling system, a tertiary air duct, and a crude liquid carbonation separation system, wherein the energy-saving preheating and predecomposition system, the kiln tail smoke chamber, the rotary kiln, and the three-stage cooling system are connected in sequence, and the tertiary air duct connects the three-stage cooling system and the decomposition furnace of the energy-saving preheating and predecomposition system; the aluminum-based clinker product outlet of the three-stage cooling system is connected to the crude liquid carbonation separation system;
[0039] The CO2 concentration, preheating and predecomposition system includes a first decomposition furnace and a first row of cyclone preheaters; a first burner is arranged on the first decomposition furnace, a high-purity oxygen inlet is connected to the bottom of the first decomposition furnace, the bottom of the first decomposition furnace is connected to the tertiary air duct, and a first row of raw material inlet is opened on the first decomposition furnace; the air inlet of the cyclone separator at the bottom end of the first row of cyclone preheaters is connected to the air outlet pipe of the first decomposition furnace, and the air outlet of the cyclone separator at the top end of the first row of cyclone preheaters discharges low-temperature medium CO2 concentration flue gas, and the air outlet of the cyclone separator at the top end of the first row of cyclone preheaters is connected to the crude liquid carbonation separation system; the feed inlet of the cyclone separator at the top end of the first row of cyclone preheaters is used for feeding raw material powder, and the discharge port of the cyclone separator at the bottom end of the first row of cyclone preheaters is connected to the kiln tail smoke chamber.
[0040] In the above technical scheme, preferably, the three-stage cooling system includes a first-stage cooling device, a second-stage cooling device and a third-stage cooling device which are connected in sequence, the first-stage cooling device includes a first-stage cooling cavity, a mechanical pushing assembly is provided at the material dropping place of the first-stage cooling cavity, the bottom of the first-stage cooling cavity is a material dropping slope, the slope angle is ≥50°, the mechanical pushing assembly pushes the clinker onto the material dropping slope, the material dropping slope adopts anti-scaling refractory material to prevent sticky materials from adhering to the slope, a plurality of compressed air blowing ports are arranged on the material dropping slope, and compressed air is blown to transform the liquid phase on the surface of the clinker particles into a solid state, and smoothly enter the second-stage cooling device; the second-stage cooling device is a single-cylinder cooler; the third-stage cooling device is a grate cooler, the cooling residual air outlet of the third-stage cooling device is connected to the cyclone dust collecting equipment and the bag dust collecting equipment in sequence, and the flue gas outlet of the bag dust collecting equipment is connected to the middle air supply port of the grate cooler.
[0041] In the above technical solution, preferably, the second-stage cooling device is arranged to be inclined downward from its inlet to its outlet, with an inclination angle of 1-5° and a rotation speed of 0.5-5 rpm.
[0042] In the above technical scheme, preferably, the crude liquid carbonation separation system includes an alkali liquid dissolution device, a separation and washing device, a crude liquid carbonation separation device and an aluminum hydroxide roasting device, the aluminum-based clinker outlet of the three-stage cooling system is connected to the feed inlet of the alkali liquid dissolution device, the dissolution liquid outlet of the alkali liquid dissolution device is connected to the liquid inlet of the separation and washing device, the liquid outlet of the separation and washing device is connected to the liquid inlet of the crude liquid carbonation separation device, the air outlet of the top cyclone separator of the first row of cyclone preheaters is connected to the air inlet of the crude liquid carbonation separation device, the aluminum hydroxide outlet of the crude liquid carbonation separation device is connected to the inlet of the aluminum hydroxide roasting device, and the outlet of the aluminum hydroxide roasting device is a finished alumina product.
[0043] In the above technical solution, preferably, the CO2 concentration, preheating and predecomposition system also includes an emergency discharge pipe, one end of which is connected to the bottom end of the first decomposition furnace, and the other end of which is connected to the kiln tail smoke chamber.
[0044] In the above technical solution, preferably, the first row of raw material inlets is provided in plurality.
[0045] In the above technical solution, preferably, the energy-saving preheating and precalcining system comprises a second calcining furnace and a second row of cyclone preheaters, the second calcining furnace is provided with a second burner, the second calcining furnace is connected with the tertiary air duct and the kiln tail smoke chamber, and the second calcining furnace is provided with a second row of raw material inlets;
[0046] The air inlet of the cyclone separator at the bottom end of the second row of cyclone preheaters is connected to the air outlet pipe of the second decomposition furnace, and the air outlet of the cyclone separator at the top end of the second row of cyclone preheaters discharges low-temperature and low-CO2 concentration flue gas; the feed port of the cyclone separator at the top end of the second row of cyclone preheaters is used for feeding raw material powder, the discharge port of the second-to-last cyclone separator of the second row of cyclone preheaters is connected to the second decomposition furnace, and the discharge port of the cyclone separator at the bottom end of the second row of cyclone preheaters is connected to the kiln tail smoke chamber.
