Preparation method of carbon ceramic green body, carbon ceramic green body and carbon ceramic brake pad
Through ultrasonic processing technology, the bonding ability between carbon fiber and resin is improved, and the problem of high wear rate of carbon fiber ceramic brake pads at high temperatures is solved, and the high mechanical strength and wear resistance of carbon ceramic brake pads are achieved, which improves production efficiency.
Patent Information
- Application Number
- CN202411098415.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-12
AI Technical Summary
The existing carbon fiber ceramic brake pads have high wear rate at high temperatures, poor mechanical strength and wear resistance. This is mainly due to the insufficient binding ability of carbon fiber and resin, which leads to the failure of the binder resin under friction and heat.
The carbon fiber preform is placed in the wetting liquid of silicone modified phenolic resin and silicone modified polyimide resin by ultrasonic cavitation. The binding capacity of carbon fiber and resin is improved through ultrasonic cavitation, and carbonization is carried out and the High temperature sintering to prepare carbon ceramic embryo bodies and carbon ceramic brake pads with excellent performance.
It significantly improves the binding ability of carbon fiber and resin, reduces the wear rate of brake pads, improves mechanical strength, high temperature and wear resistance, shortens production time, and improves production efficiency.
Smart Images

Figure CN119019181A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of brake pads, and in particular to a method for preparing a carbon-ceramic embryo, a carbon-ceramic embryo and a carbon-ceramic brake pad. Background Art
[0002] Carbon / carbon composites are used as friction elements for the new generation of civil and military aircraft due to their excellent performance. However, carbon / carbon materials used alone as friction materials often fail due to oxidation at 700°C, and are prone to brake failure in a humid environment, which greatly reduces the performance. Carbon fiber reinforced silicon carbide ceramic matrix composites (C / C-SiC) are a new type of friction material with low density, good wear resistance, oxidation resistance and thermal shock resistance, and require a smaller heat capacity volume than C / C. Brake discs using C / C-SiC composites can overcome the high temperature failure and tribological defects of traditional friction materials. Therefore, C / C-SiC composites will have broad application prospects in the field of aircraft brake materials. Research on this new type of friction material has attracted the attention of some scholars at home and abroad.
[0003] At present, brake pads are generally composite materials composed of carbon fiber matrix, binder resin, wear-resistant additives and other components. Due to the friction heat generated during the braking process, the temperature of the friction surface increases, which can easily cause the binder resin to undergo glass transition, thermal expansion, thermal decay, thermal cracking and other phenomena, thereby causing a sudden change in friction torque and leading to friction failure. Wear-resistant additives are mostly inorganic components such as graphite or silicon carbide, which are not well compatible with the binder resin, making it difficult for them to evenly adhere to the carbon fiber matrix for bonding. This results in the prepared brake pads having poor mechanical strength, high temperature resistance and wear resistance.
[0004] CN117534498 A discloses a carbon fiber ceramic brake pad and a preparation method thereof, wherein the carbon fiber ceramic brake pad is made of a carbon fiber three-dimensional needle-punched preform body, which is impregnated with a silicon-containing phenolic resin solution, heated and cured, and calcined and carbonized; the silicon-containing phenolic resin solution is made by mixing a silicon-containing mixture with a phenolic resin solution, and the components of the silicon-containing mixture include, by mass percentage, 10-30wt% of polycarbosilane, 10-30wt% of polydimethylsiloxane, 10-30wt% of polycyclosiloxane, 5-20wt% of polymethylsilane, 1-30wt% of graphite powder, and 10-30wt% of silicon carbide powder. The invention adds a certain proportion of siloxane to the phenolic resin solution, so that the carbon fiber ceramic brake pad has a certain wear resistance and high temperature resistance, but because the carbon fiber, graphite powder, and silicon carbide powder are inorganic powders, it is difficult to aggregate with the phenolic resin, so the brake pad prepared by the invention has a high wear rate at high temperature, especially after long-term service, the ceramic brake pad has a high loss.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a carbon ceramic embryo, a carbon ceramic embryo and a carbon ceramic brake pad. The preparation method of the present invention places a carbon fiber preform in a resin impregnation liquid for ultrasonic treatment, and has a good impregnation effect and dispersion effect on the carbon fiber through ultrasonic cavitation, which significantly improves the bonding ability of the carbon fiber and the resin, thereby preparing a composite material with better performance, thereby preparing a carbon ceramic brake pad with high mechanical strength, high temperature resistance and friction resistance.
[0007] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0008] In a first aspect, a method for preparing a carbon ceramic embryo body is provided, wherein the method for preparing a carbon ceramic embryo body comprises the following steps:
[0009] Placing a carbon fiber preform in an impregnation liquid and performing ultrasonic treatment to obtain a modified carbon fiber preform; wherein the impregnation liquid comprises organic silicon modified phenolic resin, siloxane modified polyimide resin, silicon carbide, graphite and silicon dioxide;
[0010] The modified carbon fiber is prefabricated and subjected to carbonization treatment and high-temperature sintering to obtain the carbon ceramic embryo body.
[0011] Preferably, the process parameters of the ultrasonic treatment are: power density is 6 to 12 W / cm 2 , the ultrasonic frequency is 40-42kHz, and the ultrasonic duty cycle is 50-60%.
[0012] Preferably, the temperature of the ultrasonic treatment is 30-40°C.
[0013] Preferably, the ultrasonic treatment time is 1 to 3 hours.
[0014] Preferably, the mass ratio of the carbon fiber preform to the impregnating liquid is 1:(1-1.5).
[0015] Preferably, the impregnation solution comprises the following components by weight:
[0016]
[0017] Preferably, the organosilicon-modified phenolic resin is prepared by the following steps:
[0018] In the presence of an acidic catalyst, a phenolic compound, an aldehyde compound and an organosilicon monomer are reacted to obtain the organosilicon-modified phenolic resin;
[0019] Preferably, the acidic catalyst is selected from any one of hydrochloric acid, phosphoric acid, sulfuric acid, oxalic acid or boric acid, or a combination of at least two thereof.
[0020] Preferably, the phenolic compound comprises resorcinol and / or catechol.
[0021] Preferably, the aldehyde compound includes any one of formaldehyde, acetaldehyde or furfural, or a combination of at least two of them.
[0022] Preferably, the organosilicon monomer comprises C10-C18 long-chain silane.
[0023] Preferably, the C10-C20 long-chain silane is selected from any one of decyltrimethoxysilane, dodecyltrimethoxysilane, tetradecyltrimethoxysilane, hexadecyltrimethoxysilane and octadecyltrimethoxysilane, or a combination of at least two thereof.
