Alkyl aluminum compound, rare earth catalyst composition prepared from alkyl aluminum compound and application of alkyl aluminum compound in preparation of double-end functionalized rubber

By using functionalized alkylaluminum compounds to prepare amine-based functionalized rare earth catalysts, the problem of poor compatibility between rare earth rubber and filler is solved, the mechanical properties of rubber and filler dispersion are improved, and the efficient preparation of double-end functionalized rare earth rubber is achieved. .

CN119019442AActive Publication Date: 2024-11-26DALIAN INSTITUTE OF CHEMICAL PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202310608157.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-26
Publication Date
2024-11-26
Estimated Expiration
2043-05-26

AI Technical Summary

Technical Problem

Rare earth rubber has poor compatibility with reinforcement fillers, which affects its performance. The traditional end capping method has low reaction efficiency and high residual small molecules content, resulting in low mechanical properties.

Method used

Using an amine-functionalized rare earth catalyst composition based on functionalized alkylaluminum compounds, the amine-functional group is efficiently introduced to the rubber molecular chain end through anionic polymerization method, combined with the end capping system, double-end functionalized rare earth rubber is prepared to improve filler dispersion. Sex and interface strength.

Benefits of technology

The nanodispersion between rubber and filler is achieved, the deformation energy consumption and rolling resistance are reduced, the mechanical properties and filler compatibility of rubber are improved, and the preparation process is simple and efficient.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004251617040000031
    Figure BDA0004251617040000031
  • Figure BDA0004251617040000041
    Figure BDA0004251617040000041
  • Figure BDA0004251617040000051
    Figure BDA0004251617040000051
Patent Text Reader

Abstract

The invention discloses a functionalized alkyl aluminum compound, a functionalized rare earth catalyst composition prepared from the functionalized alkyl aluminum compound and application of the functionalized alkyl aluminum compound to preparation of double-end functionalized rubber, the functionalized alkyl aluminum compound is an alkyl aluminum compound with an amido polar group, and the compound can be controllably prepared through an active anionic polymerization method. The method has the characteristics of flexibility and high efficiency, the prepared functionalized rare earth catalyst composition can be applied to preparation of double-end functionalized rubber, and the rare earth catalyst composition is composed of a rare earth metal compound, a functionalized alkyl aluminum compound and a chlorine source in a molar ratio of 1: (10-30): (0-5.0). The catalytic system can efficiently catalyze conjugated olefin polymerization to obtain narrow-distribution stereoregular rubber with a functionalized initiating end, the functionalization efficiency can reach 95%, the cis-diolefin stereoregularity can reach 96%, and the molecular weight distribution is lower than 2.5.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of catalysts for preparing rare earth rubber, including a functionalized alkyl aluminum compound, a configured functionalized rare earth catalyst composition and application thereof in the preparation of double-end functionalized rubber. Background Art

[0002] Rare earth rubber is a high cis-polydiolefin produced with rare earth compounds as catalysts. It has excellent flexural resistance, wear resistance and low rolling resistance, and has broad application prospects in the field of tire manufacturing. However, due to the difference in polarity, the compatibility between the rubber matrix and the reinforcing filler is poor, which becomes the main factor affecting its performance. Therefore, the development of end-group functionalized rare earth rubber is of great significance for the preparation of high-performance tires.

[0003] The rare earth rubber polymer chain is divided into an initiating end and a terminating end. The quasi-active coordination chain transfer active polymerization is used for end-capping reaction, and the terminating end functionalized rare earth rubber can be conveniently prepared. For example: the Visseaux group used benzophenone to end-cap the rare earth neodymium catalyzed isoprene system to obtain a stereoregular polymer with terminal hydroxyl groups (Macromolecules 2019, 52, 1210–1219); the Mecking group used tetraethyl orthosilicate to end-cap the rare earth neodymium catalyzed isoprene polymerization system to obtain a stereoregular rubber with terminal siloxy groups (Macromolecules 2018, 51, 763–770). However, this type of method has disadvantages such as low reaction end-capping efficiency and high residual small molecule content, resulting in low mechanical properties of the rubber. The use of a functionalized initiator system can conveniently prepare an initiator end functionalized rare earth rubber. For example, Mecking's research group used functionalized alkyl aluminum compounds in a rare earth neodymium metal catalytic system to prepare a series of cis-butadiene rubbers with amine groups at the end, but the preparation method of such functionalized alkyl aluminum is cumbersome and expensive. This type of method has the characteristics of high activity, that is, the functionalized initiator can be efficiently introduced into the polymer chain end through the method of functionalized initiator. However, this type of method requires the preparation of expensive and difficult to prepare functionalized initiators.

[0004] Based on the above background, in order to prepare high-performance double-end functionalized rare earth rubber and solve the problem of poor compatibility of non-traditional rubber with polar fillers during use, the present invention provides an amine-functionalized rare earth catalyst composition prepared based on functionalized alkyl aluminum, which can efficiently initiate (co)polymerization of butadiene and isoprene, and combined with a capping system, can prepare a double-end functionalized rare earth rubber having polar groups at both the initiating end and the terminating end. Summary of the invention

[0005] The problem to be solved by the present invention is to overcome the defect of poor compatibility between rare earth rubber and reinforcing filler, and to provide an efficient preparation method of end-group functionalized rare earth rubber based on a novel amine-functionalized rare earth catalyst composition. This method is different from the traditional end-capping method, and can efficiently introduce amine functional groups into the initiating end of the rubber molecular chain, and the product has the characteristics of uniform structure and no small molecule additive residue. Introducing amine groups into the rubber chain ends helps to achieve nano-dispersion of fillers in the rubber matrix. At the same time, the groups at the ends of the rubber molecular chains and the oxygen-containing functional groups on the surface of the reinforcing fillers will form hydrogen bonds or ionic bonds and other interactions during the processing process, which, on the one hand, improves the dispersibility of the filler and enhances the interface strength, and on the other hand, will also passivate the mobility of the rubber molecular chain ends, thereby reducing the energy consumption and rolling resistance during the deformation process of the rare earth butyl-pentene rubber.