[0047] In the above technical solution, preferably, the number of stages of the first row of cyclone preheaters is 5 to 7; the number of stages of the second row of cyclone preheaters is 5 to 7.
[0048] The advantages and positive effects of the present invention are:
[0049] (1) The present invention adopts a three-stage cooling method to cool the high-temperature aluminum-based compound clinker. Each cooling device in the three-stage cooling system performs its own function, ensuring the low energy consumption of high clinker operation rate, high dissolution rate, and spontaneous pulverization without grinding. The first stage of cooling transforms the liquid phase on the surface of the clinker particles into a solid phase, solving the problem of material adhesion and inability to transport and cool; the second stage of cooling slowly cools the clinker to an optimal phase composition of C 12 A7; The third stage cooling converts dicalcium silicate from β-C2S to γ-C2S, accompanied by a volume expansion of about 10%. The calcium aluminate clinker undergoes spontaneous pulverization and can be dissolved without crushing or grinding. The entire cooling system and equipment make the aluminum dissolution rate greater than 90% and the operating rate higher than 95%.
[0050] (2) In the present invention, the cooling residual air after the third stage cooling is subjected to cyclone dust collection and bag dust collection to reduce the loss of fine powder, and part of the flue gas is recycled and applied to the middle section of the third stage cooling device to achieve the purpose of slow cooling of the third stage cooling below 500°C, and heat is recovered and utilized.
[0051] (3) The present invention fully considers the technical characteristics that the CO2 concentration of the flue gas at the outlet of the preheater is relatively low in the conventional rotary kiln production process, and the subsequent carbonation separation of the crude liquid cannot be used for carbon utilization. The present invention sets up a CO2 concentration, preheating and predecomposition system to significantly increase the CO2 concentration of the flue gas at the outlet of the CO2 concentration, preheating and predecomposition system from 10 to 20% (wet basis) to more than 30% (wet basis), so that the subsequent crude liquid carbonation separation link can use the CO2 flue gas generated by the system itself, thereby achieving the purpose of carbon utilization and reducing production costs.
[0052] (4) Based on the reaction equation of aluminum-containing raw materials and limestone and the amount of carbon dioxide required for carbonation separation of crude liquid, the present invention is designed as two preheating and predecomposition systems with different specifications, so that the CO2 concentration preheating and predecomposition system and the energy-saving preheating and predecomposition system match different raw material feed amounts. Among them, the energy-saving preheating and predecomposition system is designed with full consideration of its heat exchange efficiency and resistance to minimize its energy consumption. The CO2 concentration preheating and predecomposition system is used to produce part of the aluminum-based clinker, and at the same time generates flue gas required by the crude liquid carbonation separation system (the CO2 concentration and the total amount of CO2 in the flue gas both meet the needs of the crude liquid carbonation separation link), and the CO2 concentration preheating and predecomposition system can be designed with the most economical oxygen production capacity to reduce the cost of oxygen production.
[0053] (5) The cyclone preheater outlet temperature of the entire system of the present invention is low, the air volume is small, and the system energy consumption is low. The flue gas at the outlet of the energy-saving preheating and predecomposition system and the cooling excess air of the three-stage cooling system can be used as waste heat to reduce the energy loss of the entire production line. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0055] Figure 1 A process flow chart of an aluminum extraction method capable of realizing carbon utilization provided by an embodiment of the present invention;
[0056] Figure 2 A flow chart of an aluminum extraction system capable of realizing carbon utilization provided by an embodiment of the present invention;
[0057] Figure 3 A schematic structural diagram of a first-stage cooling device provided in an embodiment of the present invention.
[0058] In the figure: 1. CO2 concentration preheating and predecomposition system; 2. Energy-saving preheating and predecomposition system; 3. Kiln tail smoke chamber; 4. Rotary kiln; 5. Three-stage cooling system; 5-1. First-stage cooling device; 5-11. Mechanical push assembly; 5-12. Unloading slope; 5-13. Compressed air blowing port; 5-2. Second-stage cooling device; 5-3. Third-stage cooling device; 6. Tertiary air duct; 7. Cyclone dust collector; 8. Bag dust collector. DETAILED DESCRIPTION
[0059] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solution of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0060] Example
[0061] like Figure 1 As shown, the purpose of the present invention is achieved through the following process flow, which mainly includes the following process flow:
[0062] The aluminum-containing raw materials and limestone are mixed in a certain proportion, and the mixed raw materials are fed into the raw material grinding system for grinding to prepare raw material powder with particle size meeting the requirements.
