Green unfired gypsum-based waterproof cementing material and preparation method thereof

By adding barium hydroxide, glass powder and slag to the gypsum material, and using polyethylene glycol-4000 to regulate the crystal structure, combining protein retarder and polycarboxylic acid water reducing agent, we prepare a calcination without high temperature. Gypsum-based waterproof gelling material solves the problem of poor water resistance of gypsum materials in high humidity environments, and realizes efficient waterproof and environmentally friendly concrete materials.

CN119019147APending Publication Date: 2024-11-26GUIZHOU UNIV
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411135111.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2024-06-15
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing gypsum materials have poor water resistance in high humidity environments, which limits their application scope. The comprehensive utilization rate of industrial by-product phosphogypsum is low, and a modified material is needed to improve waterproofing and environmental protection.

Method used

Using semi-water gypsum, barium hydroxide octahydrate, glass powder and slag, the crystal structure of barium sulfate is regulated through polyethylene glycol-4000, combined with protein gypsum retarder and polycarboxylic acid water reducing agent, it is prepared without any need. High-temperature calcined green gypsum-based waterproof gelling material improves the density and waterproof performance of concrete.

Benefits of technology

It has achieved high compressive strength, low water absorption and environmentally friendly concrete materials, significantly improved waterproof performance, promoted the reuse of industrial by-product materials, and reduced raw material costs and energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004999174530000061
    Figure BDA0004999174530000061
  • Figure BDA0004999174530000071
    Figure BDA0004999174530000071
Patent Text Reader

Abstract

The invention relates to the technical field of building materials, discloses a green unfired gypsum-based waterproof cementing material, and further discloses a preparation method of the green unfired gypsum-based waterproof cementing material, and the green unfired gypsum-based waterproof cementing material comprises the following components in parts by mass: 50 parts of hemihydrate gypsum, 5-20 parts of barium hydroxide octahydrate, 5-20 parts of glass powder, 10-40 parts of slag and 1.5 parts of an additive. Comprising the following steps: S1, mechanically crushing dihydrate gypsum, and drying to prepare semi-hydrated gypsum; breaking the glass; s2, packaging the semi-hydrated gypsum, the barium hydroxide octahydrate, the glass powder and the slag into bags; s3, packaging the protein gypsum retarder and polyethylene glycol-4000 into bags, and packaging the polycarboxylic acid water reducer into bags; and S4, packaging in a large bag. High-temperature calcination is not needed, energy consumption is low, and aging is not prone to occurring; the semi-hydrated gypsum, the glass powder and the slag in the cementing material are all recycled industrial byproducts, so that the raw material cost is low, and the cementing material is green and environment-friendly; the waterproof effect is excellent, the compressive strength is high, and the durability is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building materials, in particular to a green, non-burning gypsum-based waterproof gelling material and a preparation method thereof. Background Art

[0002] Gypsum resources are abundant, especially industrial by-product gypsum, such as phosphogypsum and desulfurized gypsum. The annual emission of phosphogypsum in my country has reached more than 80 million tons, and the comprehensive utilization rate is only 50%. These phosphogypsums are discarded in large quantities and occupy a large amount of land when piled up. Therefore, the comprehensive utilization of phosphogypsum has become an urgent issue for phosphorus chemical companies. Gypsum is an air-hardening cementitious material. The semi-hydrated gypsum obtained after drying is usually used as a binder for concrete. Sulfurized gypsum slag cement, alkali-activated gypsum cementitious materials and alkali-activated gypsum-based concrete have been produced. Compared with cement, gypsum has the advantages of no calcination and low carbon energy saving, but its poor water resistance limits its application range, and the prepared concrete cannot work in high humidity environments. It should be modified to improve its waterproof effect.

