Fabricated precast concrete slab suitable for oil drilling platform
Through the design of ultra-high performance concrete, combined with admixtures such as carbon nanotubes and polyimide fibers, the high cost and environmental pollution problems during the construction and demolition of the concrete platform of the petroleum drilling platform are solved, and the strength and durability of the concrete are improved. Efficient crack repair and crack resistance are achieved.
Patent Information
- Application Number
- CN202411121773.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
The concrete platforms of existing oil drilling platforms have high costs, environmental pollution, poor durability and poor anti-slip performance during construction and demolition, and conventional concrete is prone to cracks that affect integrity and safety.
Prefabricated precast concrete slabs are prepared using ultra-high performance concrete, containing cement, fly ash, silica fume, metakaolin, steel fiber, water reducer, quartz sand and admixtures, including carbon nanotube grafted polyethyleneimine /Polyimide fiber copolymer, sodium silicate modified polyvinyl alcohol and silicone amide improve interfacial strength and crack resistance through chemical bonding and physical meshing.
It significantly improves the compressive, flexural, tensile strength and durability of concrete, delays the development of cracks, enhances the mechanical properties and self-healing and repairing capabilities of the materials, meets the load requirements of heavy-load machinery construction and reduces environmental pollution.
Smart Images

Figure CN119019121A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete, and in particular to an assembled prefabricated concrete panel suitable for an oil drilling platform. Background Art
[0002] Due to the heavy weight of oil drilling equipment, a solid drilling platform needs to be set up at the bottom when the equipment is working. Conventionally, cast-in-place thick ordinary concrete or heavy steel plates are used.
[0003] There are the following problems with cast-in-place ordinary concrete: 1. The on-site concrete pouring requires a large workload, the concrete needs to be cured, and the overall operation time is long; 2. Cast-in-place concrete is a one-time investment, the platform cannot be reused, and the cost is high; 3. After the drilling operation is completed, the concrete platform needs to be chiseled off, which is extremely labor-intensive and expensive; 4. A large amount of wastewater, waste residue, noise and other pollution sources will be generated during the on-site concrete pouring and demolition process, which is extremely unfriendly to the environment.
[0004] Heavy steel plates have the following problems: 1. The steel plates are heavy, and their installation and removal require high lifting equipment. In addition, the steel plates are expensive, and the overall construction costs are high; 2. The anti-slip performance of steel plates is poorer than that of concrete; 3. Steel plates are prone to rust, have poor durability, and have a limited turnover rate.
[0005] In addition, under the influence of external forces, temperature changes, humidity changes, etc., ordinary concrete is prone to cracks, which will affect the integrity, durability, and even stability and safety of the building. Ordinary concrete has a low water-binder ratio. As the degree of hydration deepens, the internal humidity continues to decrease, and it is easy to form a concave liquid surface in the slurry, which in turn produces microcracks inside the concrete, affecting its strength and volume stability. Heavy steel plates are prone to rust.
[0006] At present, the methods used to improve the impermeability of concrete are: adding some mineral admixtures such as mineral powder and aggregate to the concrete to improve the impermeability of concrete; or coating the concrete surface with polyurethane resin, epoxy resin, styrene acrylic emulsion, pure acrylic emulsion protective coating to isolate the concrete from harmful elements. However, the above methods cannot play a very effective protective role for concrete cracks. Summary of the invention
[0007] The purpose of the present invention is to provide an assembled prefabricated concrete panel suitable for oil drilling platforms, which has high strength, a compressive strength of 130MPa, a flexural strength of 22MPa, a tensile strength of 6MPa, an elastic modulus of 45GPa, and a bulk density of 2450Kg / m3.
[0008] The embodiments of the present invention are implemented by the following technical solutions:
[0009] An assembled prefabricated concrete panel suitable for an oil drilling platform, the prefabricated concrete panel being prepared by ultra-high performance concrete, the ultra-high performance concrete comprising the following raw materials in parts by weight: 680-720 parts of cement, 180-220 parts of fly ash, 140-160 parts of silica fume, 40-60 parts of metakaolin, 145-160 parts of steel fiber, 10-20 parts of water reducer, 180-200 parts of water, 240-270 parts of quartz sand and 50-100 parts of admixture;
[0010] The additive comprises 20-30 parts of carbon nanotube grafted polyethyleneimine / polyimide fiber copolymer, 20-30 parts of sodium silicate modified polyvinyl alcohol and 10-20 parts of silicone amide.