[0063] The raw meal powder is fed into the CO2 concentration preheating and predecomposition system 1 and the energy-saving preheating and predecomposition system 2 of different equipment specifications at a predetermined feeding ratio, and the raw meal powder feeding ratio of the CO2 concentration preheating and predecomposition system 1 and the energy-saving preheating and predecomposition system 2 is 1:1-1:6. The raw meal powder is respectively fed into the CO2 concentration preheating and predecomposition system 1 and the energy-saving preheating and predecomposition system 2 through gas-solid heat exchange in the multi-stage cyclone preheaters corresponding to the two preheating and predecomposition systems, and then respectively fed into the decomposition furnaces corresponding to the two preheating and predecomposition systems for calcination and decomposition. The hot raw meal after decomposition is then all fed into the rotary kiln 4 through the kiln tail smoke chamber 3 for solid-phase reaction calcination, and kiln gas and high-temperature aluminum-based compound clinker are generated in the rotary kiln 4.
[0064] The mixed flue gas with a concentration of 50-99% high-purity O2 prepared by the oxygen production equipment and mixed with part of the high-temperature tertiary air enters the decomposition furnace of the CO2 concentration preheating and predecomposition system 1. The mixed flue gas contains 30-50% O2 and 50-70% N2. The high-concentration O2 causes the fuel in the decomposition furnace of the CO2 concentration preheating and predecomposition system 1 to burn and decompose the limestone to produce medium-concentration CO2; the flue gas discharged from the top outlet of the CO2 concentration preheating and predecomposition system 1 is low-temperature flue gas with medium CO2 concentration, and the temperature range of the low-temperature flue gas with medium CO2 concentration is 200-350°C (depending on the number of stages of the first row of cyclone preheaters), and the wet-based CO2 concentration of the low-temperature flue gas with medium CO2 concentration is 30-50%, the O2 concentration is 2-4%, the N2 concentration is 28-50%, and the H2O concentration is 8-20%;
[0065] The kiln gas enters the decomposition furnace of the energy-saving preheating and predecomposition system 2 through the kiln tail smoke chamber 3, and part of the high-temperature tertiary air enters the bottom and middle of the decomposition furnace of the energy-saving preheating and predecomposition system 2. The flue gas discharged from the top outlet of the energy-saving preheating and predecomposition system 2 is low-temperature and low-CO2 concentration flue gas. The temperature range of the low-temperature and low-CO2 concentration flue gas is 240-450°C (depending on the number of stages of the second row cyclone preheater), and the wet-based CO2 concentration of the low-temperature and low-CO2 concentration flue gas is 10-20%; the low-temperature and low-CO2 concentration flue gas enters the flue gas treatment system after part of the heat is recovered by the waste heat recovery and utilization system, and after the flue gas treatment, it enters the chimney and is discharged into the atmosphere.
[0066] The high-temperature aluminum-based compound clinker is cooled by the three-stage cooling system 5 to obtain an aluminum-based clinker product.
[0067] First stage cooling: mechanical pushing and compressed air blowing are used to transform the liquid phase on the surface of high-temperature aluminum-based compound clinker particles into a solid state; there is a mechanical pushing device at the first stage cooling drop point to force the easy-to-bond clinker to be transported to the discharge slope. The angle of the discharge slope is ≥50°. There are multiple area modules arranged on the discharge slope. Each area module is provided with a gas channel. Compressed air blowing is used to transport the clinker pneumatically. The discharge slope uses anti-scaling refractory materials to prevent the clinker from bonding to the discharge slope to form a large crust. Due to the large amount of clinker liquid phase, the purpose of the first stage cooling is to use a small air volume to transform the liquid phase on the surface of the clinker particles into a solid state, and smoothly enter the second stage cooling stage to solve the problem of material bonding and inability to transport and cool.
[0068] Second stage cooling: Use a single-drum cooler to slowly cool the clinker from 1200-1300℃ to 700-900℃ after primary cooling. The cooling time is 30-60min, so that the phase composition of the clinker is 1200-1300℃, 700-900℃, 700-13 ... 12 A7 is the main one; the second stage cooling requires a slow cooling system to make the best phase composition of clinker C 12 A7. The second stage cooling adopts a single drum cooler to complete the transportation and cooling of clinker. The second stage cooling device is arranged downwardly from its inlet to the outlet, with an inclination angle of 1-5° and a rotation speed of 0.5-5rpm. The cooling time of clinker can be controlled by designing the inclination of the single drum cooler, the material of refractory materials and adjusting the rotation speed of the single drum cooler.