[0006] The present invention provides a functionalized alkyl aluminum compound. The alkyl aluminum compound is an alkyl aluminum compound with an amino polar group, and its structure is AlR1(R2)2, wherein R1 is selected from one of the following I-XII structural formulas, wherein R′ is an alkyl group, selected from n-butyl, sec-butyl, tert-butyl, preferably n-butyl; x is 1-20, preferably 1-10; m is 5-20, preferably 5-10; n is in the range of 5-20, preferably 5-10; and R2 is selected from one of ethyl, isobutyl, n-butyl and octyl structures.

[0007]

[0008] The functionalized alkyl aluminum compound is prepared by an anionic polymerization method;

[0009] When R1 in AlR1(R2)2 is structural formula I-VI, the preparation method thereof is as follows:

[0010] The specific synthesis method is as follows:

[0011] (1) 1-(4-dimethylaminophenyl)-1'-phenylethylene or bis-1,1'-(4-dimethylaminophenyl)ethylene is dissolved in a non-polar solvent, wherein the concentration of the solute (1-(4-dimethylaminophenyl)-1'-phenylethylene or bis-1,1'-(4-dimethylaminophenyl)ethylene) is 5-30 g / L, preferably 10-20 g / L, and the non-polar solvent is n-hexane, hexane, toluene, benzene, preferably cyclohexane. Alkyl lithium is added to the obtained solution, and 1-(4-dimethylaminophenyl)-1'-phenylethylene or bis-1,1'-(4-dimethylaminophenyl)ethylene is reacted with the alkyl lithium at 0-50 degrees Celsius for 10-120 minutes, preferably at 50 degrees Celsius for 30 minutes, wherein the alkyl lithium can be n-butyl lithium, sec-butyl lithium, tert-butyl lithium, preferably sec-butyl lithium; the feeding molar ratio of 1-(4-dimethylaminophenyl)-1'-phenylethylene or bis-1,1'-(4-dimethylaminophenyl)ethylene to the alkyl lithium is in the range of 1-20:1, preferably 1-5:1.

[0012] (2) Adding a diene monomer to the solution obtained in step (1) and reacting the mixture at 0-50 degrees Celsius for 10-120 minutes, preferably at 50 degrees Celsius for 60 minutes; the diene monomer is selected from one or both of butadiene and isoprene, and the molar ratio of the diene monomer to the alkyl lithium is in the range of 10-40:1, preferably 10-20:1.

[0013] (3) Then, the solution obtained in step (2) is mixed with an alkyl aluminum chloride compound, and reacted at 0-50 degrees Celsius for 0-30 minutes, preferably at 50 degrees Celsius for 10 minutes. The alkyl aluminum chloride compound is selected from diethyl aluminum chloride, diisobutyl aluminum chloride, aluminum sesquichloride, dioctyl aluminum chloride, preferably diisobutyl aluminum chloride. The molar ratio of the added alkyl aluminum chloride compound to the alkyl lithium is 1.00-1.20:1 based on the chlorine content. The prepared functionalized alkyl aluminum compound is directly used in the preparation of the functionalized rare earth catalyst composition.

[0014] When R1 in AlR1(R2)2 is structural formula VII-IX, the preparation method thereof is as follows:

[0015]

[0016] The specific synthesis method is as follows:

[0017] (1) 4-dimethylaminostyrene and diene monomers are dissolved in a non-polar solvent, the molar ratio of 4-dimethylaminostyrene to diene monomer is in the range of 1:5-20, preferably 1:10, the concentration of solute 4-dimethylaminostyrene and diene monomer is 5-30 g / L, preferably 10-20 g / L, the non-polar solvent is n-hexane, hexane, toluene, benzene, preferably cyclohexane, and then alkyl lithium is added to the obtained solution, 4-dimethylaminostyrene and diene monomer react with alkyl lithium at 0-50 degrees Celsius for 60-240 minutes, preferably at 50 degrees Celsius for 120 minutes, the alkyl lithium can be n-butyl lithium, sec-butyl lithium, tert-butyl lithium, preferably sec-butyl lithium. The molar ratio of 4-dimethylaminostyrene to alkyl lithium is in the range of 1-20:1, preferably 1-5:1. The diene monomer is selected from one or both of butadiene and isoprene, and the molar ratio of the diene monomer to the alkyl lithium is in the range of 10-40:1, preferably 10-20:1.

[0018] (2) Then, the solution obtained in step (1) is mixed with an alkyl aluminum chloride compound, and reacted at 0-50 degrees Celsius for 0-30 minutes, preferably at 50 degrees Celsius for 10 minutes. The alkyl aluminum chloride compound is selected from diethyl aluminum chloride, diisobutyl aluminum chloride, aluminum sesquichloride, dioctyl aluminum chloride, preferably diisobutyl aluminum chloride. The molar ratio of the added alkyl aluminum chloride compound to the alkyl lithium is 1.00-1.20:1 based on the chlorine content. The prepared functionalized alkyl aluminum compound is directly used in the preparation of the functionalized rare earth catalyst composition.

[0019] When R1 in AlR1(R2)2 is structural formula X-XII, the preparation method thereof is as follows:

[0020]

[0021] The specific synthesis method is as follows:

[0022] (1) dissolving hexamethyleneimine in a non-polar solvent, wherein the concentration of the solute hexamethyleneimine is 5-30 g / L, preferably 10-20 g / L, and the non-polar solvent is n-hexane, hexane, toluene, benzene, preferably cyclohexane, and adding alkyl lithium to the obtained solution, wherein the molar ratio of hexamethyleneimine to alkyl lithium is in the range of 1-1.05:1, preferably 1.05:1, and the hexamethyleneimine and alkyl lithium are reacted at 0-50 degrees Celsius for 10-120 minutes, preferably at 25 degrees Celsius for 30 minutes, wherein the alkyl lithium can be n-butyl lithium, sec-butyl lithium, tert-butyl lithium, preferably n-butyl lithium.

[0023] (2) Subsequently, a diene monomer is added to the solution obtained in step (1) and reacted at 0-50 degrees Celsius for 10-120 minutes, preferably at 50 degrees Celsius for 60 minutes. The diene monomer is selected from one or both of butadiene and isoprene, and the molar ratio of the diene monomer to the alkyl lithium is in the range of 1-40:1, preferably 10-20:1.