[0003] A Chinese patent discloses a non-hygroscopic, efficient phosphogypsum retarder and its preparation method and application (authorization announcement number CN112500019B). The patented technology mixes and grinds calcium polyaspartate with barium hydroxide and barium carbonate for a specific period of time. The obtained product is not easy to absorb moisture and has a highly efficient retarding effect. Even when used for phosphogypsum, it can achieve a good retarding effect with a relatively small addition amount. It can be used as a phosphogypsum retarder, but its compressive strength is not high and the raw material cost is high. Summary of the invention

[0004] The object of the present invention is to provide a green, unburned, gypsum-based waterproof cementitious material and a preparation method thereof, so as to solve the problems raised in the above-mentioned background technology.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] A green, unfired gypsum-based waterproof cementitious material is composed of the following components in parts by mass: 50 parts of hemihydrate gypsum, 5 to 20 parts of barium hydroxide octahydrate, 5 to 20 parts of glass powder, 10 to 40 parts of slag and 1.25 parts of an admixture, wherein the admixture consists of a polycarboxylic acid water reducer, a protein gypsum retarder and polyethylene glycol-4000, and the mass ratio thereof is 1:0.5:1. The barium sulfate crystal structure is changed by polyethylene glycol-4000, thereby improving the density and waterproof effect of the concrete.

[0007] The semi-hydrated gypsum is prepared by air-drying dihydrated gypsum at 150-160° C., and the particle size of the semi-hydrated gypsum is less than 130 meshes.

[0008] As a further solution of the present invention: the dihydrate gypsum is one or more of phosphogypsum, natural anhydrite, desulfurized gypsum and natural dihydrate gypsum.

[0009] As a further solution of the present invention: the purity of the barium hydroxide octahydrate is greater than 98%.

[0010] As a further solution of the present invention: the particle size of the glass powder is less than 200 mesh.

[0011] As a further solution of the present invention: the slag is S95 grade granulated blast furnace slag, which has good strength development and long-term stability and can effectively prevent the aging of concrete structures.

[0012] As a further solution of the present invention: the polycarboxylic acid water reducer is one of methacrylic acid / methyl acrylate copolymer, allyl ether copolymer, amide / imide type polycarboxylic acid polymer and polyamide-polyethylene glycol branched type water reducer.

[0013] As a further solution of the present invention: the protein-based gypsum retarder is one of animal glue, gelatin, gelatin protease hydrolyzate and corn starch.

[0014] A method for preparing a green, non-burning gypsum-based waterproof gelling material comprises the following steps:

[0015] S1, after mechanically crushing the dihydrate gypsum, air drying it at 160°C for 2 days; then, grinding it twice, passing it through a 130-mesh sieve, taking the sieve residue to obtain hemihydrate gypsum; then crushing the glass, passing it through a 200-mesh sieve, taking the sieve residue to obtain glass powder;

[0016] S2, taking 50 parts by mass of hemihydrate gypsum, 5-20 parts of barium hydroxide octahydrate with a purity greater than 98%, 5-20 parts of glass powder and 10-40 parts of S95 grade granulated blast furnace slag, stirring and mixing them thoroughly, and packaging them into bags to obtain a cementitious material;

[0017] S3. Take 0.5 parts of protein gypsum retarder and 0.5 parts of polyethylene glycol-4000 by mass, mix them thoroughly, and pack them into bags. Then take 0.5 parts of polycarboxylate water reducer and pack them into bags independently.

[0018] S4. Pack the bagged gelling material in step S2, the bagged protein-based gypsum retarder and polyethylene glycol-4000 in step S3, and the independently bagged polycarboxylate water-reducing agent in a large waterproof bag.

[0019] The acquisition of raw materials and the preparation of cementitious materials do not require a high-temperature calcination process (≤160°C), and are environmentally friendly building materials that do not require calcination. In particular, S95 granulated blast furnace slag is an industrial by-product of the high-temperature iron smelting process, and the addition of slag in the present invention is a waste material utilization.