[0024] Preferably, the molar ratio of the phenolic compound, the aldehyde compound and the organosilicon monomer is 1.0:(1.0-1.2):(0.1-0.5).
[0025] Preferably, the amount of the acidic catalyst added is 0.5-1.5% of the mass of the phenolic compound.
[0026] Preferably, the reaction process is as follows: first react at 70-90°C for 5-6h, distill under reduced pressure for 1-3h, then react at 130-150°C for 0.5-2h, add solvent to adjust the solid content, and obtain the organosilicon-modified phenolic resin.
[0027] Preferably, the solvent is methanol and / or ethanol.
[0028] Preferably, the solid content of the organosilicon-modified phenolic resin is 60-70 wt %.
[0029] Preferably, the siloxane-modified polyimide resin is prepared by the following steps:
[0030] The dianhydride solution and the diamine solution are mixed to carry out a condensation reaction to obtain a polyamic acid solution;
[0031] The polyamic acid solution and the amino-containing organic siloxane are mixed and subjected to a grafting reaction to obtain the siloxane-modified polyimide resin.
[0032] Preferably, the molar ratio of the dianhydride to the diamine is 1.0:(1.0-1.2).
[0033] Preferably, the concentrations of the dianhydride solution and the diamine solution are each independently 1 to 10 wt %, and the solvents in the dianhydride solution and the diamine solution are each independently selected from any one or a combination of at least two of dimethyl sulfoxide, diethyl sulfoxide, N,N-dimethylformamide, N,N-diethylformamide or tetrahydrofuran.
[0034] Preferably, the temperature of the condensation reaction is 0 to 20° C., and the time of the condensation reaction is 4 to 6 hours.
[0035] Preferably, the mass ratio of the polyamic acid solution to the amino-containing organosiloxane is 100:(0.5-2).
[0036] Preferably, the temperature of the grafting reaction is 60-80° C., and the time of the grafting reaction is 5-7 hours.
[0037] Preferably, the amino-containing organosiloxane includes any one of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane or N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, or a combination of at least two thereof.
[0038] Preferably, the density of the carbon fiber preform is between 0.60 and 0.65 g / cm 3 .
[0039] Preferably, the carbon fiber preform is obtained by needle punching carbon fiber short filaments.
[0040] Preferably, the parameters in the needle punching process are: the weight of the carbon fiber staple is 300-310 g / m 2 The density of acupuncture is 30 to 36 punctures / m 2 , the frequency of acupuncture is 300-400 times / min;
[0041] Preferably, the diameter of the carbon fiber short filaments is 5 to 7 μm, and the length of the carbon fiber short filaments is 6 to 8 mm.
[0042] Preferably, the carbon fiber staples need to be pretreated before needling, and the pretreatment specifically includes the following steps:
[0043] The carbon fiber short fibers are immersed in ethanol and subjected to ultrasonic treatment to obtain pretreated carbon fiber short fibers.
[0044] Preferably, the mass ratio of the carbon fiber staple fibers to ethanol is 1:(3-4).
[0045] Preferably, the power of the ultrasonic treatment is 200-250W.
[0046] Preferably, the temperature of the ultrasonic treatment is 20-30°C;
[0047] Preferably, the ultrasonic treatment time is 18 to 30 hours.
[0048] Preferably, the temperature of the carbonization treatment is 750-850° C., and the time of the carbonization treatment is 60-80 hours.
[0049] Preferably, the density of the carbon ceramic body precursor obtained by the carbonization treatment is 1.60-1.85 g / cm 3 .
[0050] Preferably, the high temperature sintering temperature is 2100-2300° C., and the high temperature sintering time is 42-54 hours.
[0051] In a second aspect, the present invention provides a carbon ceramic embryo body, wherein the carbon ceramic embryo body is prepared by the method for preparing a carbon ceramic embryo body as described in the first aspect.
[0052] The wear rate of the carbon ceramic body is 0.15×10 -7 cm 3 / Nm or less.
[0053] In a third aspect, the present invention provides a carbon-ceramic brake pad, wherein the carbon-ceramic brake pad is obtained by machining the carbon-ceramic blank as described in the second aspect.
[0054] Compared with the prior art, the present invention has the following beneficial effects:
[0055] (1) The present invention adopts a method of placing a carbon fiber preform in a resin impregnation solution for ultrasonic treatment. The ultrasonic treatment can increase the active groups on the surface of the carbon fiber and improve its adhesion with the resin, thereby preparing a composite material with better performance.
[0056] (2) The impregnation liquid of the present invention includes organosilicon-modified phenolic resin, siloxane-modified polyimide resin, silicon carbide, graphite and silicon dioxide; wherein, by organosilicon-modifying the phenolic resin and siloxane-modifying the polyimide resin, not only the bonding ability of the two with the carbon fiber is further improved, but also the adhesion ability of the inorganic powders of silicon carbide, graphite and silicon dioxide on the surface of the carbon fiber is improved, which greatly avoids the loss during the friction process and further reduces the wear rate of the brake pad.
[0057] (3) The present invention places the carbon fiber preform in an impregnation liquid for ultrasonic treatment, which can greatly shorten the time for impregnating the organosilicon-modified phenolic resin in an impregnation furnace, and can be completed in only 1 to 3 hours, thereby significantly improving production efficiency.
[0058] (4) The shear strength of the carbon ceramic brake pad prepared by the present invention is 5.6 to 7.7 kN / cm 2 , hardness is 51~68HRS, density is 1.60~1.93g / cm 3 The wear rate is 0.04~0.15×10 -7 cm 3 / Nm. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0060] Figure 1 The figure is a schematic diagram of the structure of the carbon-ceramic brake pad of the present invention. DETAILED DESCRIPTION
[0061] Unless otherwise defined herein, scientific and technical terms used in conjunction with the present invention shall have the meanings commonly understood by those of ordinary skill in the art. The meaning and scope of the terms should be clear, however, in the case of any potential ambiguity, the definitions provided herein take precedence over any dictionary or external definitions. In this application, unless otherwise stated, the use of "or" means "and / or". In addition, the use of the term "including" and other forms is non-limiting.
[0062] It should be noted that specific details are described in the following description to facilitate a full understanding of the present invention. However, the present invention can be implemented in a variety of other ways different from those described herein, and those skilled in the art can make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0063] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0064] In a first aspect, the present invention provides a method for preparing a carbon ceramic embryo, the method comprising the following steps:
[0065] Placing a carbon fiber preform in an impregnation liquid and performing ultrasonic treatment to obtain a modified carbon fiber preform; wherein the impregnation liquid comprises organic silicon modified phenolic resin, siloxane modified polyimide resin, silicon carbide, graphite and silicon dioxide;
[0066] The modified carbon fiber is prefabricated and subjected to carbonization treatment and high-temperature sintering to obtain the carbon ceramic embryo body.