[0024] (3) Then, the solution obtained in step (2) is mixed with an alkyl aluminum chloride compound, and reacted at 0-50 degrees Celsius for 0-30 minutes, preferably at 50 degrees Celsius for 10 minutes. The alkyl aluminum chloride compound is selected from diethyl aluminum chloride, diisobutyl aluminum chloride, aluminum sesquichloride, dioctyl aluminum chloride, preferably diisobutyl aluminum chloride. The molar ratio of the added alkyl aluminum chloride compound to the alkyl lithium is 1.00-1.20:1 based on the chlorine content. The prepared functionalized alkyl aluminum compound is directly used in the preparation of the functionalized rare earth catalyst composition.

[0025] The present invention also provides a functionalized rare earth catalyst composition, which is composed of a rare earth metal compound, a functionalized alkyl aluminum compound and a chlorine source in a molar ratio of 1: (10-30): (0-5), preferably 1: (10-15): (0-3), wherein the functionalized alkyl aluminum compound in the functionalized rare earth catalyst composition is the alkyl aluminum compound with an amino functionalized group prepared as described above. The rare earth metal element in the rare earth metal compound is neodymium, specifically neodymium neodecanoate, neodymium cyclohexaneate, isopropoxy neodymium, preferably neodymium neodecanoate. The chlorine source is selected from dichlorodimethylsilane, silicon tetrachloride, tert-butyl chloride, diisobutylaluminum chloride, diethylaluminum chloride, ethylaluminum dichloride and ethylaluminum sesquichloride, preferably diethylaluminum chloride.

[0026] The present invention also provides a method for preparing a functionalized rare earth catalyst composition, which comprises: contacting a functionalized alkyl aluminum compound, a chlorine source and a rare earth compound in a non-polar solvent under the protection of an inert gas.

[0027] The mixing order of the three components of the rare earth compound, the functionalized alkyl aluminum compound and the chlorine source is one of the following: (1) the functionalized alkyl aluminum compound is contacted with the chlorine source and then with the rare earth compound; (2) the chlorine source, the functionalized alkyl aluminum compound and the rare earth compound are contacted in sequence; (3) the rare earth compound, the functionalized alkyl aluminum compound and the chlorine source are contacted in sequence.

[0028] The inert gas is nitrogen or argon, preferably high-purity nitrogen or high-purity argon, and more preferably high-purity argon; the non-polar solvent includes: hexane, cyclohexane, raffinate, toluene, benzene, preferably cyclohexane and hexane; the concentration of rare earth elements in the functionalized rare earth catalyst composition ranges from 5 to 30 mmol / L, preferably 10 to 20 mmol / L; the contact conditions include: temperature of 0 to 50 degrees Celsius, preferably 50 degrees Celsius, and time of 0 to 360 minutes, preferably 0 to 60 minutes.

[0029] The present invention also provides a polymerization method for double-end functionalized rare earth rubber, which comprises: contacting a conjugated diene with a functionalized rare earth catalyst composition in a non-polar solvent, adding a capping agent after polymerization for a certain period of time, contacting the capping agent with the synthesized polymerized rubber solution, and terminating the reaction, wherein the functionalized rare earth catalyst composition is any one of the functionalized rare earth catalyst compositions prepared above; wherein the conjugated diene is selected from one or two of butadiene and isoprene, and the molar ratio of the conjugated diene to the functionalized rare earth catalyst composition calculated as rare earth metal element is 1000-20000:1, preferably 5000-15000; the non-polar solvent comprises: hexane, cyclohexane, raffinate, toluene, benzene, preferably cyclohexane and hexane. wherein the conditions of the polymerization reaction comprise: a temperature of 0 to 60 degrees Celsius, preferably 60 degrees Celsius, and a time of 1 to 5 hours, preferably 2 to 4 hours.

[0030] The end-capping agent mentioned in the above-mentioned polymerization method of double-end functionalized rare earth rubber can be selected from any one of the following:

[0031] Benzophenone derivatives, including benzophenone, 4-(dimethylamino)benzophenone, 4-(diethylamino)benzophenone, 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone;

[0032] Isocyanate derivatives, including cyclohexyl isocyanate, octadecyl isocyanate, p-toluene isocyanate, tert-butyl isocyanate, and dodecyl isocyanate;

[0033] Oxygen-containing compounds, including hydrogen peroxide and oxygen.

[0034] Beneficial effects of the present invention:

[0035] The functionalized alkyl aluminum compound disclosed in the present invention has an amine functionalized group and is controllably prepared based on a living anionic polymerization method. The method is simple, flexible and efficient. The prepared functionalized alkyl aluminum has the characteristics of high reaction activity, strong controllability, etc. Functionalized alkyl aluminums of different structures can be prepared to meet catalyst configuration requirements. The functionalized alkyl aluminum compound disclosed in the present invention is a compound having an amine functionalized group. The functionalized alkyl aluminum compound can be prepared into a functionalized homogeneous catalyst after contacting with a rare earth compound and a chlorine source. The catalytic system can efficiently catalyze the polymerization of conjugated olefins to obtain a narrow distribution stereoregular rubber with functionalized initiator end groups. The functionalization efficiency can reach 95%, the stereoregularity of cis-dienes can reach 96%, the molecular weight distribution is lower than 2.5, and the amine group has little effect on the activity of the catalytic system in the rare earth catalytic initiation system. The end-group functionalized rare earth cis-butadiene rubber solves (1) the problem of poor compatibility between the rubber matrix and the polar filler, and greatly improves the mechanical properties of the rubber; and (2) the problem of free movement of the rubber end, and greatly reduces the hysteresis loss of the rubber during use. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 . The NMR spectrum of the amine-functionalized alkyl aluminum obtained in Example 1;

[0037] Figure 2 . Gel permeation chromatogram of the amine-functionalized alkyl aluminum obtained in Example 1;

[0038] Figure 3 . NMR spectrum of the sample obtained in Example 9 (initiator end functionalization);

[0039] Figure 4 . NMR spectrum of the sample obtained in Example 10 (initiator end / terminator end functionalization);

[0040] Figure 5 . NMR spectrum of the sample obtained in Example 11 (initiator / terminator functionalization);

[0041] Figure 6 .NMR spectrum of the sample obtained in Example 12 (initiation end / termination end functionalization). DETAILED DESCRIPTION

[0042] The present invention provides the following examples as further explanations, but they are not intended to limit the scope of protection of the present invention. The molecular weight and molecular weight distribution index (ratio of weight average molecular weight to number average molecular weight) of the polymer were determined by gel permeation chromatography (SEC), and the cis-trans isomer content in the polymer was determined by Fourier transform infrared spectroscopy. The ampoules mentioned in the examples were all baked at high temperature and vacuum dried before use, and all operations in the examples were carried out under the protection of high-purity argon (99.999%).