[0020] In the process of preparing the cementitious material prepared by the present invention into concrete; barium hydroxide octahydrate modified hemihydrate gypsum generates barium sulfate crystals, but the barium sulfate crystals under normal growth are cubic and cannot provide mechanical bite force. Polyethylene glycol-4000 can regulate the crystal morphology of the crystal, so that it grows directionally into rod-like and fishbone-like crystals, thereby significantly improving the mechanical bite force between crystals. The crystal fully fills the gaps between gypsum crystals and significantly improves the structural density. In addition, the modified calcium hydroxide can further react with glass powder and slag to generate calcium silicate hydrate (CSH) and calcium aluminate hydrate (CAH), and calcium aluminate hydrate reacts with gypsum to generate calcium aluminate (AFt). CSH gel wraps and bonds dihydrate gypsum crystals, barium sulfate crystals, and AFt crystals, filling the microscopic pores between the crystals and further improving the structural density. Thereby reducing the number of microscopic capillaries and lowering the water absorption rate of concrete. In addition, the solubility of barium sulfate crystals and AFt crystals is much lower than that of dihydrate gypsum, thereby improving the waterproof performance of concrete.

[0021] Compared with traditional cement adhesives, the cementitious material prepared by the present invention uses chemical excitation instead of high-temperature calcination to prepare hydraulic cementitious materials, which has lower energy consumption and is green and environmentally friendly. At the same time, it realizes the secondary utilization of industrial by-product gypsum and waste glass, which has significant solid waste significance.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The cementitious material prepared by the present invention through semi-hydrated gypsum, barium hydroxide octahydrate, glass powder, slag and additives does not need to be calcined at high temperature, has low energy consumption, and is not easy to age compared with traditional epoxy resin organic materials; the semi-hydrated gypsum, glass powder and slag in the cementitious material are all recycled industrial by-products, with low raw material cost and green environmental protection; at the same time, the concrete prepared by the cementitious material has excellent waterproof effect, high compressive strength and good durability. DETAILED DESCRIPTION

[0024] Example 1

[0025] A green, unburned, gypsum-based waterproof cementitious material comprises the following components in parts by mass: 50 parts of hemihydrate gypsum, 5 parts of barium hydroxide octahydrate, 5 parts of glass powder, 40 parts of slag, 0.5 parts of methacrylic acid / methyl acrylate copolymer, 0.25 parts of animal glue and 0.5 parts of polyethylene glycol-4000.

[0026] A method for preparing a green, non-burning gypsum-based waterproof gelling material comprises the following steps:

[0027] S1. After mechanically crushing the phosphogypsum, dry it with air at 160°C for 2 days; then, grind it twice and pass it through a 130-mesh sieve to obtain hemihydrate gypsum; then crush the glass and pass it through a 200-mesh sieve to obtain glass powder;

[0028] S2, taking 50 parts of hemihydrate gypsum, 5 parts of barium hydroxide octahydrate with a purity greater than 98%, 5 parts of glass powder and 40 parts of S95 grade granulated blast furnace slag by mass, stirring and mixing them thoroughly, and packing them into bags to obtain a gelling material;

[0029] S3, taking 0.25 parts of animal glue and 0.5 parts of polyethylene glycol-4000 by mass, mixing them thoroughly, and packaging them into bags, and then taking 0.5 parts of methacrylic acid / methyl acrylate copolymer and packaging them into bags independently;

[0030] S4, packing the gelling material bagged in step S2, the animal glue and polyethylene glycol-4000 bagged in step S3, and the methacrylic acid / methyl acrylate copolymer bagged independently into a large waterproof bag.

[0031] Example 2

[0032] A green, unburned gypsum-based waterproof cementitious material comprises the following components in parts by mass: 50 parts of hemihydrate gypsum, 10 parts of barium hydroxide octahydrate, 10 parts of glass powder, 30 parts of slag, 0.5 parts of allyl ether copolymer, 0.25 parts of gelatinase hydrolyzate and 0.5 parts of polyethylene glycol-4000.