[0011] The technical solution of the embodiment of the present invention has at least the following advantages and beneficial effects:
[0012] In the present invention, the amino groups in polyethyleneimine react chemically with the acyl chloride on the surface of the polyimide fiber to generate amide groups, polyethyleneimine is grafted onto the surface of the polyimide fiber, and the amino groups are introduced onto the surface of the polyimide fiber to greatly increase the reaction activity of the surface, and the carbon nanotubes grafted onto the fiber surface can increase the roughness of the fiber surface and also serve as a bridge for physical engagement with the oligomer matrix, overcoming the disadvantage that the molecular chains on the surface of the polyimide fiber are rigid and difficult to effectively bond and physically engage with the matrix material, greatly increasing the interface strength of the organic-inorganic composite material, and giving the material better mechanical properties. When microcracks appear in the concrete, a large number of polyimide fibers pass through the bending fracture period to form microcracks, allowing the microcracks in the concrete to be completely bridged by the polyimide fibers, delaying the development of the microcracks, making it difficult for it to debond from the matrix, and bearing greater stress through the bridging fibers, thereby enhancing the mechanical properties of the concrete. Polyethyleneimine can react with the hydroxyl groups on the surface of carbon nanotubes to form chemical bonds, reduce the mutual attraction between carbon nanotubes, effectively avoid strong agglomeration effects, and thus improve the dispersibility of carbon nanotubes in the solution. At the same time, polyethyleneimine is covalently grafted with carbon nanotubes through chemical covalent bonds, and the two are difficult to separate and fall off, which avoids the dissolution of polyethyleneimine, improves the adsorption of polyethyleneimine on cement particles, and improves the mud resistance and collapse resistance of concrete.
[0013] The molecular chain of silicone amide contains Si-O bonds, which can condense to form stable Si-OS i bonds, or react with active points on the surface of cement particles to form chemical bonds, forming a high-strength and durable gelling system, enhancing the bonding force between silicone amide and cement particles, and improving the water resistance and stability of concrete. Furthermore, silicone amide can participate in cement hydration, anchor on the inner and outer surfaces of concrete, form a dense hydrophobic film, improve the strength, water permeability and durability of concrete; can fill concrete pores, reduce concrete porosity, improve the compactness and impermeability of concrete, and thus protect concrete from water erosion. In addition, the amino ester bonds in silicone amide can be adsorbed on the surface of cement particles with negative charges. On the one hand, it can increase the adhesion between silicone amide and cement particles, significantly improve the strength of concrete, reduce the bonding force between cement particles, make it easier to disperse in water, and improve the fluidity and workability of concrete; on the other hand, silicone amide can form steric hindrance between concrete, giving concrete superior collapse resistance.
[0014] Sodium silicate and polyvinyl alcohol undergo self-condensation to form chemical bonds such as Si-OC and Si-O-Si, construct a network cross-linked structure with flexible molecular segments, form a chemical cross-linking reinforcement effect, fill or attach to the micro-voids and micro-cracks inside the concrete, form a physical support reinforcement effect, and improve the compressive strength and splitting tensile strength of the concrete. When cracks appear in the concrete and there is water in the cracks, polyvinyl alcohol undergoes a new dissolution and film-forming reaction in the water, allowing the damaged concrete to self-repair. At the same time, sodium silicate can be enriched in the cracks and react with a large amount of calcium ions, chloride ions, etc. in the concrete. They will react with silicates to form water-insoluble crystals. The crystals absorb water and expand in the cracks, from sparse to dense, and gradually form a dense crystal filling area in the depth of the cracks, thereby achieving the function of crack repair. By being reactivated by water, the concrete has the function of repeated self-healing and repair.