[0069] Third stage cooling: Use a grate cooler to cool the clinker after secondary cooling from 700-900℃ to 400-500℃ for 10-20min; then slowly cool from 400-500℃ to 70-100℃ for 40-80min; the third stage cooling needs to be slow cooling when the temperature is below 500℃, so that the best phase composition of the clinker is γ-C2S. The third stage cooling uses a grate cooler. By reasonably designing the cooling area, blast volume and grate speed of the grate cooler, the cooling time of the clinker can be controlled, and the powder can be prevented from being carried away by the wind, causing losses. The third stage cooling converts dicalcium silicate from β-C2S to γ-C2S, accompanied by a volume expansion of about 10%. The calcium aluminate clinker undergoes spontaneous pulverization and can be leached without crushing or grinding. The cooling residual air after the third stage cooling is collected by cyclone dust collector and bag dust collector at a temperature of 80-120℃, and part of it is returned to the middle air supply of the grate cooler of the third stage cooling to achieve the purpose of slow cooling below 500℃ in the third stage cooling, and heat is recovered and utilized.
[0070] The aluminum-containing clinker product is dissolved with alkaline solution, separated and washed to obtain crude sodium aluminate liquid and waste residue. The crude sodium aluminate liquid fully reacts with the medium-concentration CO2 gas produced by the CO2 concentration, preheating and predecomposition system to obtain sodium carbonate solution and aluminum hydroxide. The aluminum hydroxide is roasted to obtain finished alumina.
[0071] like Figure 2 As shown, the aluminum extraction system capable of realizing carbon utilization provided by the embodiment of the present invention comprises a CO2 concentration preheating and predecomposition system 1, an energy-saving preheating and predecomposition system 2, a kiln tail smoke chamber 3, a rotary kiln 4, a three-stage cooling system 5, a tertiary air duct 6, a cyclone dust collector 7, a bag dust collector 8 and a crude liquid carbonation separation system. The energy-saving preheating and predecomposition system 2, the kiln tail smoke chamber 3, the rotary kiln 4, and the three-stage cooling system 5 are connected in sequence, and the three-stage air duct 6 connects the three-stage cooling system 5 and the decomposition furnace of the energy-saving preheating and predecomposition system 2; the aluminum-based clinker product outlet of the three-stage cooling system 5 is connected to the crude liquid carbonation separation system;
[0072] The CO2 concentration preheating and predecomposition system 1 includes a first decomposition furnace and a first row of cyclone preheaters; a first burner is arranged on the first decomposition furnace, a high-purity oxygen inlet is connected to the bottom of the first decomposition furnace, the bottom of the first decomposition furnace is connected to the tertiary air duct 6, and a first row of raw material inlet is opened on the first decomposition furnace; a first air outlet pipe is arranged at the top of the first decomposition furnace, and it should be noted that the first air outlet pipe can also be arranged on the side of the first decomposition furnace; an emergency unloading pipe is designed at the bottom of the first decomposition furnace. The air inlet of the cyclone separator at the bottom end of the first row of cyclone preheaters is connected to the first air outlet pipe, and the air outlet of the cyclone separator at the top end of the first row of cyclone preheaters discharges low-temperature medium CO2 concentration flue gas, and the air outlet of the cyclone separator at the top end of the first row of cyclone preheaters is connected to the crude liquid carbonation separation system; the feed inlet of the cyclone separator at the top end of the first row of cyclone preheaters is used for raw material powder feeding, and the discharge port of the cyclone separator at the bottom end of the first row of cyclone preheaters is connected to the kiln tail smoke chamber 3.
[0073] In order to adjust the temperature field distribution in the first decomposition furnace, the first row of raw material inlets can be set to multiple, and those skilled in the art can set them according to actual needs. Figure 2 The first row of raw material inlets is shown in FIG. 1 , including a first raw material inlet and a second raw material inlet.
[0074] One end of the emergency unloading pipe is connected to the bottom of the first decomposition furnace, and the other end is connected to the kiln tail smoke chamber 3. A valve is arranged on the emergency unloading pipe. The emergency unloading pipe has the following functions: when the system suddenly loses power or other faults occur, the valve on the emergency unloading pipe opens, and the hot material in the first decomposition furnace is unloaded into the kiln tail smoke chamber 3 through the emergency unloading pipe to ensure the safety of the system.
[0075] The energy-saving preheating and predecomposition system 2 includes a second decomposition furnace and a second row of cyclone preheaters, a second burner is arranged on the second decomposition furnace, the bottom and the middle of the second decomposition furnace are connected to the tertiary air duct 6, a second row of raw material inlet is opened on the second decomposition furnace, a second air outlet pipe is arranged at the top of the second decomposition furnace, and the bottom end of the second decomposition furnace is connected to the kiln tail smoke chamber 3; the air inlet of the cyclone separator at the bottom end of the second row of cyclone preheaters is connected to the second air outlet pipe, and the air outlet of the cyclone separator at the top end of the second row of cyclone preheaters discharges low-temperature and low-CO2 concentration flue gas; the feed port of the cyclone separator at the top end of the second row of cyclone preheaters is used for feeding raw material powder, the discharge port of the second to last stage cyclone separator of the second row of cyclone preheaters is connected to the second decomposition furnace, and the discharge port of the cyclone separator at the bottom end of the second row of cyclone preheaters is connected to the kiln tail smoke chamber 3.