[0043] Examples 1-8 are preparations of amine-functionalized alkyl aluminum compounds

[0044] Example 1

[0045] 1-(4-dimethylaminophenyl)-1'-phenylethylene (0.23 g) and 9 mL of dry cyclohexane were added to a 20 mL ampoule, and then 0.9 mL of a hexane solution of sec-butyl lithium (1.13 M) was added. After reacting at 25 degrees Celsius for 30 minutes, 2 mL of isoprene was added, and then the reaction was carried out at 50 degrees Celsius for 4 hours. Then, a hexane solution of diisobutylaluminum monochloride (0.6 M, 1.7 mL) was added, and the reaction was carried out at room temperature for 30 minutes to obtain an amine-functionalized alkylaluminum reagent 1, whose structure was characterized by H NMR and gel permeation chromatography as shown in FIG. Figure 1 , 2 shown.

[0046] Example 2

[0047] To a 20 mL ampoule, 1-(4-dimethylaminophenyl)-1'-phenylethylene (0.27 g) and 9 mL of dry cyclohexane were added in sequence, followed by 0.9 mL of a hexane solution of sec-butyl lithium (1.13 M). After reacting at 50 °C for 30 minutes, 1 mL of isoprene was added, followed by reacting at 50 °C for 4 hours. Then, a hexane solution of diisobutylaluminum monochloride (0.6 M, 1.7 mL) was added, and the reaction was carried out at room temperature for 30 minutes to obtain an amine-functionalized alkylaluminum reagent 2.

[0048] Example 3

[0049] To a 20 mL ampoule, 4-dimethylaminostyrene (1.47 g) and a cyclohexane solution of butadiene (9 mL, butadiene concentration is 1.11 M) were added in sequence, and then 0.9 mL of a n-hexane solution of sec-butyl lithium (1.13 M) was added, and the mixture was reacted at 50 °C for 4 hours. Then, a hexane solution of diethylaluminum monochloride (1.0 M, 1.0 mL) was added, and the mixture was reacted at room temperature for 30 minutes to obtain an amino-functionalized alkylaluminum reagent 3.

[0050] Example 4

[0051] To a 20 mL ampoule, hexamethyleneimine (0.14 g) and 9 mL of dry cyclohexane were added in sequence, and then 0.9 mL of a hexane solution of sec-butyl lithium (1.13 M) was added, and the mixture was reacted at room temperature for 2 hours. Then, 2 mL of a mixed solution of butadiene and isoprene (0.27 g of butadiene, 0.34 g of isoprene, and the solvent was cyclohexane) was added, and the mixture was reacted at 50° C. for 4 hours. Then, a hexane solution of diethylaluminum monochloride (1.0 M, 1.0 mL) was added, and the mixture was reacted at room temperature for 30 minutes to obtain an amine-functionalized alkylaluminum reagent 4.

[0052] Example 5

[0053] To a 20 mL ampoule, 1,1'-(4-dimethylaminophenyl)ethylene (0.27 g) and 9 mL of dry cyclohexane were added in sequence, followed by 0.67 mL of n-butyllithium in n-hexane solution (1.60 M). After reacting at 0 °C for 120 min, 2 mL of isoprene was added, followed by reacting at 0 °C for 2 h. Then, a hexane solution of diisobutylaluminum monochloride (0.6 M, 1.7 mL) was added, and the reaction was carried out at room temperature for 0 min to obtain the amino-functionalized alkylaluminum reagent 5.

[0054] Example 6

[0055] To a 20 mL ampoule, 1,1'-(4-dimethylaminophenyl)ethylene (0.27 g) and 9 mL of dry cyclohexane were added in sequence, followed by the addition of 0.67 mL of n-butyllithium in n-hexane solution (1.60 M). After reacting at 50 °C for 10 minutes, 2 mL of a mixed solution of butadiene and isoprene (0.27 g of butadiene, 0.34 g of isoprene, and the solvent was cyclohexane) was added, followed by reacting at 50 °C for 2 hours, followed by the addition of a hexane solution of dioctylaluminum monochloride (0.6 M, 1.7 mL), and the reaction was carried out at room temperature for 30 minutes to obtain an amine-functionalized alkylaluminum reagent 6.

[0056] Example 7

[0057] To a 20 mL ampoule, 4-dimethylaminostyrene (1.47 g) and a cyclohexane solution of isoprene (9 mL, isoprene concentration is 1.40 M) were added in sequence, and then 0.9 mL of a hexane solution of n-butyl lithium (1.60 M) was added, and the mixture was reacted at 50 °C for 4 hours. Then, a hexane solution of diethylaluminum monochloride (1.0 M, 1.0 mL) was added, and the mixture was reacted at room temperature for 30 minutes to obtain an amino-functionalized alkylaluminum reagent 7.

[0058] Example 8

[0059] To a 20 mL ampoule, hexamethyleneimine (0.14 g) and 9 mL of dry cyclohexane were added in sequence, and then 0.9 mL of sec-butyllithium in n-hexane solution (1.13 M) was added, and the mixture was reacted at room temperature for 2 hours. Then, isoprene in cyclohexane solution (9 mL, isoprene concentration was 1.40 M) was added, and the mixture was reacted at 50°C for 4 hours. Then, diethylaluminum monochloride in hexane solution (1.0 M, 1.0 mL) was added, and the mixture was reacted at room temperature for 30 minutes to obtain amino-functionalized alkylaluminum reagent 8.