[0067] In the present invention, the carbon fiber preform is placed in a resin impregnation solution for ultrasonic treatment. The ultrasonic treatment can increase the active groups on the surface of the carbon fiber and improve its adhesion with the resin, thereby preparing a composite material with better performance.
[0068] More specifically, the ultrasonic treatment shows its unique advantages in the modification of carbon fiber surface, especially its high-frequency vibration can effectively promote the addition of functional groups, thereby making the carbon fiber surface more active. The ultrasonic cavitation effect of ultrasonic treatment can further improve the good wetting effect and dispersion effect of the impregnation liquid of the present invention on carbon fiber. In addition, the energy input of ultrasonic waves will cause the microstructure of the carbon fiber surface to change, and the ultrasonic cavitation effect is a phenomenon that occurs through the interaction between the sound pressure field and the fluid.
[0069] Under the action of ultrasound, an acoustic-solid coupling interface is formed between the carbon fiber and the silicone-modified phenolic resin and siloxane-modified polyimide resin, causing a series of physical and chemical processes to occur inside the fiber; and the high-frequency vibration generated by the ultrasound not only helps the carbon fiber surface to be more evenly distributed in the composite resin, but also generates high-speed microjets and shock waves when the bubbles burst, thereby causing pitting on the carbon fiber surface.
[0070] In addition, when the ultrasonic cavitation bubbles burst, the high temperature and high pressure environment generated can significantly increase the speed and activity of the chemical reaction on the carbon fiber surface; at the same time, due to the thermal decomposition of the fiber inside caused by ultrasonic radiation, the chemical reaction rate is further enhanced, and the formation and diffusion of the product are promoted, ultimately achieving the purpose of improving the material properties and improving the binding ability of carbon fiber, silicone-modified phenolic resin, and siloxane-modified polyimide resin; and it can significantly improve the dispersion and binding ability of silicon carbide, graphite and silicon dioxide in the resin, making the impregnation process more stable.
[0071] Furthermore, the impregnation liquid of the present invention includes organosilicon-modified phenolic resin, siloxane-modified polyimide resin, silicon carbide, graphite and silicon dioxide; wherein, by organosilicon-modifying the phenolic resin and siloxane-modifying the polyimide resin, not only the binding ability of the two with carbon fiber is further improved, but also the adhesion ability of silicon carbide, graphite and silicon dioxide inorganic powders on the surface of carbon fiber is improved, which greatly avoids the loss during the friction process and further reduces the wear rate of the brake pad. Therefore, the mechanical strength, high temperature resistance and friction resistance of the composite material can be significantly improved by using the specific impregnation liquid of the present invention for impregnation, and then under the action of ultrasonic treatment.
[0072] As an optional embodiment of the present invention, the process parameters of the ultrasonic treatment are: power density is 6 to 12 W / cm 2 , for example, it can be 6W / cm 2 , 7W / cm 2 , 8W / cm 2 , 9W / cm 2 , 10W / cm 2The ultrasonic frequency is 40-42kHz, for example, 40kHz, 40.5kHz, 41kHz, 41.5kHz, 42kHz, etc. The ultrasonic duty cycle is 50-60%, for example, 50%, 52%, 54%, 56%, 58%, 60%, etc.
[0073] As an optional embodiment of the present invention, the temperature of ultrasonic treatment of the carbon fiber preform in the impregnation liquid is 30-40°C, for example, 30°C, 32°C, 34°C, 36°C, 38°C, 40°C, etc.
[0074] As an optional embodiment of the present invention, the carbon fiber preform is ultrasonically treated in the impregnation liquid for 1 to 3 hours, for example, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, etc.
[0075] It should be noted that, in the prior art, an impregnation furnace is generally used to impregnate phenolic resin, but the time required is generally about 48 hours. In the present invention, the carbon fiber preform is placed in an impregnation liquid for ultrasonic treatment under the ultrasonic conditions as described above, which can greatly shorten the time for impregnation of organosilicon-modified phenolic resin in the impregnation furnace. It only takes 1 to 3 hours to complete, which significantly improves production efficiency.
[0076] As an optional embodiment of the present invention, the mass ratio of the carbon fiber preform to the impregnating liquid is 1:(1-1.5), for example, it can be 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, etc.
[0077] As an optional embodiment of the present invention, the infiltration liquid comprises the following components in parts by weight:
[0078]
[0079] In the impregnation solution, the content of the silicone-modified phenolic resin is 20 to 40 parts, for example, 20 parts, 22 parts, 24 parts, 26 parts, 28 parts, 30 parts, 32 parts, 34 parts, 36 parts, 38 parts, 40 parts, etc.
[0080] In the impregnation solution, the content of the siloxane-modified polyimide resin is 10 to 20 parts, for example, 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, etc.
[0081] In the infiltration liquid, the content of silicon carbide is 15 to 25 parts, for example, it can be 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, 21 parts, 22 parts, 23 parts, 24 parts, 25 parts, etc.
[0082] In the impregnation solution, the content of graphite is 10 to 20 parts, for example, it can be 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, etc.
[0083] In the infiltration solution, the content of silicon dioxide is 10 to 20 parts, for example, it can be 10 parts, 11 parts, 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts, 18 parts, 19 parts, 20 parts, etc.
[0084] As an optional embodiment of the present invention, the organosilicon-modified phenolic resin is prepared by the following steps:
[0085] In the presence of an acidic catalyst, a phenolic compound, an aldehyde compound and an organosilicon monomer are reacted to obtain the organosilicon-modified phenolic resin.
[0086] In the present invention, during the preparation of phenolic resin, organic silicon monomers are added for grafting modification, which further improves the bonding ability of phenolic resin with carbon fiber, improves its adhesion ability with silicon carbide, graphite and silicon dioxide inorganic powders on the surface of carbon fiber, and further improves the mechanical strength, high temperature resistance and wear resistance of the brake pad.
[0087] As an optional embodiment of the present invention, the acidic catalyst is selected from any one of hydrochloric acid, phosphoric acid, sulfuric acid, oxalic acid or boric acid, or a combination of at least two thereof.
[0088] As an optional embodiment of the present invention, the phenolic compound includes resorcinol and / or catechol.