[0076] The number of stages of the first row of cyclone preheaters is preferably 5 to 7; the number of stages of the second row of cyclone preheaters is preferably 5 to 7.
[0077] It should be noted that the number of CO2 concentration preheating and predecomposition systems 1 and energy-saving preheating and predecomposition systems 2 is only for illustration. Technical personnel in this field can set them according to actual needs. The cooler can be a grate cooler, a single-cylinder cooler, a multi-cylinder cooler, or a combined cooler, and the fan can adopt a combination of existing multiple fans.
[0078] The three-stage cooling system 5 comprises a first-stage cooling device 5-1, a second-stage cooling device 5-2 and a third-stage cooling device 5-3 connected in sequence, the first-stage cooling device 5-1 comprises a first-stage cooling cavity, a mechanical pushing component 5-11 is arranged at the material dropping position of the first-stage cooling cavity, the bottom of the first-stage cooling cavity is a material dropping slope 5-12, the material dropping slope angle is ≥50°, the mechanical pushing component 5-11 pushes the clinker onto the material dropping slope 5-12, the material dropping slope adopts anti-scaling refractory material to prevent sticky materials from sticking to the slope, and a plurality of There are compressed air blowing ports 5-13, which spray compressed air to transform the liquid phase on the surface of the clinker particles into a solid state, and smoothly enter the second-stage cooling device 5-2; the second-stage cooling device 5-2 is a single-cylinder cooler, which is arranged tilted downward from its inlet to the outlet, with an inclination angle of 1-5° and a rotation speed of 0.5-5rmp, which is convenient for clinker transportation; the third-stage cooling device 5-3 is a grate cooler, and the cooling residual air outlet of the third-stage cooling device 5-3 is connected to the cyclone dust collector 7 and the bag dust collector 8 in sequence, and the flue gas outlet of the bag dust collector is connected to the air supply port of the middle section of the grate cooler. The third-stage cooling residual air outlet is connected to the cyclone dust collector and the bag dust collector to collect fine powder, and part of the residual air is circulated and applied to the middle section of the grate cooler to achieve the purpose of slow cooling below 500°C in the third-stage cooling, and heat is recycled.
[0079] The crude liquid carbonation separation system includes an alkali liquid dissolution device, a separation and washing device, a crude liquid carbonation separation device and an aluminum hydroxide roasting device. The aluminum-based clinker outlet of the three-stage cooling system is connected to the feed inlet of the alkali liquid dissolution device, the dissolution liquid outlet of the alkali liquid dissolution device is connected to the liquid inlet of the separation and washing device, the liquid outlet of the separation and washing device is connected to the liquid inlet of the crude liquid carbonation separation device, the air outlet of the top cyclone separator of the first row of cyclone preheaters is connected to the air inlet of the crude liquid carbonation separation device, the aluminum hydroxide outlet of the crude liquid carbonation separation device is connected to the inlet of the aluminum hydroxide roasting device, and the outlet of the aluminum hydroxide roasting device is an aluminum oxide product.
[0080] A method for extracting aluminum based on the above system that can realize carbon utilization includes the following steps:
[0081] The aluminum-containing raw materials and limestone are mixed in a certain proportion, and the mixed raw materials are ground to prepare raw meal powder with particle size meeting the requirements.