[0015] Steel fibers can be randomly distributed in concrete to form a nested mesh structure, thus having the effect of fine reinforcement and effectively improving the compressive strength of concrete. In addition, randomly distributed steel fibers can play a bridging role, connecting the cementitious system in concrete, allowing them to entangle and bond to form a larger network cross-linked structure, enhancing their steric hindrance effect inside the concrete, effectively hindering the expansion of micro cracks inside the concrete and the formation of macro cracks, significantly improving the tensile, bending, impact and fatigue resistance of concrete, and having good ductility. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 A schematic diagram of the structure of a precast concrete slab provided in an embodiment of the present invention;
[0017] Figure 2 A schematic structural diagram of an assembled precast concrete slab provided in an embodiment of the present invention.
[0018] Icons: 1-precast concrete panel, 2-tenon, 3-mortise and tenon, 4-protruding pattern. DETAILED DESCRIPTION
[0019] The present invention is further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form. Unless otherwise specified, the raw materials and reagents used in the embodiments of the present invention are conventionally purchased raw materials and reagents.
[0020] An assembled prefabricated concrete panel suitable for an oil drilling platform, the prefabricated concrete panel being prepared by ultra-high performance concrete, the ultra-high performance concrete comprising the following raw materials in parts by weight: 680-720 parts of cement, 180-220 parts of fly ash, 140-160 parts of silica fume, 40-60 parts of metakaolin, 145-160 parts of steel fiber, 10-20 parts of water reducer, 180-200 parts of water, 240-270 parts of quartz sand and 50-100 parts of admixture;
[0021] The additive comprises 20-30 parts of carbon nanotube grafted polyethyleneimine / polyimide fiber copolymer, 20-30 parts of sodium silicate modified polyvinyl alcohol and 10-20 parts of silicone amide.
[0022] The inorganic glass and oxides in fly ash can participate in the hydration reaction to form new hydration products, further increasing the strength of concrete. Fly ash also contains a small amount of soluble silicates, which combine with hydroxide in water to form silicate gel, enhancing the toughness and impermeability of concrete. The iron oxide and calcium silicate in fly ash can form relatively stable calcium sulfoaluminate compounds with sulfates, reducing the corrosive effect of sulfates on concrete, making concrete more durable under some special environmental conditions. Fly ash and silica fume can fill the microscopic pores in concrete, reduce the porosity in cement paste, increase the homogeneity of concrete, and improve the density of concrete. It can also fill the microscopic cracks in concrete and improve the crack resistance of concrete.
[0023] Metakaolin can improve the pore structure of concrete, reduce the number of capillaries and cracks, reduce the permeability of concrete, and inhibit the alkali-quartz sand reaction to improve the durability of concrete. Metakaolin can also play a filling effect in concrete, reduce the gaps between cement particles, improve the porosity and pore structure in the hardened body, form a denser filling structure and a micro-level self-tight stacking system, and improve the mechanical properties and durability of concrete.
[0024] Polyethyleneimine contains a large number of positively charged amine groups, which can be adsorbed on the surface of negatively charged cement particles, significantly reducing the intercalation adsorption consumption of water reducer molecules on clay minerals such as kaolin, and improving the anti-clay performance. At the same time, a large number of phosphites with two negative charges are introduced into the polyethyleneimine molecules, which can be adsorbed on the surface of positively charged cement particles to disperse the cement particles. It exists in the form of aggregates in aqueous solution, and the steric hindrance effect of the aggregates can effectively disperse the cement particles. Carbon nanotubes have an excellent aspect ratio, which can extend the transmission path of water molecules and delay the corrosion of concrete. The rich hydroxyl groups in carbon nanotubes can enhance the compressive properties of cement.
[0025] Sodium silicate and polyvinyl alcohol undergo self-condensation to form chemical bonds such as Si-OC and S iOS i, constructing a network cross-linked structure with flexible molecular segments, forming a chemical cross-linking reinforcement effect, filling or attaching to the micro-voids and micro-cracks inside the concrete, forming a physical support reinforcement effect, and improving the compressive strength and splitting tensile strength of the concrete.