[0089] As an optional embodiment of the present invention, the aldehyde compound includes any one of formaldehyde, acetaldehyde or furfural, or a combination of at least two of them.
[0090] As an optional embodiment of the present invention, the organosilicon monomer includes C10-C18 long-chain silane.
[0091] As an optional embodiment of the present invention, the C10-C20 long-chain silane is selected from any one of decyltrimethoxysilane, dodecyltrimethoxysilane, tetradecyltrimethoxysilane, hexadecyltrimethoxysilane or octadecyltrimethoxysilane, or a combination of at least two thereof.
[0092] In the present invention, by selecting a long carbon chain silane coupling agent to modify the phenolic resin, the heat resistance and friction resistance of the modified phenolic resin are further improved, and the problem of reduced friction coefficient due to thermal decomposition of the resin is effectively avoided.
[0093] As an optional embodiment of the present invention, the molar ratio of the phenolic compound, the aldehyde compound and the organosilicon monomer is 1.0:(1.0-1.2):(0.1-0.5);
[0094] Here, “1.0-1.2” may be, for example, 1.0, 1.05, 1.1, 1.15, 1.2, etc.;
[0095] Here, “0.1 to 0.5” may be, for example, 0.1, 0.2, 0.3, 0.4, 0.5, etc.
[0096] As an optional embodiment of the present invention, the amount of the acidic catalyst added is 0.5-1.5% of the mass of the phenolic compound, for example, it can be 0.5%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.5%, etc.
[0097] As an optional embodiment of the present invention, the reaction process is specifically as follows:
[0098] First, react at 70-90°C (for example, 70°C, 75°C, 80°C, 85°C, 90°C, etc.) for 5-6h (for example, 5h, 5.2h, 5.4h, 5.6h, 5.8h, 6h, etc.), distill under reduced pressure for 1-3h (for example, 1h, 1.5h, 2h, 2.5h, 3h, etc.), and then react at 130-150°C (for example, 130°C, 135°C, 140°C, 145°C, 150°C, etc.) for 0.5-2h (for example, 0.5h, 0.6h, 0.8h, 1h, 1.2h, 1.4h, 1.6h, 1.8h, 2h, etc.), add a solvent to adjust the solid content, and obtain the organosilicon-modified phenolic resin.
[0099] As an optional embodiment of the present invention, the solvent is methanol and / or ethanol.
[0100] As an optional embodiment of the present invention, the solid content of the organosilicon-modified phenolic resin is 60-70wt%, for example, it can be 60wt%, 62wt%, 64wt%, 66wt%, 68wt%, 70wt% and the like.
[0101] As an optional embodiment of the present invention, the siloxane-modified polyimide resin is prepared by the following steps:
[0102] The dianhydride solution and the diamine solution are mixed to carry out a condensation reaction to obtain a polyamic acid solution;
[0103] The polyamic acid solution and the amino-containing organic siloxane are mixed and subjected to a grafting reaction to obtain the siloxane-modified polyimide resin.
[0104] In the present invention, during the preparation of phenolic resin, amino-containing organosiloxane is added for grafting modification, thereby further improving the strength and friction resistance of the carbon ceramic body and the carbon ceramic brake pad prepared therefrom, and avoiding the generation of debris during high temperature and / or repeated friction.
[0105] As an optional embodiment of the present invention, the molar ratio of the dianhydride to the diamine is 1.0:(1.0-1.2), for example, it can be 1.0:1.0, 1.0:1.05, 1.0:1.1, 1.0:1.15, 1.0:1.2, etc.
[0106] As an optional embodiment of the present invention, the concentration of the dianhydride solution and the diamine solution is independently 1 to 10wt%, for example, it can be 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt%, 10wt% and the like.
[0107] As an optional embodiment of the present invention, each group of solvents in the dianhydride solution and the diamine solution is independently selected from any one or a combination of at least two of dimethyl sulfoxide, diethyl sulfoxide, N,N-dimethylformamide, N,N-diethylformamide or tetrahydrofuran.
[0108] As an optional embodiment of the present invention, the temperature of the condensation reaction is 0-20°C, for example, it can be 0°C, 2°C, 4°C, 6°C, 8°C, 10°C, 12°C, 14°C, 16°C, 18°C, 20°C, etc., and the time of the condensation reaction is 4-6h, for example, it can be 4h, 4.5h, 5h, 5.5h, 6h, etc.
[0109] As an optional embodiment of the present invention, the mass ratio of the polyamic acid solution to the amino-containing organosiloxane is 100:(0.5-2), for example, it can be 100:0.5, 100:0.6, 100:0.8, 100:1.0, 100:1.2, 100:1.4, 100:4.6, 100:1.8, 100:2, etc.
[0110] As an optional embodiment of the present invention, the temperature of the grafting reaction is 60-80°C, for example, 60°C, 65°C, 70°C, 75°C, 80°C, etc., and the time of the grafting reaction is 5-7h, for example, 5h, 5.5h, 6h, 6.5h, 7h, etc.
[0111] As an optional embodiment of the present invention, the amino-containing organosiloxane includes any one of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane or N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, or a combination of at least two thereof.
[0112] As an optional embodiment of the present invention, the density of the carbon fiber preform is 0.60 to 0.65 g / cm 3 , for example, it can be 0.60 g / cm 3 、0.61g / cm 3 , 0.62g / cm 3 , 0.63g / cm 3 , 0.64g / cm 3 , 0.65g / cm 3 wait.
[0113] As an optional embodiment of the present invention, the carbon fiber preform is obtained by needle punching carbon fiber short filaments.
[0114] As an optional embodiment of the present invention, the parameters in the needle punching process are: the weight of the carbon fiber staple is 300-310 g / m 2 , for example, it can be 300g / m 2 , 302g / m 2 , 304g / m 2 , 306g / m 2 , 308g / m 2 , 310g / m 2 The density of acupuncture is 30 to 36 punctures / m 2 , for example, it can be 30 thorns / m 2 , 31 thorns / m 2 、32 thorns / m 2 、33 thorns / m 2 、34 thorns / m 2 , 35 thorns / m 2 , 36 thorns / m 2 The acupuncture frequency is 300 to 400 times / min, for example, 300 times / min, 320 times / min, 340 times / min, 360 times / min, 380 times / min, 400 times / min, etc.
[0115] As an optional embodiment of the present invention, the diameter of the carbon fiber staple filaments is 5 to 7 μm, for example, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, etc., and the length of the carbon fiber staple filaments is 6 to 8 mm, for example, 6 mm, 6.5 mm, 7 mm, 7.5 mm, 8 mm, etc.