[0082] The raw meal powder is fed into the first row cyclone preheater and the second row cyclone preheater at a predetermined feeding ratio, and the raw meal powder is heat exchanged and gas-solid separated with the corresponding flue gas in each cyclone preheater;
[0083] The raw meal preheated by the first row of cyclone preheaters enters the first decomposition furnace, and the raw meal preheated by the second row of cyclone preheaters enters the second decomposition furnace;
[0084] High-purity oxygen with a concentration of 80-99% is mixed with high-temperature tertiary air and enters the first decomposition furnace. The large amount of heat released by the combustion of fuel in the first decomposition furnace is used for the raw material in the first decomposition furnace to absorb heat and decompose, thereby obtaining hot raw material and generating a large amount of flue gas. The flue gas generated in the first decomposition furnace enters the first row of cyclone preheaters and exchanges heat with the raw material to become low-temperature flue gas. The low-temperature flue gas is discharged through the air outlet of the cyclone separator at the top of the first row of cyclone preheaters, and enters the crude liquid carbonation separation system to perform carbonation separation on the dissolved liquid. The temperature range of this low-temperature flue gas is 200-350°C, and the wet-basis CO2 concentration in the low-temperature flue gas is 30-50%, the O2 concentration is 2-4%, the N2 concentration is 28-50%, and the H2O concentration is 8-20%;
[0085] The kiln gas enters the second decomposition furnace through the kiln tail smoke chamber 3, and the high-temperature tertiary air enters the second decomposition furnace. The large amount of heat released by the fuel combustion is used for the raw material in the second decomposition furnace to absorb heat and decompose, obtaining hot raw material and generating a large amount of flue gas. The flue gas generated in the second decomposition furnace enters the second row of cyclone preheaters to exchange heat with the raw material to become low-temperature flue gas. The low-temperature flue gas is discharged through the air outlet of the cyclone separator at the top of the second row of cyclone preheaters, and the waste heat is utilized. The temperature range of this low-temperature flue gas is 240-450℃, and the wet-basis CO2 concentration in the low-temperature flue gas is 10-20%. This low-temperature flue gas enters the flue gas treatment system after recovering part of the heat through the waste heat recovery and utilization system, and enters the chimney and is discharged into the atmosphere after the flue gas treatment.
[0086] The hot raw materials generated in the first decomposition furnace and the second decomposition furnace enter the rotary kiln 4 through the kiln tail smoke chamber 3, and are calcined in the rotary kiln 4 to form high-temperature aluminum-based compound clinker. Fuel burns in the rotary kiln 4 to generate kiln gas, and the high-temperature aluminum-based compound clinker enters the three-stage cooling system 5 from the outlet of the rotary kiln 4 to exchange heat with air to obtain cooled aluminum-based clinker.
[0087] Three-stage cooling of high-temperature aluminum-based compound clinker:
[0088] First stage cooling: mechanical pushing and compressed air blowing are used to transform the liquid phase on the surface of high-temperature aluminum-based compound clinker particles into a solid state;
[0089] Second stage cooling: Use a single-drum cooler to slowly cool the clinker from 1200-1300℃ to 700-900℃ after primary cooling. The cooling time is 30-60min, so that the optimal phase composition of the clinker is C12 A7;
[0090] Third stage cooling: The grate cooler is used to cool the clinker after the second stage cooling from 700-900℃ to 400-500℃ for 10-20min; then it is slowly cooled from 400-500℃ to 70-100℃ for 40-80min. The temperature of the residual cooling air is 80-120℃ after the cyclone dust collector and bag dust collector, and part of it returns to the middle air supply of the grate cooler of the third stage cooling.
[0091] The aluminum-containing clinker product is dissolved with alkaline solution, separated and washed to obtain crude sodium aluminate liquid and waste residue. The crude sodium aluminate liquid fully reacts with the high CO2 concentration gas produced by the CO2 concentration, preheating and predecomposition system to obtain sodium carbonate solution and aluminum hydroxide. The aluminum hydroxide is roasted to obtain finished alumina.
[0092] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in the relevant field can still modify or replace the specific implementation methods of the present invention with equivalents, such as other implementation cases: Raw material preparation: aluminum-containing raw materials and limestone are mixed to prepare raw material powder; clinker and medium CO2 concentration flue gas preparation: raw material powder is fed into the CO2 concentration preheating and predecomposition system and the energy-saving preheating system in proportion, and then all enter the CO2 concentration preheating and predecomposition system decomposition furnace, and then calcined, three-stage Cooling to obtain aluminum-based clinker products; high-purity O2 and high-temperature kiln gas enter the decomposition furnace, and the CO2 concentration preheating and predecomposition system discharges low-temperature flue gas with medium CO2 concentration at the top outlet; high-temperature tertiary air enters the energy-saving preheating system, and the CO2 concentration in the exhaust flue gas is zero; crude liquid carbonation separation: aluminum-containing clinker products are dissolved with alkaline solution, separated and washed to obtain sodium aluminate crude liquid and waste residue, and the sodium aluminate crude liquid fully reacts with the medium CO2 concentration gas produced by the CO2 concentration preheating and predecomposition system to obtain sodium carbonate solution and aluminum hydroxide products, and the aluminum hydroxide is roasted to obtain finished alumina. Any modifications or equivalent substitutions that do not depart from the spirit and scope of the present invention are within the scope of protection of the claims of the present invention.