[0026] The Si-O bonds contained in silicone amide can condense to form stable Si-O-Si bonds, and can also react with the active points on the surface of cement particles to form chemical bonds, forming a high-strength and durable gelling system, enhancing the bonding force between silicone amide and cement particles, and improving the water resistance and stability of concrete. The amino ester bonds in silicone amide can be adsorbed on the surface of negatively charged cement particles. On the one hand, it can increase the adhesion between silicone amide and cement particles, significantly improve the strength of concrete, and reduce the bonding force between cement particles, making it easier to disperse in water, improving the fluidity and workability of concrete; on the other hand, silicone amide can form steric hindrance between concrete, giving concrete superior collapse resistance.
[0027] Furthermore, the preparation method of the admixture is: dissolving silicone amide in an ethanol solution, adding sodium dodecyl sulfate to prepare an emulsion; adding carbon nanotube grafted polyethyleneimine / polyimide fiber copolymer to the emulsion, stirring and mixing, and then dropping a sodium silicate modified polyvinyl alcohol solution dissolved in water, and drying to obtain the admixture.
[0028] Among them, the admixture is a capsule-like structure with silicone amide as the core, carbon nanotube grafted polyethyleneimine as the doping enhancer, and sodium silicate modified polyvinyl alcohol as the wall. In this way, concrete cracks can be filled and repaired by sodium silicate modified polyvinyl alcohol first, allowing the concrete to heal itself, while carbon nanotube grafted polyethyleneimine is used to extend the transmission path of water molecules and delay the corrosion of concrete. In addition, silicone amide as the core will not be activated during mixing due to the protection of the wall material. When cracks and water infiltration occur in concrete, silicone amide is activated by water and reacts with the active points on the surface of cement particles to form chemical bonds, forming a high-strength and durable gelling system to fill the pores, which can catalyze the secondary reaction of cement particles that are not fully hydrated in the concrete, further fill the pores, and thus block the micro-cracks inside the concrete.
[0029] Furthermore, the preparation method of the carbon nanotube grafted polyethyleneimine / polyimide fiber copolymer comprises the following steps:
[0030] (1) dispersing carboxylated polyimide fiber into thionyl chloride solution, dropping N,N-dimethylformamide into the solution, and reacting at 35° C. for 24 h to obtain chlorinated polyimide fiber;
[0031] (2) mixing polyethyleneimine and phosphorous acid, stirring, heating to 40-50° C., adding formaldehyde dropwise, and continuing to heat to 80-90° C., reacting for 2-4 hours to obtain phosphorylated polyethyleneimine;
[0032] (3) adding phosphorylated polyethyleneimine to an N-methylpyrrolidone solution, ultrasonically treating for 10 min, then dispersing the chlorinated polyimide fiber in the solution, reacting at room temperature for 24 h, rinsing, and drying to obtain a polyethyleneimine / polyimide fiber copolymer;
[0033] (4) Add the carboxylated multi-walled carbon nanotubes to a thionyl chloride solution, add N,N-dimethylformamide dropwise, perform ultrasonic dispersion for 30 minutes, and reflux at 75° C. for 24 hours to obtain chlorinated multi-walled carbon nanotubes; disperse the chlorinated multi-walled carbon nanotubes in a N,N-dimethylformamide solution under ultrasonic conditions, add polyethyleneimine / polyimide fiber copolymer, react at room temperature for 12 hours, wash with ethanol, and dry to obtain the product.
[0034] Furthermore, the method for modifying polyvinyl alcohol with sodium silicate is as follows: sodium silicate and polyvinyl alcohol are mixed, phosphoric acid is added, the pH value is less than 2, and heat-treated at 120-140° C. for 40-50 minutes.
[0035] Furthermore, the water reducing agent is polyether polycarboxylic acid, sulfonated melamine formaldehyde resin or lignin sulfonate.
[0036] Furthermore, the precast concrete slab is provided with tenons and mortise grooves around its periphery, a plurality of anti-cracking steel meshes are provided inside the slab, and convex patterns are provided on the surface of the slab.
[0037] Furthermore, the tenon and the mortise have the same structure, the cross section is an isosceles trapezoid, the height of the protruding lines is 2-3 mm, and the spacing between adjacent anti-cracking steel meshes is 150 mm.
