Preparation method of calcium hydroxide with high specific surface area, calcium hydroxide and application
By reacting graphene oxide modified concave and convex rod soil with calcium salt, high specific surface area calcium hydroxide was prepared, solving the problems of high cost and low performance, and achieving higher surface area and stronger desulfurization performance.
Patent Information
- Application Number
- CN202410951602.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-26
AI Technical Summary
The high specific surface area calcium hydroxide has high preparation cost and is low in performance when used as a desulfurizer.
By modifying graphene oxide with concave and concave rod earth, graphene oxide particles are embedded in the concave and concave rod earth structure, mixed with calcium salt and reacted with liquid alkali, calcium hydroxide with a high specific surface area is prepared to avoid particles agglomeration and improve their Dispersibility and reactivity.
The preparation cost of calcium hydroxide is reduced, its specific surface area and desulfurization properties are significantly improved, and its penetration ability and efficiency as a desulfurization agent are enhanced.
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of calcium hydroxide, and in particular to a preparation method of high specific surface area calcium hydroxide, calcium hydroxide and applications. Background Art
[0002] Calcium hydroxide with a high specific surface area (commonly known as active calcium hydroxide or highly active lime) has a higher reactivity due to its larger surface contact area, which makes it widely used in multiple industries; among them, desulfurization agent is an important application of calcium hydroxide with a high specific surface area.
[0003] However, the current preparation cost of high specific surface area calcium hydroxide is relatively high, the specific surface area is relatively low, and the performance as a desulfurization agent is relatively low. Summary of the invention
[0004] In order to solve at least one of the above technical problems, a calcium hydroxide with low preparation cost, high specific surface area and good effect when used as a desulfurizer is developed. The present application provides a preparation method of high specific surface area calcium hydroxide, calcium hydroxide and application.
[0005] On the one hand, the present application provides a method for preparing calcium hydroxide with a high specific surface area, characterized in that it comprises the following steps:
[0006] S1 Preparation of graphene oxide modified attapulgite
[0007] Adding graphene oxide to attapulgite, adding water to mix evenly, and drying to obtain modified attapulgite;
[0008] S2 Preparation of Calcium Hydroxide
[0009] The modified attapulgite and calcium salt in S1 are mixed evenly with water, and an excess amount of liquid alkali is added to react. The solid is obtained by centrifugal filtration, and the solid is washed with water and dried to obtain calcium hydroxide powder.
[0010] Optionally, in S1, the graphene oxide has a diameter of 0.01 to 15 μm, a thickness of 0.55 to 3.85 nm, a number of layers of less than 10, and a purity of more than 99% wt.
[0011] Optionally, in S1, the particle size of the attapulgite is 0.2 to 1 μm.
[0012] Optionally, in S1, the weight ratio of graphene oxide to attapulgite is 1:50-120.
[0013] Optionally, in S1, the drying temperature is 200-250°C.
[0014] Optionally, in S2, the weight ratio of the modified attapulgite to the calcium content in the calcium salt is 1:20 to 50.
[0015] In a second aspect, the present application provides calcium hydroxide with a high specific surface area prepared by the above preparation method.
[0016] In a third aspect, the present application provides the application of the above-mentioned high specific surface area calcium hydroxide in the field of desulfurization agent.
[0017] In summary, in the process of preparing calcium hydroxide, the present application first modifies attapulgite by graphene oxide, so that the graphene oxide particles are partially embedded in the structural channels inside the attapulgite; the modified attapulgite is then mixed with a calcium salt and reacted with liquid alkali. Since the attapulgite itself is negatively charged, the high conductivity of graphene oxide and the negative charge of calcium hydroxide particles make the prepared calcium hydroxide particles not agglomerate and disperse more evenly, thereby obtaining calcium hydroxide with a higher specific surface area. DETAILED DESCRIPTION
[0018] The present application is further described in detail below with reference to the embodiments.
[0019] In the technical solution of this application, the main components involved, unless otherwise specified, are purchased from commercially available products.
[0020] Attapulgite: particle size is 0.2~1μm.
[0021] Graphene oxide: diameter 0.01-15 μm, thickness 0.55-3.85 nm, number of layers <10, purity >99% wt. Specific embodiments
[0023] Example 1
[0024] This embodiment discloses a method for preparing calcium hydroxide with a high specific surface area, comprising the following steps:
[0025] Adding graphene oxide to attapulgite, adding water to mix evenly, and drying at 200° C. to obtain modified attapulgite;
[0026] The weight ratio of graphene oxide to attapulgite is 1:50.
[0027] The modified attapulgite prepared above and the calcium salt are mixed evenly with water, and the weight ratio of the modified attapulgite to the calcium content in the calcium salt is 1:20. Liquid alkali is added to react, centrifuged and filtered to obtain a solid, which is washed with water and dried to obtain calcium hydroxide powder.