Claims
1. A method for extracting aluminum that can achieve carbon utilization, characterized in that: The steps include: Raw material preparation: The aluminum-containing raw materials and limestone are mixed in a certain proportion, and the mixed raw materials are ground to prepare raw meal powder with a particle size that meets the requirements; Clinker preparation and medium CO2 concentration flue gas preparation: The raw meal powder is fed into the CO2 concentration preheating and predecomposition system and the energy-saving preheating and predecomposition system of different equipment specifications at a predetermined feeding ratio, and is respectively fed into the corresponding multi-stage cyclone preheaters of the two preheating and predecomposition systems for gas-solid heat exchange, and then is respectively fed into the corresponding decomposition furnaces of the two preheating and predecomposition systems for calcination and decomposition; The mixed flue gas after high-purity O2 and part of high-temperature tertiary air are mixed into the decomposition furnace of the CO2 concentration preheating and predecomposition system. The mixed flue gas contains 30-50% O2 and 50-70% N2. The high-concentration O2 causes the fuel in the decomposition furnace of the CO2 concentration preheating and predecomposition system to burn and decompose the limestone to produce medium-concentration CO2. The flue gas discharged from the top outlet of the CO2 concentration preheating and predecomposition system is low-temperature medium-concentration CO2 flue gas. The temperature range of the low-temperature medium-concentration CO2 flue gas is 200-350°C. The wet-base CO2 concentration of the low-temperature medium-concentration CO2 flue gas is 30-50%, the O2 concentration is 2-4%, the N2 concentration is 28-50%, and the H2O concentration is 8-20%. The kiln gas and part of the high-temperature tertiary air enter the decomposition furnace of the energy-saving preheating and predecomposition system. The flue gas discharged from the top outlet of the energy-saving preheating and predecomposition system is low-temperature and low-CO2 concentration flue gas. The temperature range of the low-temperature and low-CO2 concentration flue gas is 240-450°C, and the wet-based CO2 concentration in the low-temperature and low-CO2 concentration flue gas is 10-20%; All the hot raw materials after decomposition enter the rotary kiln through the kiln tail smoke chamber for calcination. Kiln gas and high-temperature aluminum-based compound clinker are generated in the rotary kiln. The high-temperature aluminum-based compound clinker is cooled in three stages to obtain aluminum-based clinker products. First stage cooling: mechanical pushing and compressed air blowing are used to transform the liquid phase on the surface of high-temperature aluminum-based compound clinker particles into a solid state; Second stage cooling: Use a single-drum cooler to slowly cool the clinker from 1200-1300℃ to 700-900℃ after primary cooling. The cooling time is 30-60min, so that the phase composition of the clinker is 1200-1300℃, 700-900℃, 700-13 ... 12 A7 is the main one; Third stage cooling: Use a grate cooler to cool the clinker after secondary cooling from 700-900℃ to 400-500℃ for 10-20min; then slowly cool from 400-500℃ to 70-100℃ for 40-80min; Clinker Carbonation Separation: The aluminum-based clinker product is dissolved with alkaline solution, separated and washed to obtain crude sodium aluminate liquid and waste residue; the crude sodium aluminate liquid fully reacts with the medium-concentration CO2 flue gas produced by the CO2 concentration preheating and predecomposition system to obtain sodium carbonate solution and aluminum hydroxide, and the aluminum hydroxide is roasted to obtain alumina finished product.
2. The aluminum extraction method capable of realizing carbon utilization according to claim 1, characterized in that: The residual cooling air after the third stage cooling has a temperature of 80-120℃ after being collected by cyclone and bag dust collector, and part of it returns to the middle air supply of the grate cooler of the third stage cooling.
3. The aluminum extraction method capable of realizing carbon utilization according to claim 1, characterized in that: The raw meal powder feeding ratio of the CO2 concentration preheating and predecomposition system and the energy-saving preheating and predecomposition system is 1:1 to 1:
6.
4. The aluminum extraction method capable of realizing carbon utilization according to claim 1, characterized in that: The O2 concentration in the high-purity O2 is 50-99%.
5. The aluminum extraction method capable of realizing carbon utilization according to claim 1, characterized in that: The low-temperature and low-CO2 concentration flue gas discharged from the outlet of the energy-saving preheating and predecomposition system recovers part of the heat through the waste heat recovery system and then enters the flue gas treatment system. After the flue gas treatment, it enters the chimney and is discharged into the atmosphere.