[0038] Example 1
[0039] An assembled prefabricated concrete panel suitable for an oil drilling platform is prepared by ultra-high performance concrete, which includes the following raw materials: 700 kg of cement, 200 kg of fly ash, 150 kg of silica fume, 50 kg of metakaolin, 157 kg of steel fiber, 17.9 kg of water reducer, 185 kg of water, 250 kg of quartz sand and 60 kg of admixture. Among them, the admixture includes 25 kg of carbon nanotube grafted polyethyleneimine / polyimide fiber copolymer, 20 kg of sodium silicate modified polyvinyl alcohol and 15 kg of silicone amide. The water reducer is polyether polycarboxylic acid.
[0040] The preparation method of the admixture is as follows: dissolving silicone amide in an ethanol solution, adding sodium dodecyl sulfate to prepare an emulsion; adding carbon nanotube grafted polyethyleneimine / polyimide fiber copolymer to the emulsion, stirring and mixing, then dropping a sodium silicate modified polyvinyl alcohol solution dissolved in water, and drying to obtain the admixture.
[0041] The preparation method of carbon nanotube grafted polyethyleneimine / polyimide fiber copolymer comprises the following steps:
[0042] (5) dispersing the carboxylated polyimide fiber into a thionyl chloride solution, dropping N,N-dimethylformamide into the solution, and reacting the solution at 35° C. for 24 h to obtain chlorinated polyimide fiber;
[0043] (6) Mix polyethyleneimine and phosphorous acid, stir, heat to 40°C, add formaldehyde dropwise, continue heating to 80°C, react for 2 hours, and obtain phosphorylated polyethyleneimine;
[0044] (7) adding phosphorylated polyethyleneimine to an N-methylpyrrolidone solution, ultrasonically treating for 10 min, then dispersing the chlorinated polyimide fiber in the solution, reacting at room temperature for 24 h, rinsing, and drying to obtain a polyethyleneimine / polyimide fiber copolymer;
[0045] The carboxylated multi-walled carbon nanotubes are added to a thionyl chloride solution, N,N-dimethylformamide is added dropwise, ultrasonic dispersion is performed for 30 minutes, and reflux is performed at 75°C for 24 hours to obtain chlorinated multi-walled carbon nanotubes; the chlorinated multi-walled carbon nanotubes are dispersed in a N,N-dimethylformamide solution under ultrasonic conditions, polyethyleneimine / polyimide fiber copolymer is added, the reaction is performed at room temperature for 12 hours, the product is washed with ethanol, and dried to obtain the product.
[0046] The method for modifying polyvinyl alcohol with sodium silicate is as follows: sodium silicate and polyvinyl alcohol are mixed, phosphoric acid is added, the pH value is less than 2, and heat-treated at 120° C. for 40 minutes.
[0047] Example 2
[0048] An assembled prefabricated concrete panel suitable for an oil drilling platform is prepared by ultra-high performance concrete, and the ultra-high performance concrete includes the following raw materials: 680 kg of cement, 180 kg of fly ash, 140 kg of silica fume, 40 kg of metakaolin, 145 kg of steel fiber, 10 kg of water reducer, 180 kg of water, 240 kg of quartz sand and 50 kg of admixture. Among them, the admixture includes 20 kg of carbon-carbon nanotube grafted polyethyleneimine / polyimide fiber copolymer, 20 kg of sodium silicate modified polyvinyl alcohol and 10 kg of silicone amide. The water reducer is sulfonated melamine formaldehyde resin.
[0049] Example 3
[0050] An assembled prefabricated concrete panel suitable for oil drilling platforms is made of ultra-high performance concrete, which includes the following raw materials: 690 kg of cement, 210 kg of fly ash, 145 kg of silica fume, 55 kg of metakaolin, 155 kg of steel fiber, 15 kg of water reducer, 190 kg of water, 260 kg of quartz sand and 70 kg of admixture. Among them, the admixture includes 28 kg of carbon nanotube grafted polyethyleneimine / polyimide fiber copolymer, 21 kg of sodium silicate modified polyvinyl alcohol and 12 kg of silicone amide. The water reducer is lignin sulfonate.