[0060] Examples 9 to 25 are preparations of rare earth catalyst compositions based on amine-functionalized alkylaluminum 1-8 and their use in diene polymerization

[0061] Example 9

[0062] 0.2 mL of diisobutylaluminum chloride hexane solution (0.05 M) was added to 1.3 mL of amine functionalized alkylaluminum reagent 1 (0.08 M), and 0.05 mL of neodymium neodecanoate hexane solution (0.1 M) was added after preheating at 50° C. for 10 minutes, and kept for 30 minutes. 1.0 mL of isoprene was immediately added, and the polymerization was terminated by adding anhydrous ethanol after 2.5 hours at 50° C. The molecular weight of the obtained polymer was 11.5 kg / mol and the molecular weight distribution was 1.1 by gel permeation chromatography. The cis content was 87.0% by nuclear magnetic carbon spectrum. The efficiency of terminal amine functionalization (initiator end) was 95.0% by nuclear magnetic hydrogen spectrum.

[0063] Example 10

[0064] 0.3 mL of diisobutylaluminum chloride hexane solution (0.05 M) was added to 1.9 mL of amino-functionalized alkylaluminum reagent 1 (0.08 M), and 0.05 mL of neodymium neodecanoate hexane solution (0.1 M) was added after preheating at 50 ° C for 10 minutes, and kept for 30 minutes. 2.5 mL of isoprene was immediately added, and the polymerization was carried out at 50 ° C for 3.5 hours, and then 2.0 g of dodecyl isocyanate was added to terminate. The molecular weight of the obtained polymer was 7.8 kg / mol and the molecular weight distribution was 1.04 by gel permeation chromatography. The cis content was 90.7% by nuclear magnetic carbon spectrum. According to nuclear magnetic hydrogen spectrum, the initiation end functionalization efficiency was 95.0%, and the termination end functionalization efficiency was 91%.

[0065] Embodiment 11

[0066] To 0.9 mL of amino-functionalized alkylaluminum reagent 1 (0.08 M), 0.1 mL of diisobutylaluminum chloride hexane solution (0.05 M) was added, and after preheating at 50 ° C for 10 minutes, 0.05 mL of neodymium neodecanoate hexane solution (0.1 M) was added and maintained for 120 minutes. 3.4 g of isoprene was immediately added, and the polymerization was carried out at 50 ° C for 1.5 hours, and then 1.0 g of 4-dimethylaminobenzophenone was added. The molecular weight of the obtained polymer was 12.4 kg / mol and the molecular weight distribution was 1.20 according to gel permeation chromatography. The cis content was 94.7% according to nuclear magnetic carbon spectrum. According to nuclear magnetic hydrogen spectrum, the initiation end functionalization efficiency was 91.0%, and the termination end functionalization efficiency was 82.0%

[0067] Example 12

[0068] 0.6 mL of amino-functionalized alkylaluminum reagent 1 (0.08 M) was preheated at 50°C for 10 minutes, and then 0.05 mL of neodymium neodecanoate hexane solution (0.1 M) was added and maintained for 60 minutes. 0.4 mL of isoprene was immediately added, and the polymerization was carried out at 50°C for 1.5 hours. 5 mL of hydrogen peroxide (30 wt.%) was first added, and then 5 ml of sodium hydroxide aqueous solution (10 wt.%) was added. The molecular weight of the obtained polymer was 6.3 kg / mol and the molecular weight distribution was 1.05 according to gel permeation chromatography. The cis content was 85.0% according to nuclear magnetic carbon spectrum. According to nuclear magnetic hydrogen spectrum, the initiator end functionalization efficiency was 95.0%, and the termination end functionalization efficiency was 82.0%

[0069] Embodiment 13

[0070] To 1.3 mL of amino-functionalized alkylaluminum reagent 1 (0.08 M), 0.4 mL of diisobutylaluminum chloride hexane solution (0.05 M) was added, and after preheating at 0 ° C for 10 minutes, 0.05 mL of neodymium neodecanoate hexane solution (0.1 M) was added and maintained for 180 minutes. Immediately thereafter, 1.4 g of isoprene and 40 mL of butadiene hexane solution (2.0 M) were added, and the polymerization was terminated by adding ethanol after 5.0 hours at 60 ° C. The molecular weight of the obtained polymer was 23.5 kg / mol and the molecular weight distribution was 1.30 by gel permeation chromatography. The cis content was 98.7% by nuclear magnetic carbon spectrum. According to nuclear magnetic hydrogen spectrum, the initiation end functionalization efficiency was 94.3%, and the termination end functionalization efficiency was 83.5%.

[0071] Embodiment 14

[0072] To 1.9 mL of amino-functionalized alkylaluminum reagent 2 (0.08 M), 0.2 mL of diethylaluminum chloride hexane solution (0.05 M) was added, and after preheating at 30 ° C for 10 minutes, 0.05 mL of neodymium neodecanoate hexane solution (0.1 M) was added and maintained for 240 minutes. Then 75 mL of butadiene hexane solution (2.0 M) was immediately added, and the polymerization was carried out at 30 ° C for 4.5 hours, and 2.0 g of dodecyl isocyanate was added to terminate. The molecular weight of the obtained polymer was 43.2 kg / mol and the molecular weight distribution was 1.40 by gel permeation chromatography. The cis content was 99.6% by nuclear magnetic carbon spectrum. According to nuclear magnetic hydrogen spectrum, the initiation end functionalization efficiency was 95.3%, and the termination end functionalization efficiency was 92.4%.

[0073] Embodiment 15

[0074] To 0.6 mL of amine-functionalized alkylaluminum reagent 3 (0.08 M), 0.15 mL of ethylaluminum sesquichloride hexane solution (0.05 M) was added, and after preheating at 30° C. for 10 minutes, 0.05 mL of neodymium neodecanoate hexane solution (0.1 M) was added and maintained for 300 minutes. Immediately thereafter, 1.0 g of isoprene and 30 mL of butadiene hexane solution (2.0 M) were added, and the polymerization was carried out at 0° C. for 1.0 hour, and then 1.0 g of 4-dimethylaminobenzophenone was added to terminate the polymerization. The molecular weight of the obtained polymer was 15.6 kg / mol and the molecular weight distribution was 1.21 according to gel permeation chromatography. The cis content was 98.5% according to nuclear magnetic carbon spectrum. According to nuclear magnetic hydrogen spectrum, the initiation end functionalization efficiency was 93.2%, and the termination end functionalization efficiency was 89.4%.