[0116] As an optional embodiment of the present invention, the carbon fiber staples need to be pretreated before needling, and the pretreatment specifically includes the following steps:
[0117] The carbon fiber short fibers are immersed in ethanol and subjected to ultrasonic treatment to obtain pretreated carbon fiber short fibers.
[0118] As an optional embodiment of the present invention, the mass ratio of the carbon fiber staple filaments to ethanol is 1:(3-4), for example, it can be 1:3, 1:3.2, 1:3.4, 1:3.6, 1:3.8, 1:4, etc.
[0119] As an optional embodiment of the present invention, during the pretreatment process, the power of the ultrasonic treatment is 200-250W, for example, it can be 200W, 210W, 220W, 230W, 240W, 250W, etc.
[0120] As an optional embodiment of the present invention, during the pretreatment process, the temperature of the ultrasonic treatment is 20-30°C, for example, it can be 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, etc.
[0121] As an optional embodiment of the present invention, during the pretreatment process, the ultrasonic treatment time is 18 to 30 hours, for example, it can be 18 hours, 20 hours, 22 hours, 24 hours, 26 hours, 28 hours, 30 hours, etc.
[0122] As an optional embodiment of the present invention, the temperature of the carbonization treatment is 750-850°C, for example, it can be 750°C, 760°C, 780°C, 800°C, 820°C, 840°C, 850°C, etc., and the time of the carbonization treatment is 60-80h, for example, it can be 60h, 62h, 64h, 66h, 68h, 70h, 72h, 74h, 76h, 78h, 80h, etc.
[0123] As an optional embodiment of the present invention, the density of the carbon ceramic embryo precursor obtained by the carbonization treatment is 1.60-1.85 g / cm 3 , for example, it can be 1.60 g / cm 3 , 1.65g / cm 3 , 1.70g / cm 3 , 1.75g / cm 3 , 1.80g / cm 3 , 1.85g / cm 3 wait.
[0124] As an optional embodiment of the present invention, the high temperature sintering temperature is 2100-2300°C, for example, it can be 2100°C, 2150°C, 2200°C, 2250°C, 2300°C, etc., and the high temperature sintering time is 42-54h, for example, it can be 42h, 44h, 46h, 48h, 50h, 52h, 54h, etc.
[0125] In a second aspect, the present invention provides a carbon ceramic embryo body, wherein the carbon ceramic embryo body is prepared by the method for preparing a carbon ceramic embryo body as described in the first aspect.
[0126] As an optional embodiment of the present invention, the wear rate of the carbon ceramic body is 0.15×10 -7 cm 3 / Nm or less, for example, 0.15×10 -7 cm 3 / Nm, 0.14cm 3 / Nm, 0.13cm 3 / Nm, 0.12cm 3 / Nm, 0.11cm 3 / Nm, 0.10cm 3 / Nm, 0.09cm 3 / Nm, 0.08cm 3 / Nm, 0.07cm 3 / Nm, 0.06cm 3 / Nm, 0.05cm 3 / Nm, 0.04cm 3 / Nm, 0.03cm 3 / Nm, 0.02cm 3 / Nm, 0.01cm 3 / Nm, etc.
[0127] In a third aspect, the present invention provides a carbon ceramic brake pad (such as Figure 1 As shown), the carbon-ceramic brake pad is obtained by machining the carbon-ceramic embryo as described in the second aspect.
[0128] The present invention is further described below by way of examples. Unless otherwise specified, the materials in the examples are prepared according to existing methods or directly purchased from the market.
[0129] Preparation Example 1
[0130] This preparation example provides a silicone-modified phenolic resin, which is prepared by the following steps:
[0131] Resorcinol, formaldehyde and dodecyltrimethoxysilane are mixed in a molar ratio of 1.0:1.05:0.2, and hydrochloric acid accounting for 1.0% of the mass of the resorcinol is added to obtain a reaction solution; the reaction solution is first reacted at 80°C for 5.5 hours, distilled under reduced pressure for 2 hours, and then reacted at 140°C for 1 hour, and methanol is added to adjust the solid content to 65wt% to obtain the organosilicon-modified phenolic resin.
[0132] Preparation Example 2
[0133] This preparation example provides a silicone-modified phenolic resin, which is prepared by the following steps:
[0134] The molar ratio of catechol, formaldehyde and tetradecyltrimethoxysilane is 1.0:1.05:0.25, and then 1.0% of phosphoric acid by mass of the catechol is added to obtain a reaction solution; the reaction solution is first reacted at 80° C. for 5.5 hours, distilled under reduced pressure for 2 hours, and then reacted at 150° C. for 1 hour, and methanol is added to adjust the solid content to 65wt% to obtain the organosilicon-modified phenolic resin.
[0135] Preparation Example 3
[0136] This preparation example provides a silicone-modified phenolic resin, which is prepared by the following steps:
[0137] The molar ratio of catechol, formaldehyde and hexadecyltrimethoxysilane is 1.0:1.1:0.3, and then 1.2% of boric acid by mass of the catechol is added to obtain a reaction solution; the reaction solution is first reacted at 85°C for 5 hours, and then distilled under reduced pressure for 2 hours, and then reacted at 140°C for 2 hours, and ethanol is added to adjust the solid content to 65wt% to obtain the organosilicon-modified phenolic resin.
[0138] Preparation Example 4
[0139] This preparation example provides a siloxane-modified polyimide resin, which is prepared by the following steps:
[0140] (a) preparing a 5 wt % m-phenylenediamine solution and a 5 wt % pyromellitic anhydride solution using N,N-dimethylformamide respectively; mixing the m-phenylenediamine solution and the pyromellitic anhydride solution at a molar ratio of 1:1, and reacting them at 10° C. for 5 hours to obtain a polyamic acid solution;
[0141] (b) mixing the polyamic acid solution and γ-aminopropyltrimethoxysilane at a mass ratio of 100:1, and reacting at 70° C. for 6 hours to obtain the siloxane-modified polyimide resin.
[0142] Preparation Example 5
[0143] This preparation example provides a siloxane-modified polyimide resin, which is prepared by the following steps:
[0144] (a) preparing a 5 wt % p-phenylenediamine solution and a 5 wt % 3,3',4,4'-biphenyltetracarboxylic acid dianhydride solution respectively using N,N-dimethylformamide; mixing the p-phenylenediamine solution and the 3,3',4,4'-biphenyltetracarboxylic acid dianhydride solution at a molar ratio of 1:1.05, and reacting at 5° C. for 6 hours to obtain a polyamic acid solution;
[0145] (b) The polyamic acid solution and N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane were mixed at a mass ratio of 100:1, and reacted at 75° C. for 5.5 hours to obtain the siloxane-modified polyimide resin.