[0051] Example 4
[0052] An assembled prefabricated concrete panel suitable for an oil drilling platform is prepared by ultra-high performance concrete, which includes the following raw materials: 710 kg of cement, 190 kg of fly ash, 148 kg of silica fume, 45 kg of metakaolin, 152 kg of steel fiber, 12 kg of water reducer, 195 kg of water, 265 kg of quartz sand and 85 kg of admixture. Among them, the admixture includes 21 kg of carbon nanotube grafted polyethyleneimine / polyimide fiber copolymer, 28 kg of sodium silicate modified polyvinyl alcohol and 16 kg of silicone amide. The water reducer is lignin sulfonate.
[0053] Example 5
[0054] An assembled prefabricated concrete panel suitable for an oil drilling platform is prepared by ultra-high performance concrete, which includes the following raw materials: 720 kg of cement, 220 kg of fly ash, 160 kg of silica fume, 60 kg of metakaolin, 160 kg of steel fiber, 20 kg of water reducer, 200 kg of water, 270 kg of quartz sand and 100 kg of admixture. The admixture includes 30 kg of carbon nanotube grafted polyethyleneimine / polyimide fiber copolymer, 30 kg of sodium silicate modified polyvinyl alcohol and 20 kg of silicone amide. The water reducer is lignin sulfonate.
[0055] Example 6
[0056] like Figure 1-2 As shown, this embodiment provides an assembled prefabricated concrete panel suitable for oil drilling platforms. The prefabricated concrete panel 1 is cast with ultra-high performance concrete. The prefabricated concrete panel 1 is provided with tenons 2 and tenons 3 around it, a plurality of anti-cracking steel meshes are provided inside the panel, and a convex pattern 4 is provided on the panel surface. Different concrete panels can be connected through the tenons 2 and tenons 3, which is convenient for installation and positioning between panels, so that the assembled concrete panel has the functions of anti-slip and anti-shear. Preferably, the aspect ratio of the assembled concrete panel is 2:1, the length is 1500mm, the width is 750mm, and the thickness is 50mm.
[0057] Among them, the tenon 2 and the tenon groove 3 have the same structure, the cross-section is an isosceles trapezoid, and the size difference between the tenon 2 and the tenon groove 3 is 5 mm, which can reduce the installation accuracy and also serve as a drainage channel for the panel.
[0058] The height of the protruding lines 4 is 2-3 mm. In other embodiments, the protruding lines 4 may also be irregular protruding lines 4, and the protruding lines 4 may be used to improve the anti-slip performance of the surface of the concrete slab.
[0059] The spacing between adjacent anti-crack steel meshes is 150mm, and the diameter of the steel bars is 6mm. The anti-crack steel mesh can improve the strength of the concrete slab and meet the construction load requirements of the upper heavy-duty machinery.
[0060] Comparative Example 1
[0061] The difference between this comparative example and Example 1 is that the additives include carbon nanotube grafted polyethyleneimine, sodium silicate modified polyvinyl alcohol, and silicone amide.
[0062] Comparative Example 2
[0063] The difference between this comparative example and Example 1 is that the additives include carbon nanotube grafted polyimide fibers, sodium silicate modified polyvinyl alcohol, and silicone amide.
[0064] Comparative Example 3
[0065] The difference between this comparative example and Example 1 is that the additives include polyethyleneimine / polyimide fiber copolymer, sodium silicate-modified polyvinyl alcohol, and silicone amide.
[0066] Comparative Example 4
[0067] The difference between this comparative example and Example 1 is that the additives include carbon nanotube grafted polyethyleneimine / polyimide fiber copolymer, a mixture of sodium silicate and polyvinyl alcohol, and silicone amide.
[0068] Comparative Example 5
[0069] The difference between this comparative example and Example 1 is that the additives include 10 kg of carbon nanotube grafted polyethyleneimine / polyimide fiber copolymer, 15 kg of sodium silicate modified polyvinyl alcohol and 25 kg of silicone amide.
[0070] Comparative Example 6
[0071] The difference between this comparative example and Example 1 is that the content of admixture in the concrete is 120 kg.
[0072] Comparative Example 7
[0073] The difference between this comparative example and Example 1 is that the preparation method of the additive is: directly mixing the carbon nanotube grafted polyethyleneimine / polyimide fiber copolymer, sodium silicate modified polyvinyl alcohol and silicone amide.