[0028] Example 2
[0029] This embodiment discloses a method for preparing calcium hydroxide with a high specific surface area, comprising the following steps:
[0030] Adding graphene oxide to attapulgite, adding water to mix evenly, and drying at 200° C. to obtain modified attapulgite;
[0031] The weight ratio of graphene oxide to attapulgite is 1:60.
[0032] The modified attapulgite prepared above and the calcium salt are mixed evenly with water, and the weight ratio of the modified attapulgite to the calcium content in the calcium salt is 1:30. Liquid alkali is added to react, centrifuged and filtered to obtain a solid, which is washed with water and dried to obtain calcium hydroxide powder.
[0033] Example 3
[0034] This embodiment discloses a method for preparing calcium hydroxide with a high specific surface area, comprising the following steps:
[0035] Adding graphene oxide to attapulgite, adding water to mix evenly, and drying at 200° C. to obtain modified attapulgite;
[0036] The weight ratio of graphene oxide to attapulgite is 1:70.
[0037] The modified attapulgite prepared above and the calcium salt are mixed evenly with water, and the weight ratio of the modified attapulgite to the calcium content in the calcium salt is 1:40. Liquid alkali is added to react, centrifuged and filtered to obtain a solid, which is washed with water and dried to obtain calcium hydroxide powder.
[0038] Example 4
[0039] This embodiment discloses a method for preparing calcium hydroxide with a high specific surface area, comprising the following steps:
[0040] Adding graphene oxide to attapulgite, adding water to mix evenly, and drying at 200° C. to obtain modified attapulgite;
[0041] The weight ratio of graphene oxide to attapulgite is 1:80.
[0042] The modified attapulgite prepared above and the calcium salt are mixed evenly with water, and the weight ratio of the modified attapulgite to the calcium content in the calcium salt is 1:50. Liquid alkali is added to react, centrifuged and filtered to obtain a solid, which is washed with water and dried to obtain calcium hydroxide powder.
[0043] Example 5
[0044] This embodiment discloses a method for preparing calcium hydroxide with a high specific surface area, comprising the following steps:
[0045] Adding graphene oxide to attapulgite, adding water to mix evenly, and drying at 200° C. to obtain modified attapulgite;
[0046] The weight ratio of graphene oxide to attapulgite is 1:90.
[0047] The modified attapulgite prepared above and the calcium salt are mixed evenly with water, and the weight ratio of the modified attapulgite to the calcium content in the calcium salt is 1:20. Liquid alkali is added to react, centrifuged and filtered to obtain a solid, which is washed with water and dried to obtain calcium hydroxide powder.
[0048] Example 6
[0049] This embodiment discloses a method for preparing calcium hydroxide with a high specific surface area, comprising the following steps:
[0050] Adding graphene oxide to attapulgite, adding water to mix evenly, and drying at 200° C. to obtain modified attapulgite;
[0051] The weight ratio of graphene oxide to attapulgite is 1:100.
[0052] The modified attapulgite prepared above and the calcium salt are mixed evenly with water, and the weight ratio of the modified attapulgite to the calcium content in the calcium salt is 1:30. Liquid alkali is added to react, centrifuged and filtered to obtain a solid, which is washed with water and dried to obtain calcium hydroxide powder.
[0053] Example 7
[0054] This embodiment discloses a method for preparing calcium hydroxide with a high specific surface area, comprising the following steps:
[0055] Adding graphene oxide to attapulgite, adding water to mix evenly, and drying at 200° C. to obtain modified attapulgite;
[0056] The weight ratio of graphene oxide to attapulgite is 1:110.
[0057] The modified attapulgite prepared above and the calcium salt are mixed evenly with water, and the weight ratio of the modified attapulgite to the calcium content in the calcium salt is 1:40. Liquid alkali is added to react, centrifuged and filtered to obtain a solid, which is washed with water and dried to obtain calcium hydroxide powder.
[0058] Example 8
[0059] This embodiment discloses a method for preparing calcium hydroxide with a high specific surface area, comprising the following steps:
[0060] Adding graphene oxide to attapulgite, adding water to mix evenly, and drying at 200° C. to obtain modified attapulgite;
[0061] The weight ratio of graphene oxide to attapulgite is 1:120.
[0062] The modified attapulgite prepared above and the calcium salt are mixed evenly with water, and the weight ratio of the modified attapulgite to the calcium content in the calcium salt is 1:50. Liquid alkali is added to react, centrifuged and filtered to obtain a solid, which is washed with water and dried to obtain calcium hydroxide powder.
[0063] Comparative Example 1
[0064] This comparative example discloses a method for preparing calcium hydroxide with a high specific surface area. The difference from Example 1 is that this comparative example does not add graphene oxide; specifically, the following steps are included:
[0065] Add water to evenly mix the attapulgite and calcium salt, wherein the weight ratio of the calcium content in the attapulgite to the calcium salt is 1:20, add liquid alkali for reaction, centrifuge to obtain a solid, wash with water, and dry to obtain calcium hydroxide powder.