[0146] Preparation Example 6
[0147] This preparation example provides a siloxane-modified polyimide resin, which is prepared by the following steps:
[0148] (a) preparing 5 wt% p-phenylenediamine solution and 5 wt% 3,3',4,4'-benzophenonetetracarboxylic dianhydride respectively by using N,N-dimethylformamide; mixing the p-phenylenediamine solution and the 3,3',4,4'-benzophenonetetracarboxylic dianhydride solution at a molar ratio of 1:1, and reacting at 10° C. for 6 hours to obtain a polyamic acid solution;
[0149] (b) mixing the polyamic acid solution and N-(β-aminoethyl)-γ-aminopropyltriethoxysilane at a mass ratio of 100:1, and reacting at 80° C. for 5 hours to obtain the siloxane-modified polyimide resin.
[0150] Comparative Preparation Example 1
[0151] This comparative preparation example provides a phenolic resin, which is prepared by the following steps:
[0152] Resorcinol and formaldehyde are mixed at a molar ratio of 1.0:1.05, and hydrochloric acid accounting for 1.0% of the mass of the resorcinol is added to obtain a reaction solution; the reaction solution is first reacted at 80° C. for 5.5 hours, distilled under reduced pressure for 2 hours, and then reacted at 140° C. for 1 hour, and methanol is added to adjust the solid content to 65wt% to obtain the phenolic resin.
[0153] Comparative Preparation Example 2
[0154] This preparation example provides a polyimide resin, which is prepared by the following steps:
[0155] N,N-dimethylformamide was used to prepare 5 wt% m-phenylenediamine solution and 5 wt% pyromellitic anhydride solution respectively; the m-phenylenediamine solution and the pyromellitic anhydride solution were mixed at a molar ratio of 1:1, and reacted at 10° C. for 5 hours to obtain a polyamic acid solution.
[0156] Example 1
[0157] This embodiment provides a carbon ceramic embryo body, and the carbon ceramic embryo body is prepared by the following steps:
[0158] S1. Preparation of carbon fiber preform:
[0159] S1-1, placing carbon fiber short filaments with a diameter of 6 μm and a length of 7 mm in an ultrasonic cleaning apparatus filled with ethanol, and ultrasonicating at 26° C. and a power of 220 W for 24 h to obtain pretreated carbon fiber short filaments;
[0160] S1-2, needle punching the pretreated carbon fiber short filaments into a carbon fiber preform; wherein the weight of the carbon fiber short filaments is 305g / m 2 The density of acupuncture is 33 punctures / m 2 The needle punching frequency is 350 times / min; the density of the obtained carbon fiber preform is 0.45g / cm 3 .
[0161] S2. Ultrasonic treatment:
[0162] S2-1, 30 parts of the organosilicon-modified phenolic resin provided in Preparation Example 1, 15 parts of the siloxane-modified polyimide resin provided in Preparation Example 4, 20 parts of silicon carbide, 20 parts of graphite and 15 parts of silicon dioxide are mixed to obtain an impregnation solution;
[0163] S2-2, placing 100 parts of the carbon fiber preform in 100 parts of the impregnation solution, and then ultrasonicating for 2 hours to obtain a modified carbon fiber preform; the process parameters of the ultrasonic treatment are: power density of 9W / cm 2 , the ultrasonic frequency is 41kHz, and the ultrasonic duty cycle is 55%.
[0164] S3, Carbonization treatment:
[0165] The modified carbon fiber preform is carbonized at 800°C for 70 hours to obtain a precursor of a carbon ceramic body; wherein the density of the precursor of the carbon ceramic body is 1.8 g / cm 3 .
[0166] S4. High temperature treatment:
[0167] The precursor of the carbon ceramic embryo body is subjected to high temperature treatment at 2200° C. for 48 hours to obtain the carbon ceramic embryo body.
[0168] Example 2
[0169] This embodiment provides a carbon ceramic embryo body, and the carbon ceramic embryo body is prepared by the following steps:
[0170] S1. Preparation of carbon fiber preform:
[0171] S1-1, placing carbon fiber short filaments with a diameter of 6 μm and a length of 7 mm in an ultrasonic cleaning apparatus filled with ethanol, and ultrasonicating at 26° C. and a power of 220 W for 24 h to obtain pretreated carbon fiber short filaments;
[0172] S1-2, needle punching the pretreated carbon fiber short filaments into a carbon fiber preform; wherein the weight of the carbon fiber short filaments is 305g / m 2 The density of acupuncture is 33 punctures / m 2 The needle punching frequency is 350 times / min; the density of the obtained carbon fiber preform is 0.45g / cm 3 .
[0173] S2. Ultrasonic treatment:
[0174] S2-1, 40 parts of the organosilicon-modified phenolic resin provided in Preparation Example 2, 10 parts of the siloxane-modified polyimide resin provided in Preparation Example 5, 25 parts of silicon carbide, 15 parts of graphite and 10 parts of silicon dioxide are mixed to obtain an impregnation solution;
[0175] S2-2, placing 100 parts of the carbon fiber preform in 100 parts of the impregnation solution, and then ultrasonicating for 2 hours to obtain a modified carbon fiber preform; the process parameters of the ultrasonic treatment are: power density of 8W / cm 2 , the ultrasonic frequency is 42kHz, and the ultrasonic duty cycle is 58%.
[0176] S3, Carbonization treatment:
[0177] The modified carbon fiber preform is carbonized at 800°C for 70 hours to obtain a precursor of a carbon ceramic body; wherein the density of the precursor of the carbon ceramic body is 1.8 g / cm 3 .
[0178] S4. High temperature treatment:
[0179] The precursor of the carbon ceramic embryo body is subjected to high temperature treatment at 2200° C. for 48 hours to obtain the carbon ceramic embryo body.
[0180] Example 3
[0181] This embodiment provides a carbon ceramic embryo body, and the carbon ceramic embryo body is prepared by the following steps:
[0182] S1. Preparation of carbon fiber preform:
[0183] S1-1, placing carbon fiber short filaments with a diameter of 6 μm and a length of 7 mm in an ultrasonic cleaning apparatus filled with ethanol, and ultrasonicating at 26° C. and a power of 220 W for 24 h to obtain pretreated carbon fiber short filaments;
[0184] S1-2, needle punching the pretreated carbon fiber short filaments into a carbon fiber preform; wherein the weight of the carbon fiber short filaments is 305g / m 2 The density of acupuncture is 33 punctures / m 2 The needle punching frequency is 350 times / min; the density of the obtained carbon fiber preform is 0.45g / cm 3 .