[0075] Example 16

[0076] 0.2 mL of diisobutylaluminum chloride hexane solution (0.05 M) was added to 0.9 mL of amino-functionalized alkylaluminum reagent 4 (0.08 M), and 0.05 mL of neodymium neodecanoate hexane solution (0.1 M) was added after preheating at 50° C. for 10 minutes, and the mixture was kept at this temperature for 360 minutes. 6.8 g of isoprene was then added immediately, and the polymerization was carried out at 30° C. for 0.5 hours, and then 5 mL of hydrogen peroxide (30 wt.%) was added, and then 5 ml of sodium hydroxide aqueous solution (10 wt.%) was added to terminate the polymerization. The molecular weight of the obtained polymer was 13.3 kg / mol and the molecular weight distribution was 1.20 according to gel permeation chromatography. The cis content was 97.5% according to nuclear magnetic carbon spectrum. According to nuclear magnetic hydrogen spectrum, the initiator end functionalization efficiency was 95.5%, and the termination end functionalization efficiency was 86.0%.

[0077] Embodiment 17

[0078] To 1.3 mL of amino-functionalized alkylaluminum reagent 1 (0.08 M), 0.1 mL of ethylaluminum dichloride hexane solution (0.05 M) was added, and after preheating at 50° C. for 10 minutes, 0.05 mL of neodymium neodecanoate hexane solution (0.1 M) was added. Immediately thereafter, 0.14 g of isoprene and 4 mL of butadiene hexane solution (2.0 M) were added, and polymerization was carried out at 50° C. for 2.5 hours, followed by addition of 2.5 g of dodecyl isocyanate for termination. The molecular weight of the obtained polymer was 11.7 kg / mol and the molecular weight distribution was 1.13 as characterized by gel permeation chromatography. The cis content was 85.6% as characterized by nuclear magnetic carbon spectrum. As characterized by nuclear magnetic hydrogen spectrum, the initiation end functionalization efficiency was 94.6% and the termination end functionalization efficiency was 90.7%.

[0079] Embodiment 18

[0080] To 1.3 mL of amino-functionalized alkylaluminum reagent 2 (0.08 M), 0.05 mL of dichlorodimethylsilane hexane solution (0.05 M) was added, and after preheating at 50 ° C for 10 minutes, 0.05 mL of neodymium neodecanoate hexane solution (0.1 M) was added, and the aging time was 30 minutes. Then 5 mL of butadiene hexane solution (2.0 M) was immediately added, and the polymerization was carried out at 50 ° C for 3.5 hours, and 1.5 g of 4,4'-bis (dimethylamino) benzophenone was added to terminate. The molecular weight of the obtained polymer was 12.4 kg / mol and the molecular weight distribution was 1.19 by gel permeation chromatography. The cis content was 88.7% by nuclear magnetic carbon spectrum. According to nuclear magnetic hydrogen spectrum characterization, the initiation end functionalization efficiency was 95.2%, and the termination end functionalization efficiency was 90.1%.

[0081] Embodiment 19

[0082] To 0.6 mL of amino-functionalized alkylaluminum reagent 3 (0.08 M), 0.025 mL of silicon tetrachloride hexane solution (0.05 M) was added, and after preheating at 50 ° C for 10 minutes, 0.05 mL of neodymium neodecanoate hexane solution (0.1 M) was added, and the aging time was 60 minutes. Then 1.0 mL of isoprene was added immediately, and the polymerization was carried out at 50 ° C for 1.5 hours, and then 5 mL of hydrogen peroxide (30 wt.%) was added, and then 5 ml of sodium hydroxide aqueous solution (10 wt.%) was added to terminate. The molecular weight of the obtained polymer was 10.8 kg / mol and the molecular weight distribution was 1.07 by gel permeation chromatography. The cis content was 84.30% by nuclear magnetic carbon spectrum. According to nuclear magnetic hydrogen spectrum, the initiator end functionalization efficiency was 93.5%, and the termination end functionalization efficiency was 89.5%.

[0083] Embodiment 20

[0084] To 0.9 mL of amino-functionalized alkylaluminum reagent 4 (0.08 M), 0.4 mL of tert-butyl chloride hexane solution (0.05 M) was added, and after preheating at 50 ° C for 10 minutes, 0.05 mL of neodymium neodecanoate hexane solution (0.1 M) was added, and the aging time was 60 minutes. 1.0 mL of isoprene was immediately added, and the polymerization was carried out at 50 ° C for 1.5 hours, and then 1.0 g of dodecyl isocyanate was added to terminate. The molecular weight of the obtained polymer was 9.6 kg / mol and the molecular weight distribution was 1.16 by gel permeation chromatography. The cis content was 82.40% by nuclear magnetic carbon spectrum. According to nuclear magnetic hydrogen spectrum characterization, the initiation end functionalization efficiency was 95.8%, and the termination end functionalization efficiency was 88.6%.

[0085] Embodiment 21

[0086] 0.1 mL of ethylaluminum dichloride (0.05 M) was added to 1.3 mL of a hexane solution (0.08 M) of an amino-functionalized alkylaluminum reagent 5, and after preheating at 0°C for 10 minutes, 0.05 mL of a hexane solution (0.1 M) of neodymium neodecanoate was added, and after keeping at 0°C for 360 minutes, 0.14 g of isoprene and 4 mL of a hexane solution (2.0 M) of butadiene were added, and polymerization was carried out at 0°C for 5 hours, and then 2.5 g of dodecyl isocyanate was added to terminate the polymerization. The molecular weight of the obtained polymer was 12.8 kg / mol and the molecular weight distribution was 1.32 according to gel permeation chromatography, and the cis content was 87.2% according to nuclear magnetic carbon spectrum. According to nuclear magnetic hydrogen spectrum, the initiation end functionalization efficiency was 95.4%, and the termination end functionalization efficiency was 92.3%.