[0074] Comparative Example 8
[0075] The difference between this comparative example and Example 1 is that the additives include graphene-grafted polyethyleneimine / polyimide fiber copolymer, sodium silicate-modified polyvinyl alcohol and silicone amide.
[0076] Comparative Example 9
[0077] The difference between this comparative example and Example 1 is that the additives include carbon nanotube grafted polyethyleneimine / polyimide fiber copolymer and silicone amide.
[0078] Comparative Example 10
[0079] The difference between this comparative example and Example 1 is that the admixture includes sodium silicate-modified polyvinyl alcohol and silicone amide.
[0080] Test results
[0081] The concrete slabs prepared in Examples 1-5 and Comparative Examples 1-10 were subjected to performance tests, and the results are shown in Table 1.
[0082] 28-day compressive strength, flexural strength, tensile strength and splitting strength: tested in accordance with GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete".
[0083] Slump: Tested in accordance with GB / T50080-2016 "Standard for Test Methods for Performance of Ordinary Concrete Mixtures".
[0084] Table 1 Performance test results
[0085]
[0086]
[0087] According to Table 1, the concrete slab prepared in the embodiment has a 28-day compressive strength of up to 130 MPa, a flexural strength of up to 22 MPa, a tensile strength of up to 6 MPa, a splitting strength of up to 2.98 MPa, and a slump of up to 235 mm.
[0088] Comparative Example 1 uses carbon nanotube grafted polyethyleneimine, Comparative Example 2 uses carbon nanotube grafted polyimide fiber, Comparative Example 3 uses polyethyleneimine / polyimide fiber copolymer, and Comparative Example 4 uses a mixture of sodium silicate and polyvinyl alcohol. The performance of the concrete slabs prepared in the four comparative examples is lower than that of the embodiment. The bridging effect produced by the carbon nanotube grafted polyethyleneimine in Comparative Example 1 is weak, which is not enough to bridge the microcracks of the concrete, causing the microcracks to expand and affecting the performance of the concrete. The carbon nanotube grafted polyimide fiber in Comparative Example 2 has low surface activity, weak binding ability, low material interface strength, and low improvement in the mechanical properties of the concrete. The interlayer shear force of the polyethyleneimine / polyimide fiber copolymer in Comparative Example 3 is weak, making it difficult to effectively bond and physically engage with the matrix material, reducing the mechanical properties of the concrete. The mixture of sodium silicate and polyvinyl alcohol in Comparative Example 4 has a low probability of self-condensation, a low chemical cross-linking enhancement effect, and a small filling effect on the microvoids and microcracks inside the concrete, affecting the performance of the concrete.
[0089] The ratio of each raw material in the admixture of Comparative Example 5 exceeds that of the embodiment. The network cross-linked structure formed by sodium silicate-modified polyvinyl alcohol is not sufficient to fill or adhere to the micro-voids and micro-cracks inside the concrete. The carbon nanotube-grafted polyethyleneimine absorbs less cement particles, and silicone amide participates less in cement hydration, so the performance of the obtained concrete is low.
[0090] Adding excessive admixtures in Comparative Example 6 will reduce the fluidity of the concrete, increase internal defects, easily cause micro cracks and pores, and easily generate stress concentration around the pores, thereby reducing the performance of the concrete.
[0091] In Comparative Example 7, the admixture is directly mixed with various raw materials, and a core-shell structure with silicone amide as the core and carbon nanotube-grafted polyethyleneimine as the shell cannot be formed. Silicone amide will be activated prematurely, and when cracks appear in the concrete, it will not be sufficient to fill the cracks, and it is not easy to absorb cement particles, which reduces the performance of the concrete.
[0092] In comparative example 8, graphene grafted polyethyleneimine was used, and the admixture components in comparative examples 9 and 10 were different from those in example 1. The concrete properties of comparative examples 8-10 all declined. It was shown that the use of the raw materials of the admixtures in the examples of the present application can improve the compressive strength, flexural strength, splitting strength and slump of the concrete.
[0093] The concrete slabs prepared in Examples 1-6 were subjected to load tests, and the results were as follows:
[0094] Table 2 Load test results
[0095]
[0096]
[0097] It can be seen from Table 2 that the concrete slab prepared in the example meets the construction requirements.