[0185] S2. Ultrasonic treatment:
[0186] S2-1, 20 parts of the organosilicon-modified phenolic resin provided in Preparation Example 3, 20 parts of the siloxane-modified polyimide resin provided in Preparation Example 6, 25 parts of silicon carbide, 20 parts of graphite and 15 parts of silicon dioxide are mixed to obtain an impregnation solution;
[0187] S2-2, placing 100 parts of the carbon fiber preform in 100 parts of the impregnation solution, and then ultrasonicating for 2 hours to obtain a modified carbon fiber preform; the process parameters of the ultrasonic treatment are: power density of 10W / cm 2 , the ultrasonic frequency is 40kHz, and the ultrasonic duty cycle is 54%.
[0188] S3, Carbonization treatment:
[0189] The modified carbon fiber preform is carbonized at 800°C for 70 hours to obtain a precursor of a carbon ceramic body; wherein the density of the precursor of the carbon ceramic body is 1.8 g / cm 3 .
[0190] S4. High temperature treatment:
[0191] The precursor of the carbon ceramic embryo body is subjected to high temperature treatment at 2200° C. for 48 hours to obtain the carbon ceramic embryo body.
[0192] Example 4
[0193] This embodiment provides a carbon ceramic embryo body, which is different from the embodiment 1 in that, in S2-2, the process parameters of the ultrasonic treatment are: power density is 4W / cm 2 , the ultrasonic frequency is 45 kHz, the ultrasonic duty cycle is 45%, and the other steps are exactly the same as those in Example 1.
[0194] Example 5
[0195] This embodiment provides a carbon ceramic embryo body, which is different from the embodiment 1 in that, in S2-2, the process parameters of the ultrasonic treatment are: power density is 15W / cm 2 , the ultrasonic frequency is 35 kHz, the ultrasonic duty cycle is 40%, and the other steps are exactly the same as those in Example 1.
[0196] Example 6
[0197] This embodiment provides a carbon ceramic body, which is different from Embodiment 1 in that, in S2-3, the temperature of the carbonization treatment is 700° C., the time of the carbonization treatment is 80 h, and the other steps are completely consistent with Embodiment 1.
[0198] Example 7
[0199] This embodiment provides a carbon ceramic body, which is different from the embodiment 1 in that, in S2-3, the temperature of the carbonization treatment is 900° C., the time of the carbonization treatment is 60 h, and the other steps are completely consistent with the embodiment 1.
[0200] Example 8
[0201] This embodiment provides a carbon ceramic body, which is different from the embodiment 1 in that, in S2-3, the temperature of the carbonization treatment is 2000° C., the time of the carbonization treatment is 60 h, and the other steps are completely consistent with the embodiment 1.
[0202] Example 9
[0203] This embodiment provides a carbon ceramic body, which is different from Embodiment 1 in that, in S2-3, the temperature of the carbonization treatment is 2400° C., the time of the carbonization treatment is 36 h, and the other steps are completely consistent with Embodiment 1.
[0204] Comparative Example 1
[0205] This comparative example provides a carbon ceramic embryo, which is different from Example 1 only in that S2-2 does not use ultrasonic treatment, 100 parts of carbon fiber preforms are placed in 100 parts of impregnation liquid, and then immersed at 30°C for 48 hours, and the other steps are completely consistent with Example 1.
[0206] Comparative Example 2
[0207] This comparative example provides a carbon ceramic embryo, which is different from Example 1 only in that S2-2 does not use ultrasonic treatment, 100 parts of carbon fiber preforms are placed in 100 parts of impregnation liquid, and then stirred at 25°C and 500 rpm for 12 hours, and the other steps are exactly the same as Example 1.
[0208] Comparative Example 3
[0209] This comparative example provides a carbon ceramic body, which differs from Example 1 only in that in S2-1, the organosilicon-modified phenolic resin provided in Preparation Example 1 is replaced with an equal mass of phenolic resin provided in Comparative Preparation Example 1, and the other steps are completely consistent with Example 1.
[0210] Comparative Example 4
[0211] This comparative example provides a carbon ceramic body, which differs from Example 1 only in that in S2-1, the siloxane-modified polyimide resin provided in Preparation Example 4 is replaced by an equal mass of the polyimide resin provided in Comparative Preparation Example 2, and the other steps are completely consistent with Example 1.
[0212] Comparative Example 5
[0213] This comparative example provides a carbon ceramic embryo body, which is different from Example 1 in that the impregnation liquid does not contain silicone-modified phenolic resin, the content of siloxane-modified polyimide resin is increased to 45 parts, and the other steps are completely consistent with Example 1.
[0214] Comparative Example 6
[0215] This comparative example provides a carbon ceramic embryo body, which is different from Example 1 in that the impregnation liquid does not contain siloxane-modified polyimide resin, the content of organosilicon-modified phenolic resin is increased to 45 parts, and the other steps are completely consistent with Example 1.
[0216] Test Case
[0217] Test samples: carbon ceramic embryos provided in Examples 1 to 9 and carbon ceramic embryos provided in Comparative Examples 1 to 6;
[0218] Test method:
[0219] According to the standard GB / T223102008, the shear test is done, the hardness test is done according to GB / T57662007, the density test is done according to JC / T6852009, and the wear rate test is done according to GB / T118342000.
[0220] The test results are shown in Table 1 below:
[0221] Table 1
[0222]
[0223] As shown in Table 1 above, the shear force of the carbon ceramic body prepared by the present invention is 7.2-8.5 kN / cm 2 , hardness is 57~68HRS, density is 1.82~1.93g / cm 3 The wear rate is 0.04~0.09×10 -7 cm 3 / Nm, and the silicon carbide content is 26.09-28.56wt%. This shows that the preparation method of the present invention places the carbon fiber preform in the resin impregnation liquid for ultrasonic treatment, which has a good impregnation effect and dispersion effect on the carbon fiber through ultrasonic cavitation, significantly improves the bonding ability of the carbon fiber and the resin, thereby preparing a composite material with better performance, thereby preparing a carbon-ceramic brake pad with high mechanical strength, high temperature resistance and friction resistance.
[0224] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a carbon ceramic embryo body, characterized in that: The method for preparing the carbon ceramic embryo body comprises the following steps: Placing a carbon fiber preform in an impregnation liquid and performing ultrasonic treatment to obtain a modified carbon fiber preform; wherein the impregnation liquid comprises organic silicon modified phenolic resin, siloxane modified polyimide resin, silicon carbide, graphite and silicon dioxide; The modified carbon fiber is prefabricated and subjected to carbonization treatment and high-temperature sintering to obtain the carbon ceramic embryo body.