6. An aluminum extraction system capable of realizing carbon utilization, characterized in that: It includes a CO2 concentration preheating and predecomposition system, an energy-saving preheating and predecomposition system, a kiln tail smoke chamber, a rotary kiln, a three-stage cooling system, a tertiary air duct and a crude liquid carbonation separation system. The energy-saving preheating and predecomposition system, the kiln tail smoke chamber, the rotary kiln and the three-stage cooling system are connected in sequence. The tertiary air duct connects the three-stage cooling system and the decomposition furnace of the energy-saving preheating and predecomposition system; the aluminum-based clinker product outlet of the three-stage cooling system is connected to the crude liquid carbonation separation system; The CO2 concentration, preheating and predecomposition system includes a first decomposition furnace and a first row of cyclone preheaters; a first burner is arranged on the first decomposition furnace, a high-purity oxygen inlet is connected to the bottom of the first decomposition furnace, the bottom of the first decomposition furnace is connected to the tertiary air duct, and a first row of raw material inlet is opened on the first decomposition furnace; the air inlet of the cyclone separator at the bottom end of the first row of cyclone preheaters is connected to the air outlet pipe of the first decomposition furnace, and the air outlet of the cyclone separator at the top end of the first row of cyclone preheaters discharges low-temperature medium CO2 concentration flue gas, and the air outlet of the cyclone separator at the top end of the first row of cyclone preheaters is connected to the crude liquid carbonation separation system; the feed inlet of the cyclone separator at the top end of the first row of cyclone preheaters is used for feeding raw material powder, and the discharge port of the cyclone separator at the bottom end of the first row of cyclone preheaters is connected to the kiln tail smoke chamber.
7. The aluminum extraction system capable of realizing carbon utilization according to claim 6 is characterized in that: The three-stage cooling system includes a first-stage cooling device, a second-stage cooling device and a third-stage cooling device which are connected in sequence. The first-stage cooling device includes a first-stage cooling cavity. A mechanical pushing component is provided at the material dropping position of the first-stage cooling cavity. The bottom of the first-stage cooling cavity is a material dropping slope. The material dropping slope has an angle of ≥50°. The mechanical pushing component pushes the clinker onto the material dropping slope. The material dropping slope is made of anti-scaling refractory material. A plurality of compressed air blowing ports are arranged on the material dropping slope. Compressed air is blown to transform the liquid phase on the surface of the clinker particles into a solid state, and the clinker particles smoothly enter the second-stage cooling device. The second-stage cooling device is a single-cylinder cooler. The third-stage cooling device is a grate cooler. The cooling residual air outlet of the third-stage cooling device is connected to a cyclone dust collecting device and a bag dust collecting device in sequence. The smoke outlet of the bag dust collecting device is connected to the middle air supply port of the grate cooler.
8. The aluminum extraction system capable of realizing carbon utilization according to claim 7, characterized in that: The second stage cooling device is arranged to be tilted downward from its inlet to its outlet, with an inclination angle of 1-5° and a rotation speed of 0.5-5 rpm.
9. The aluminum extraction system capable of realizing carbon utilization according to claim 6, characterized in that: The crude liquid carbonation separation system includes an alkali liquid dissolution device, a separation and washing device, a crude liquid carbonation separation device and an aluminum hydroxide roasting device. The aluminum-based clinker outlet of the three-stage cooling system is connected to the feed inlet of the alkali liquid dissolution device, the dissolution liquid outlet of the alkali liquid dissolution device is connected to the liquid inlet of the separation and washing device, the liquid outlet of the separation and washing device is connected to the liquid inlet of the crude liquid carbonation separation device, the air outlet of the top cyclone separator of the first row of cyclone preheaters is connected to the air inlet of the crude liquid carbonation separation device, the aluminum hydroxide outlet of the crude liquid carbonation separation device is connected to the inlet of the aluminum hydroxide roasting device, and the outlet of the aluminum hydroxide roasting device is an aluminum oxide product.
10. The aluminum extraction system capable of realizing carbon utilization according to claim 6, characterized in that: The CO2 concentration, preheating and predecomposition system also includes an emergency discharge pipe, one end of which is connected to the bottom end of the first decomposition furnace, and the other end of which is connected to the kiln tail smoke chamber.
11. The aluminum extraction system capable of realizing carbon utilization according to claim 6, characterized in that: The first row of raw material inlets is provided with a plurality of inlets.
12. The aluminum extraction system capable of realizing carbon utilization according to claim 6, characterized in that: The energy-saving preheating and precalcining system comprises a second calcining furnace and a second row of cyclone preheaters, the second calcining furnace is provided with a second burner, the second calcining furnace is connected with the tertiary air duct and the kiln tail smoke chamber, and the second calcining furnace is provided with a second row of raw material inlets; The air inlet of the cyclone separator at the bottom end of the second row of cyclone preheaters is connected to the air outlet pipe of the second decomposition furnace, and the air outlet of the cyclone separator at the top end of the second row of cyclone preheaters discharges low-temperature and low-CO2 concentration flue gas; the feed port of the cyclone separator at the top end of the second row of cyclone preheaters is used for feeding raw material powder, the discharge port of the second-to-last cyclone separator of the second row of cyclone preheaters is connected to the second decomposition furnace, and the discharge port of the cyclone separator at the bottom end of the second row of cyclone preheaters is connected to the kiln tail smoke chamber.