[0087] Embodiment 22

[0088] 0.05 mL of neodymium neodecanoate hexane solution (0.1 M) was added to 1.3 mL of amino-functionalized alkylaluminum reagent 6 (0.08 M), and 0.05 mL of dichlorodimethylsilane hexane solution (0.05 M) was added after preheating at 25°C for 10 minutes. After keeping at 25°C for 180 minutes, 5 mL of butadiene hexane solution (2.0 M) was added. The polymerization was carried out at 50°C for 3.5 hours and then 1.5 g of 4,4'-bis(dimethylamino)benzophenone was added to terminate the polymerization. The molecular weight of the obtained polymer was 11.4 kg / mol and the molecular weight distribution was 1.29 according to gel permeation chromatography. The cis content was 90.6% according to nuclear magnetic carbon spectrum. According to nuclear magnetic hydrogen spectrum, the initiation end functionalization efficiency was 94.2% and the termination end functionalization efficiency was 85.4%.

[0089] Embodiment 23

[0090] 0.025 mL of a hexane solution of silicon tetrachloride (0.05 M) was added to 0.6 mL of an amino-functionalized alkylaluminum reagent 7 (0.08 M), and after preheating at 50° C. for 10 minutes, 0.05 mL of a hexane solution of neodymium neodecanoate (0.1 M) was added, and the aging time was 60 minutes. 1.0 mL of isoprene was then immediately added, and the polymerization was carried out at 50° C. for 1.5 hours, and then 5 mL of hydrogen peroxide (30 wt.%) was added, and then 5 ml of a sodium hydroxide aqueous solution (10 wt.%) was added to terminate. The molecular weight of the obtained polymer was 9.7 kg / mol and the molecular weight distribution was 1.34 by gel permeation chromatography. The cis content was 85.8% by nuclear magnetic carbon spectrum. According to nuclear magnetic hydrogen spectrum, the initiator end functionalization efficiency was 95.4%, and the termination end functionalization efficiency was 83.2%.

[0091] Embodiment 24

[0092] To 0.9 mL of amino-functionalized alkylaluminum reagent 8 (0.08 M), 0.4 mL of hexane solution of tert-butyl chloride (0.05 M) was added, and after preheating at 50 ° C for 10 minutes, 0.05 mL of hexane solution of neodymium neodecanoate (0.1 M) was added, and the aging time was 60 minutes. 1.0 mL of isoprene was immediately added, and the polymerization was carried out at 50 ° C for 1.5 hours, and then 1.0 g of dodecyl isocyanate was added to terminate. The molecular weight of the obtained polymer was 10.3 kg / mol and the molecular weight distribution was 1.25 by gel permeation chromatography. The cis content was 83.5% by nuclear magnetic carbon spectrum. According to nuclear magnetic hydrogen spectrum characterization, the initiation end functionalization efficiency was 94.0%, and the termination end functionalization efficiency was 81.3%.

[0093] Embodiment 25

[0094] To 0.6 mL of amino-functionalized alkylaluminum reagent 3 (0.08 M), 0.025 mL of silicon tetrachloride hexane solution (0.05 M) was added, and after preheating at 50 ° C for 10 minutes, 0.05 mL of neodymium neodecanoate hexane solution (0.1 M) was added, and the aging time was 60 minutes. 1.0 mL of isoprene was immediately added, and the polymerization was carried out at 50 ° C for 1.5 hours. Dry oxygen was introduced (2 ml / min, 5 minutes). The molecular weight of the obtained polymer was 9.70 kg / mol and the molecular weight distribution was 1.36 by gel permeation chromatography. The cis content was 86.5% by nuclear magnetic carbon spectrum. According to nuclear magnetic hydrogen spectrum, the initiator end functionalization efficiency was 95.2%, and the termination end functionalization efficiency was 85.2%.

Claims

1. A functionalized alkyl aluminum compound, characterized in that Its structure is AlR1(R2)2, wherein R1 is selected from one of the following structural formulas I-XII, wherein R′ is an alkyl group selected from n-butyl, sec-butyl, tert-butyl, x is 1-20, m is 5-20, and n is 5-20; R2 is selected from one of ethyl, isobutyl, n-butyl and octyl; 2. The method for preparing the functionalized alkyl aluminum compound according to claim 1, characterized in that: When R1 in AlR1(R2)2 is a structural formula I-VI, the preparation method of the functionalized alkyl aluminum compound comprises the following steps: (1) dissolving 1-(4-dimethylaminophenyl)-1'-phenylethylene or bis-1,1'-(4-dimethylaminophenyl)ethylene in a non-polar solvent, adding alkyl lithium to the resulting solution, and reacting at 0-50 degrees Celsius for 10-120 minutes; (2) adding diene monomer to the solution obtained in step (1) and reacting at 0-50 degrees Celsius for 10-120 minutes; (3) mixing the solution obtained in step (2) with an alkylaluminum chloride compound, and reacting at 0-50 degrees Celsius for 0-30 minutes to obtain a functionalized alkylaluminum compound; When R1 in AlR1(R2)2 is structural formula VII-IX, the preparation method of the functionalized alkyl aluminum compound comprises the following steps: (1) dissolving 4-dimethylaminostyrene and diene monomer in a non-polar solvent, and then adding alkyl lithium to the resulting solution, and reacting at 0-50 degrees Celsius for 60-240 minutes; (2) mixing the solution obtained in step (1) with an alkyl aluminum chloride compound, reacting at 0-50 degrees Celsius for 0-30 minutes to obtain a functionalized alkyl aluminum compound; When R1 in AlR1(R2)2 is a structural formula X-XII, the preparation method of the functionalized alkyl aluminum compound comprises the following steps: (1) dissolving hexamethyleneimine in a non-polar solvent, adding alkyl lithium to the resulting solution, and reacting at 0-50 degrees Celsius for 10-120 minutes; (2) adding diene monomer to the solution obtained in step (1) and reacting at 0-50 degrees Celsius for 10-120 minutes; (3) Mixing the solution obtained in step (2) with an alkylaluminum chloride compound, reacting at 0-50 degrees Celsius for 0-30 minutes to obtain a functionalized alkylaluminum compound.