2. The method for preparing a carbon ceramic embryo body according to claim 1, characterized in that: The process parameters of the ultrasonic treatment are: power density of 6 to 12 W / cm 2 , the ultrasonic frequency is 40-42kHz, and the ultrasonic duty cycle is 50-60%; And / or, the temperature of the ultrasonic treatment is 30-40°C; And / or, the ultrasonic treatment time is 1 to 3 hours.
3. The method for preparing a carbon ceramic embryo body according to claim 1, characterized in that: The mass ratio of the carbon fiber preform to the impregnation liquid is 1:(1-1.5); Preferably, the impregnation solution comprises the following components by weight:
4. The method for preparing a carbon ceramic embryo body according to claim 1 or 3, characterized in that: The organosilicon-modified phenolic resin is prepared by the following steps: In the presence of an acidic catalyst, a phenolic compound, an aldehyde compound and an organosilicon monomer are reacted to obtain the organosilicon-modified phenolic resin; Preferably, the acidic catalyst is selected from any one or a combination of at least two of hydrochloric acid, phosphoric acid, sulfuric acid, oxalic acid or boric acid; Preferably, the phenolic compound comprises resorcinol and / or catechol; Preferably, the aldehyde compound includes any one or a combination of at least two of formaldehyde, acetaldehyde or furfural; Preferably, the organosilicon monomer comprises a C10-C18 long-chain silane; Preferably, the C10-C20 long-chain silane is selected from any one or a combination of at least two of decyltrimethoxysilane, dodecyltrimethoxysilane, tetradecyltrimethoxysilane, hexadecyltrimethoxysilane or octadecyltrimethoxysilane; Preferably, the molar ratio of the phenolic compound, the aldehyde compound and the organosilicon monomer is 1.0:(1.0-1.2):(0.1-0.5); Preferably, the amount of the acidic catalyst added is 0.5 to 1.5% of the mass of the phenolic compound; Preferably, the reaction process is specifically as follows: first react at 70-90° C. for 5-6 hours, distill under reduced pressure for 1-3 hours, then react at 130-150° C. for 0.5-2 hours, add a solvent to adjust the solid content, and obtain the organosilicon-modified phenolic resin; Preferably, the solvent is methanol and / or ethanol; Preferably, the solid content of the organosilicon-modified phenolic resin is 60-70 wt %.
5. The method for preparing a carbon ceramic embryo body according to claim 1 or 3, characterized in that: The siloxane-modified polyimide resin is prepared by the following steps: The dianhydride solution and the diamine solution are mixed to carry out a condensation reaction to obtain a polyamic acid solution; The polyamic acid solution and the amino-containing organosiloxane are mixed to carry out a grafting reaction to obtain the siloxane-modified polyimide resin; Preferably, the molar ratio of the dianhydride to the diamine is 1.0:(1.0-1.2); Preferably, the concentrations of the dianhydride solution and the diamine solution are independently 1 to 10 wt %, and the solvents in the dianhydride solution and the diamine solution are independently selected from any one or a combination of at least two of dimethyl sulfoxide, diethyl sulfoxide, N,N-dimethylformamide, N,N-diethylformamide or tetrahydrofuran; Preferably, the condensation reaction temperature is 0 to 20°C, and the condensation reaction time is 4 to 6 hours; Preferably, the mass ratio of the polyamic acid solution to the amino-containing organosiloxane is 100:(0.5-2); Preferably, the temperature of the grafting reaction is 60 to 80° C., and the time of the grafting reaction is 5 to 7 hours; Preferably, the amino-containing organosiloxane includes any one of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane or N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, or a combination of at least two thereof.
6. The method for preparing a carbon ceramic embryo body according to claim 1, characterized in that: The density of the carbon fiber preform is 0.60-0.65 g / cm 3 ; Preferably, the carbon fiber preform is obtained by needle punching short carbon fiber filaments; Preferably, the parameters during the needle punching process are: the weight of the carbon fiber staple is 300-310 g / m 2 The density of acupuncture is 30 to 36 punctures / m 2 , the frequency of acupuncture is 300-400 times / min; Preferably, the diameter of the carbon fiber short filaments is 5 to 7 μm, and the length of the carbon fiber short filaments is 6 to 8 mm; Preferably, the carbon fiber staples need to be pretreated before needling, and the pretreatment specifically includes the following steps: The carbon fiber short fibers are immersed in ethanol and subjected to ultrasonic treatment to obtain pretreated carbon fiber short fibers; Preferably, the mass ratio of the carbon fiber short filaments to ethanol is 1:(3-4); Preferably, the power of the ultrasonic treatment is 200-250W; And / or, the temperature of the ultrasonic treatment is 20-30°C; And / or, the ultrasonic treatment time is 18 to 30 hours.
7. The method for preparing a carbon ceramic embryo body according to claim 1, characterized in that: The temperature of the carbonization treatment is 750-850°C, and the time of the carbonization treatment is 60-80h; Preferably, the density of the carbon ceramic body precursor obtained by the carbonization treatment is 1.60-1.85 g / cm 3 .
8. The method for preparing a carbon ceramic embryo body according to claim 1, characterized in that: The high temperature sintering temperature is 2100-2300° C., and the high temperature sintering time is 42-54 hours.
9. A carbon ceramic embryo body, characterized in that: The carbon ceramic embryo body is prepared by the method for preparing a carbon ceramic embryo body according to any one of claims 1 to 8; The wear rate of the carbon ceramic body is 0.15×10 -7 cm 3 / Nm or less.
10. A carbon ceramic brake pad, characterized in that: The carbon ceramic brake pad is obtained by machining the carbon ceramic blank as claimed in claim 9.
Citation Information
Patent Citations
Preparation method and application of polyimide-containing carbon / carbon composite material dipping slurry
CN114195541A
Carbon fiber ceramic brake pad and preparation method thereof
CN117534498A
Friction material, brake pad prepared from friction material as well as preparation method and application of friction material
CN117887204A
Carbon fiber reinforced ceramic matrix composite carbon interface layer and preparation method thereof
CN117923930A
Production of fiber reinforced composite material
JP1993070227A
Cited By
Aqueous polyamic acid composition, electrode mixture slurry, electrode, secondary battery, method for producing aqueous polyamic acid composition, and method for producing electrode
WO2026211811A1