[0066] Comparative Example 2
[0067] This comparative example discloses a method for preparing calcium hydroxide with a high specific surface area. The difference from Example 2 is that this comparative example does not add graphene oxide; specifically, the following steps are included:
[0068] Add water to evenly mix the attapulgite and calcium salt, wherein the weight ratio of the calcium content in the attapulgite to the calcium salt is 1:30, add liquid alkali for reaction, centrifuge to obtain a solid, wash with water, and dry to obtain calcium hydroxide powder.
[0069] Comparative Example 3
[0070] This comparative example discloses a method for preparing calcium hydroxide with a high specific surface area, wherein graphene oxide and attapulgite are not added in this comparative example; the method specifically comprises the following steps:
[0071] The calcium salt is added to the liquid alkali for reaction, and the solid is obtained by centrifugation and filtration. The solid is washed with water and dried to obtain calcium hydroxide powder.
[0072] The specific surface area of the calcium hydroxide powders prepared in Examples 1 to 8 and Comparative Examples 1 to 3 was tested, and the test results are shown in Table 1.
[0073] The desulfurization performance of the calcium hydroxide powder obtained in Examples 1 to 8 and Comparative Examples 1 to 3 was tested by a fixed bed reactor experiment. The fixed bed reactor used had an inner diameter of 12 mm and a length of 300 mm. The simulated flue gas composition was a mixed gas of SO2, CO2, O2, and N2, wherein the SO2 concentration was 500 ppmV, the volume fractions of CO2 and O2 were 10% and 5%, respectively, and the remainder was N2. The flue gas flow rate was 1000 mL / min, and an infrared gas analyzer was used to analyze the SO2 content at the reactor outlet. For all samples, the loading amount in the reactor was 30 mL. The time from the start of flue gas introduction to the time when the SO2 content in the reactor outlet gas reaches 20 ppm is defined as the desulfurization penetration time of the corresponding adsorbent, and the test results are shown in Table 1.
[0074] Table 1 Specific surface area test results of calcium hydroxide prepared in Examples 1 to 8 and Comparative Examples 1 to 3
[0075] Calcium hydroxide <![CDATA[Specific surface area / m 2 ·g -1 > Penetration time / s Example 1 42.1 5860 Example 2 42.6 6010 Example 3 43.4 5930 Example 4 45.7 6110 Example 5 47.9 6240 Example 6 46.7 5980 Example 7 44.9 5910 Example 8 43.4 5960 Comparative Example 1 23.2 1940 Comparative Example 2 25.9 2010 Comparative Example 3 13.5 1590
[0076] It can be seen from Examples 1 to 8, Comparative Examples 1 to 3 and Table 1 that after adding attapulgite modified with graphene oxide in the technical solution of the present application, the specific surface area of the calcium hydroxide prepared is greatly increased, and when used as a desulfurizer, the penetration time is improved and the desulfurization performance is stronger.
[0077] It can be seen from Comparative Examples 1 to 2 that after only adding attapulgite, the specific surface area of calcium hydroxide and the effect of using it as a desulfurizer are slightly improved. Therefore, only adding attapulgite cannot well improve the comprehensive performance of the prepared calcium hydroxide.
[0078] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing high specific surface area calcium hydroxide, characterized in that: The following steps are involved: S1 Preparation of graphene oxide modified attapulgite Adding graphene oxide to attapulgite, adding water to mix evenly, and drying to obtain modified attapulgite; S2 Preparation of Calcium Hydroxide The modified attapulgite and calcium salt in S1 are mixed evenly with water, and an excess amount of liquid alkali is added to react. The solid is obtained by centrifugal filtration, and the solid is washed with water and dried to obtain calcium hydroxide powder.
2. The preparation method according to claim 1, characterized in that: In the S1, the graphene oxide has a diameter of 0.01 to 15 μm, a thickness of 0.55 to 3.85 nm, a layer number of less than 10, and a purity of more than 99% wt.
3. The preparation method according to claim 1, characterized in that: In the S1, the particle size of the attapulgite is 0.2 to 1 μm.
4. The preparation method according to claim 1, characterized in that: In the S1, the weight ratio of graphene oxide to attapulgite is 1:50-120.
5. The preparation method according to claim 1, characterized in that: In the step S1, the drying temperature is 200-250°C.
6. The preparation method according to claim 1, characterized in that: In the S2, the weight ratio of the modified attapulgite to the calcium content in the calcium salt is 1:20-50.
7. A high specific surface area calcium hydroxide prepared by the preparation method according to claim 1.
8. Use of the high specific surface area calcium hydroxide according to claim 7 in the field of desulfurization agents.
Citation Information
Cited By
Preparation method and preparation system of calcium hydroxide with high specific surface area
CN120309203A