3. The method for preparing a functionalized alkyl aluminum compound according to claim 2, characterized in that: When R1 in AlR1(R2)2 is a structural formula I-VI, the concentration of the solute (1-(4-dimethylaminophenyl)-1'-phenylethylene or bis-1,1'-(4-dimethylaminophenyl)ethylene) is 5-30 g / L, the non-polar solvent is selected from n-hexane, hexane, toluene, and benzene, the alkyl lithium is selected from n-butyl lithium, sec-butyl lithium, and tert-butyl lithium, and the molar ratio of 1-(4-dimethylaminophenyl)-1'-phenylethylene or bis-1,1'-(4-dimethylaminophenyl)ethylene to the alkyl lithium is 1-20:1; the diene monomer is selected from one or two of butadiene and isoprene, and the molar ratio of the diene monomer to the alkyl lithium is 10-40:1; the alkyl aluminum chloride compound is selected from diethyl aluminum monochloride, diisobutyl aluminum monochloride, aluminum sesquichloride, and dioctyl aluminum monochloride; and the molar ratio of the alkyl aluminum chloride compound to the alkyl lithium is 1.00-1.20:1 based on the chlorine content; When R1 in AlR1(R2)2 is a structural formula VII-IX, the molar ratio of 4-dimethylaminostyrene to diene monomer is 1:5-20, the concentration of solute 4-dimethylaminostyrene and diene monomer is 5-30 g / L, the non-polar solvent is selected from n-hexane, hexane, toluene, benzene, the alkyl lithium is selected from n-butyl lithium, sec-butyl lithium, tert-butyl lithium, the molar ratio of 4-dimethylaminostyrene to alkyl lithium is 1-20:1, the diene monomer is selected from one or two of butadiene and isoprene, and the molar ratio of diene monomer to alkyl lithium is 10-40:1; the alkyl aluminum chloride compound is selected from diethyl aluminum monochloride, diisobutyl aluminum monochloride, aluminum sesquichloride, dioctyl aluminum monochloride; and based on the chlorine content, the molar ratio of the added alkyl aluminum chloride compound to the alkyl lithium is 1.00-1.20:

1. When R1 in AlR1(R2)2 is structural formula X-XII, the concentration of solute hexamethyleneimine is 5-30g / L, the non-polar solvent is selected from n-hexane, hexane, toluene, benzene, the molar ratio of hexamethyleneimine to alkyl lithium is 1-1.05:1, and the alkyl lithium is selected from n-butyl lithium, sec-butyl lithium, and tert-butyl lithium; the diene monomer is selected from one or two of butadiene and isoprene, and the molar ratio of the diene monomer to the alkyl lithium is 1-40:1; the alkyl aluminum chloride compound is selected from diethyl aluminum monochloride, diisobutyl aluminum monochloride, sesquialuminum, and dioctyl aluminum monochloride; and based on the chlorine content, the molar ratio of the added alkyl aluminum chloride compound to the alkyl lithium is 1.00-1.20:

1.

4. A functionalized rare earth catalyst composition, characterized in that: It consists of a rare earth metal compound, a functionalized alkyl aluminum and a chlorine source in a molar ratio of 1:(10-30):(0-5.0); the functionalized alkyl aluminum is the functionalized alkyl aluminum compound described in claim 1.

5. The composition according to claim 4, characterized in that The rare earth metal element in the rare earth metal compound is neodymium, and the rare earth metal compound is selected from neodymium neodecanoate, neodymium naphthenate, and neodymium isopropoxide; The chlorine source is selected from dichlorodimethylsilane, silicon tetrachloride, tert-butyl chloride, diisobutylaluminum chloride, diethylaluminum chloride, ethylaluminum dichloride and ethylaluminum sesquichloride.

6. The method for preparing the functionalized rare earth catalyst composition according to any one of claims 4 to 5, characterized in that: The method comprises: under the protection of an inert gas, contacting a rare earth compound, a functionalized alkyl aluminum compound and a chlorine source in a non-polar solvent, wherein the contact sequence is one of the following: (1) contacting the functionalized alkyl aluminum compound with a chlorine source and then with the rare earth compound; (2) contacting the chlorine source, the functionalized alkyl aluminum compound and the rare earth compound in sequence; (3) contacting the rare earth compound, the functionalized alkyl aluminum compound and the chlorine source in sequence; wherein the concentration of the rare earth element in the functionalized rare earth catalyst composition is 5-30 mmol / L, and the contact conditions comprise: a temperature of 0-50 degrees Celsius and a time of 0-360 minutes.

7. A method for polymerizing a double-end functionalized conjugated diene, characterized in that: The method comprises: contacting a conjugated diene with a functionalized rare earth catalyst composition in a non-polar solvent, polymerizing for a certain period of time, and then adding a capping agent to terminate the reaction. The functionalized rare earth catalyst composition is the functionalized rare earth catalyst composition described in any one of claims 4-5.

8. The method according to claim 7, characterized in that The conjugated diene is selected from one or two of butadiene and isoprene; the molar ratio of the conjugated diene to the functionalized rare earth catalyst composition calculated as rare earth metal element is 1000-20000:1; the conditions of the polymerization reaction include: temperature of 0 degrees Celsius to 60 degrees Celsius, and time of 1-5 hours.

9. The method according to claim 7, characterized in that: The blocking agent is selected from one of benzophenone derivatives, isocyanate derivatives and oxygen-containing compounds.

10. The method according to claim 9, characterized in that The benzophenone derivatives include one or more of benzophenone, 4-(dimethylamino)benzophenone, 4-(diethylamino)benzophenone, 4,4'-bis(dimethylamino)benzophenone, and 4,4'-bis(diethylamino)benzophenone; The isocyanate derivatives include one or more of cyclohexyl isocyanate, octadecyl isocyanate, p-toluene isocyanate, tert-butyl isocyanate, and dodecyl isocyanate; The oxygen-containing compound includes one or more of hydrogen peroxide and oxygen.

Citation Information

Patent Citations

  • Rare earth catalyst composition and preparation method of rare earth catalyst

    CN101838350A

  • Catalyst for use in preparation of high cis-polyisoprene with narrow molecular weight distribution and preparation method and application thereof

    CN102585061A

  • Wide-distribution, high-elasticity and functionalized solution polymerized styrene-butadiene rubber, preparation method and application thereof in tire tread rubber

    CN111777729A

  • Hydrogenated amino functionalized styrene-butadiene rubber and preparation method thereof

    CN111892669A

  • Amino multifunctional SEBS thermoplastic elastomer and preparation method thereof

    CN112759730A