[0033] A method for preparing a green, non-burning gypsum-based waterproof gelling material comprises the following steps:

[0034] S1, crushing the natural anhydrite mechanically, and drying it at 160°C for 2 days; then, grinding it twice, passing it through a 130-mesh sieve, taking the sieve residue to obtain hemihydrate gypsum; crushing the glass, passing it through a 200-mesh sieve, taking the sieve residue to obtain glass powder;

[0035] S2, taking 50 parts of hemihydrate gypsum, 10 parts of barium hydroxide octahydrate with a purity greater than 98%, 10 parts of glass powder and 30 parts of S95 grade granulated blast furnace slag by mass, stirring and mixing them thoroughly, and packing them into bags to obtain a cementitious material;

[0036] S3, taking 0.25 parts of gelatinase hydrolysate and 0.5 parts of polyethylene glycol-4000 by mass, mixing them thoroughly, and packaging them into bags, and then taking 0.5 parts of allyl ether copolymer and packaging them into bags independently;

[0037] S4. Pack the gelling material bagged in step S2, the gelatinase hydrolyzate and polyethylene glycol-4000 bagged in step S3, and the independently bagged propylene ether copolymer into a large waterproof bag.

[0038] Example 3

[0039] A green, unburned gypsum-based waterproof cementitious material comprises the following components in parts by mass: 50 parts of hemihydrate gypsum, 15 parts of barium hydroxide octahydrate, 15 parts of glass powder, 20 parts of slag, 0.5 parts of amide / imide type polycarboxylic acid polymer, 0.25 parts of corn starch and 0.5 parts of polyethylene glycol-4000.

[0040] A method for preparing a green, non-burning gypsum-based waterproof gelling material comprises the following steps:

[0041] S1. After mechanically crushing the phosphogypsum, dry it with air at 160°C for 2 days; then, grind it twice and pass it through a 130-mesh sieve to obtain hemihydrate gypsum; then crush the glass and pass it through a 200-mesh sieve to obtain glass powder;

[0042] S2, taking 50 parts of hemihydrate gypsum, 15 parts of barium hydroxide octahydrate with a purity greater than 98%, 15 parts of glass powder and 20 parts of S95 grade granulated blast furnace slag by mass, stirring and mixing them thoroughly, and packing them into bags to obtain a cementitious material;

[0043] S3, taking 0.25 parts of corn starch and 0.5 parts of polyethylene glycol-4000 by mass, stirring and mixing them thoroughly, and then packing them into bags, and then taking 0.5 parts of amide / imide type polycarboxylic acid polymer and packing them into bags independently;

[0044] S4, packing the gelling material bagged in step S2, the corn starch and polyethylene glycol-4000 bagged in step S3, and the amide / imide type polycarboxylic acid polymer bagged independently into a large waterproof bag.

[0045] In order to better illustrate the technical effect of the present invention, the following experiments are used to illustrate:

[0046] Example 1 of a high-strength water-resistant plaster gypsum mortar and a preparation method thereof (CN112159196B) disclosed in the patent website was used as comparative example 1; Example 1 of a non-hygroscopic high-efficiency phosphogypsum retarder and a preparation method and application thereof (CN112500019A) disclosed in the patent website was used as comparative example 2.

[0047] The waterproof cementitious materials prepared in Examples 1 to 3 of the present invention are respectively prepared into concrete as Example 1 Group, Example 2 Group and Example 3 Group;

[0048] The preparation method of the concrete of Example 1 is as follows:

[0049] 220 parts of sand with a particle size of 0.5 mm and 270 parts of gravel with a particle size of 10 mm were poured into a concrete mixer and dry mixed for 30 seconds, and then 50 parts of hemihydrate gypsum, 5 parts of barium hydroxide octahydrate, 5 parts of glass powder, 40 parts of S95 grade granulated blast furnace slag, 0.25 parts of animal glue and 0.5 parts of polyethylene glycol-4000 were poured and mixed for another 30 seconds; then 0.5 parts of methacrylic acid / methyl acrylate copolymer was added to the mixing water and fully diluted, and then poured into the mixer and mixed for another 3 minutes; the concrete was poured out to prepare a test piece and cured in a natural state indoors for 28 days to obtain the concrete of Example 1;