[0098] In summary, the concrete slab of the present application has extremely high strength, with a compressive strength of 130MPa, a flexural strength of 22MPa, and a tensile strength of 6MPa, which can meet the construction load requirements of the upper heavy-duty machinery.
[0099] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An assembled prefabricated concrete panel suitable for oil drilling platforms, characterized in that: The precast concrete slab is made of ultra-high performance concrete, which includes the following raw materials by weight: 680-720 parts of cement, 180-220 parts of fly ash, 140-160 parts of silica fume, 40-60 parts of metakaolin, 145-160 parts of steel fiber, 10-20 parts of water reducer, 180-200 parts of water, 240-270 parts of quartz sand and 50-100 parts of admixture; The additive comprises 20-30 parts of carbon nanotube grafted polyethyleneimine / polyimide fiber copolymer, 20-30 parts of sodium silicate modified polyvinyl alcohol and 10-20 parts of silicone amide.
2. The assembled prefabricated concrete panel suitable for oil drilling platform according to claim 1 is characterized in that: The preparation method of the additive is as follows: dissolving silicone amide in an ethanol solution, adding sodium dodecyl sulfate to prepare an emulsion; adding carbon nanotube grafted polyethyleneimine / polyimide fiber copolymer to the emulsion, stirring and mixing, then dripping a sodium silicate modified polyvinyl alcohol solution dissolved in water, and drying to obtain the additive.
3. The assembled prefabricated concrete panel suitable for oil drilling platforms according to claim 2 is characterized in that: The preparation method of the carbon nanotube grafted polyethyleneimine / polyimide fiber copolymer comprises the following steps: (1) dispersing carboxylated polyimide fiber into thionyl chloride solution, dropping N,N-dimethylformamide into the solution, and reacting at 35° C. for 24 h to obtain chlorinated polyimide fiber; (2) mixing polyethyleneimine and phosphorous acid, stirring, heating to 40-50° C., adding formaldehyde dropwise, and continuing to heat to 80-90° C., reacting for 2-4 hours to obtain phosphorylated polyethyleneimine; (3) adding phosphorylated polyethyleneimine to an N-methylpyrrolidone solution, ultrasonically treating for 10 min, then dispersing the chlorinated polyimide fiber in the solution, reacting at room temperature for 24 h, rinsing, and drying to obtain a polyethyleneimine / polyimide fiber copolymer; (4) Add the carboxylated multi-walled carbon nanotubes to a thionyl chloride solution, add N,N-dimethylformamide dropwise, perform ultrasonic dispersion for 30 minutes, and reflux at 75° C. for 24 hours to obtain chlorinated multi-walled carbon nanotubes; disperse the chlorinated multi-walled carbon nanotubes in a N,N-dimethylformamide solution under ultrasonic conditions, add polyethyleneimine / polyimide fiber copolymer, react at room temperature for 12 hours, wash with ethanol, and dry to obtain the product.
4. The assembled prefabricated concrete panel suitable for oil drilling platforms according to claim 2 is characterized in that: The method for modifying polyvinyl alcohol with sodium silicate is as follows: sodium silicate and polyvinyl alcohol are mixed, phosphoric acid is added, the pH value is less than 2, and heat treatment is performed at 120-140° C. for 40-50 minutes.
5. The assembled prefabricated concrete panel suitable for oil drilling platforms according to claim 1 is characterized in that: The water reducing agent is polyether polycarboxylic acid, sulfonated melamine formaldehyde resin or lignin sulfonate.
6. The assembled prefabricated concrete panel suitable for oil drilling platforms according to claim 1 is characterized in that: The precast concrete slab is provided with tenons and tenons around its periphery, a plurality of anti-cracking steel mesh sheets are provided inside the slab, and convex patterns are provided on the surface of the slab.
7. The assembled prefabricated concrete panel suitable for oil drilling platforms according to claim 6 is characterized in that: The tenon and the mortise have the same structure, and the cross section is an isosceles trapezoid. The height of the protruding lines is 2-3 mm, and the spacing between adjacent anti-cracking steel meshes is 150 mm.