[0050] The preparation method of the concrete of Example 2 is as follows:

[0051] 220 parts of sand with a particle size of 0.5 mm and 270 parts of gravel with a particle size of 10 mm were poured into a concrete mixer by mass and dry mixed for 30 seconds, and then 50 parts of hemihydrate gypsum, 10 parts of barium hydroxide octahydrate, 10 parts of glass powder, 30 parts of S95 grade granulated blast furnace slag, 0.25 parts of gelatinase hydrolyzate and 0.5 parts of polyethylene glycol-4000 were poured and mixed for another 30 seconds; then 0.5 parts of allyl ether copolymer was added to the mixing water and fully diluted, and then poured into the mixer and mixed for another 3 minutes; the concrete was poured out to prepare a test piece and cured in a natural state indoors for 28 days to obtain the concrete of Example 1.

[0052] The preparation method of the concrete of Example 3 is as follows:

[0053] 220 parts of sand with a particle size of 0.5 mm and 270 parts of gravel with a particle size of 10 mm were poured into a concrete mixer and dry mixed for 30 seconds, and then 50 parts of hemihydrate gypsum, 15 parts of barium hydroxide octahydrate, 15 parts of glass powder, 20 parts of S95 grade granulated blast furnace slag, 0.25 parts of corn starch and 0.5 parts of polyethylene glycol-4000 were poured and mixed for another 30 seconds; then 0.5 parts of amide / imide type polycarboxylic acid polymer was added to the mixing water and fully diluted, and then poured into the mixer and mixed for another 3 minutes; the concrete was poured out to prepare a test piece and cured in a natural state indoors for 28 days to obtain the concrete of Example 1.

[0054] The concrete in the above Examples 1 to 3 groups are divided into two groups, and the water-cement ratios are 0.33 and 0.36 respectively.

[0055] According to GB / T 50081-2019, the 28d compressive strength and water absorption of the specimens were tested, and the mechanical strength and water resistance of the concrete prepared in Examples 1 to 3 of the present invention and Comparative Example 1 and Comparative Example 2 were respectively tested and recorded in Tables 1 and 2 below; wherein, the specimens were considered to be in an air-dried state after 28d of natural curing, the 28d-old specimens were considered to be in a saturated water absorption state after being immersed in water for 48h, and the 28d-old specimens were considered to be in an absolutely dry state after being dried at 105°C for 48h.

[0056] Table 1 Mechanical strength and water resistance index of concrete when water-cement ratio is 0.33

[0057]

[0058] It can be concluded from Table 1 above that when the water-cement ratio is 0.33, the concrete prepared by using Examples 1 to 3 of the present invention has a 28d compressive strength in the air-dried state, the saturated water absorption state and the absolutely dry state that is significantly higher than that of the comparative example 1 group and the comparative example 2 group; and the 28d water absorption rate of the concrete prepared by Examples 1 to 3 of the present invention is significantly lower than that of the comparative example 2 group, but higher than that of the comparative example 1 group; at the same time, the concrete prepared by Examples 1 to 3 of the present invention has a 28d softening coefficient in the air-dried state that is lower than that of the comparative examples 1 and 2 groups, but greater than 0.84; and the 28d softening coefficient in the absolutely dry state is greater than that of the comparative examples 1 and 2 groups; and it can be concluded that the concrete prepared by the cementitious material prepared by the present invention has a high compressive strength, a low water absorption rate and a good waterproof effect, whether in a dry state or a water-absorbed state.

[0059] Table 2 Mechanical strength and water resistance index of concrete when water-cement ratio is 0.36

[0060]

[0061] It can be concluded from Table 1 above that when the water-cement ratio is 0.36, the concrete prepared by using Examples 1 to 3 of the present invention has significantly higher 28d compressive strength in air-dried state, saturated water absorption state and absolute dry state than those of Comparative Example 1 and Comparative Example 2; and the 28d water absorption rate of the concrete prepared by Examples 1 to 3 of the present invention is significantly lower than that of Comparative Example 2, but higher than that of Comparative Example 1; at the same time, the 28d softening coefficient of the concrete prepared by Examples 1 to 3 of the present invention in air-dried state is lower than that of Comparative Examples 1 and 2, but greater than 0.85; the 28d softening coefficient in absolute dry state is significantly greater than that of Comparative Examples 1 and 2; further, it can be concluded that the concrete prepared by the cementitious material prepared by the present invention has higher compressive strength, lower water absorption and better waterproof effect, whether in dry state or water absorption state.

[0062] What is described above is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A green, non-burning, gypsum-based waterproof cementitious material, characterized in that: The composition by mass is as follows: 50 parts of hemihydrate gypsum, 5-20 parts of barium hydroxide octahydrate, 5-20 parts of glass powder, 10-40 parts of slag and 1.25 parts of admixture, wherein the admixture is composed of polycarboxylic acid water reducer, protein gypsum retarder and polyethylene glycol-4000, and the mass ratio thereof is 1:0.5:

1.

2. A green, non-burning gypsum-based waterproof cementitious material according to claim 1, characterized in that: The semi-hydrated gypsum is prepared by air-drying dihydrated gypsum at 150-160° C., and the particle size of the semi-hydrated gypsum is less than 130 meshes.

3. A green, non-burning gypsum-based waterproof cementitious material according to claim 2, characterized in that: The dihydrate gypsum is one or more of phosphogypsum, natural anhydrite, desulfurized gypsum and natural dihydrate gypsum.

4. A green, unburned, gypsum-based waterproof cementitious material according to claim 1, characterized in that: The purity of the barium hydroxide octahydrate is greater than 98%.

5. The green, unburned, gypsum-based waterproof cementitious material according to claim 1, characterized in that: The particle size of the glass powder is less than 200 meshes.

6. A green, non-burning gypsum-based waterproof cementitious material according to claim 1, characterized in that: The slag is S95 grade granulated blast furnace slag.

7. A green, non-burning gypsum-based waterproof cementitious material according to claim 1, characterized in that: The polycarboxylic acid water reducer is one of methacrylic acid / methyl acrylate copolymer, allyl ether copolymer, amide / imide type polycarboxylic acid polymer and polyamide-polyethylene glycol branched type water reducer.

8. The green, non-fired gypsum-based waterproof cementitious material according to claim 1, characterized in that: The protein-based gypsum retarder is one of animal glue, gelatin, gelatinase hydrolyzate and corn starch.

9. A method for preparing the green, unburned, gypsum-based waterproof gelling material according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1, after mechanically crushing the dihydrate gypsum, air drying it at 160°C for 2 days; then, grinding it twice, passing it through a 130-mesh sieve, taking the sieve residue to obtain hemihydrate gypsum; then crushing the glass, passing it through a 200-mesh sieve, taking the sieve residue to obtain glass powder; S2, taking 50 parts by mass of hemihydrate gypsum, 5-20 parts of barium hydroxide octahydrate with a purity greater than 98%, 5-20 parts of glass powder and 10-40 parts of S95 grade granulated blast furnace slag, stirring and mixing them thoroughly, and packaging them into bags to obtain a cementitious material; S3. Take 0.25 parts of protein gypsum retarder and 0.5 parts of polyethylene glycol-4000 by mass, mix them thoroughly, and pack them into bags. Then take 0.5 parts of polycarboxylate water reducer and pack them into bags independently. S4. Pack the bagged gelling material in step S2, the bagged protein-based gypsum retarder and polyethylene glycol-4000 in step S3, and the independently bagged polycarboxylate water-reducing agent in a large waterproof bag.

Citation Information

Patent Citations

  • A high-strength, water-resistant plastering gypsum mortar and its preparation method

    CN112159196B

  • Moisture-absorption-free efficient gypsum retarder as well as preparation method and application thereof

    CN112500019A

  • A non-hygroscopic, high-efficiency phosphogypsum retarder, its preparation method and application

    CN112500019B