Salt-resistant emulsion polymer and preparation method thereof

By developing anti-salt emulsion polymers, using reverse-phase emulsion polymers and specific functional groups, the problem of low efficiency of existing anti-salt polymers in low permeability reservoirs has been solved, achieving efficient oil displacement and good resistance to Salt properties.

CN119019601APending Publication Date: 2024-11-26HEILONGJIANG LONGHUI CHEM CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411111060.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Most of the existing salt-resistant polymers are medium and high molecular weight and solids, which cannot meet the needs of low permeability reservoirs, and have low viscosity in high mineralization water, resulting in low oil displacement efficiency.

Method used

Develop an anti-salt emulsion polymer, prepared by reverse-phase emulsion polymerization reaction, with a molecular weight adjustable between 1 million and 10 million, containing -SO3-, -(CH2)n-CH3 long chain side groups and six-membered ring structures , improve the salt resistance and viscosity of the polymer.

Benefits of technology

The oil flooding recovery rate is significantly improved in low permeability reservoirs. The polymer is an emulsion, which has fast dissolution speed, convenient on-site application, and has good salt resistance and displacement performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019601A_ABST
    Figure CN119019601A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of oilfield chemistry, and discloses a salt-resistant emulsion polymer and a preparation method thereof, the molecular weight is adjustable between 1 million and 10 million, and the salt-resistant emulsion polymer is suitable for exploitation of second-class and third-class oil reservoirs with low permeability. Under the condition of oilfield sewage, the polymer has good salt resistance, the polymer flooding recovery efficiency can be well improved, and meanwhile, the polymer is emulsion, high in dissolution speed and convenient to apply on site. The invention provides a salt-resistant emulsion polymer, the salt-resistant emulsion polymer is prepared by inverse emulsion polymerization reaction of a water-phase material comprising a monomer A, a monomer B and a monomer C, the monomer A is a monomer with a structure as shown in a formula (a), the monomer B is a monomer with a structure as shown in a formula (b), and the monomer C is a monomer with a structure as shown in a formula (c).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of oilfield chemistry, in particular to a salt-resistant emulsion polymer and a preparation method thereof. Background Art

[0002] Chemical flooding is one of the most effective methods to improve crude oil recovery among many tertiary oil recovery technologies. Polymer flooding can increase crude oil recovery by more than 10% on the basis of water flooding. It is the most mature and widely used technology in chemical flooding. It is of great significance to increase crude oil production and ensure national energy security. Polyacrylamide is the most widely used polymer flooding agent in tertiary oil recovery in oil fields. At present, most domestic oil fields have entered the development stage of Class II and Class III reservoirs. In order to adapt to the characteristics of small pores and low permeability of such reservoirs, the demand for low molecular weight polymers for oil recovery in oil fields is increasing. Ordinary low molecular weight polymers have low viscosity in high-salinity water, and problems such as "fingering" and "sudden advance" are prone to occur during oil recovery, resulting in low displacement efficiency. Therefore, oil fields are in urgent need of low molecular weight salt-resistant polymers for oil recovery to improve the oil recovery efficiency of Class II and Class III reservoirs.

[0003] Many domestic scientific research institutions and enterprises have carried out research on salt-resistant polymers, but currently most of these salt-resistant polymers are medium molecular weight, high molecular weight and ultra-high molecular weight polymers, which are not suitable for low permeability reservoirs; and most of them are solid, and when used on-site in oil fields, they require more complex preparation equipment and processes. Due to the advantages of fast dissolution, simple preparation, and quick and convenient application of emulsion polymers, domestic research on emulsion polymers has continued to deepen in recent years. Although some emulsion polymers are currently used on-site in oil fields, they are all ordinary emulsion polymers with poor salt resistance and cannot meet the needs of oil fields. Summary of the invention

[0004] To achieve the above purpose, the present invention discloses a salt-resistant emulsion polymer and a preparation method thereof, which are achieved through the following technical scheme: a salt-resistant emulsion polymer, the molecular weight of which is adjustable between 1 million and 10 million, is suitable for the exploitation of Class II and Class III oil reservoirs with low permeability; and under oilfield sewage conditions, the polymer has good salt resistance and can better improve the polymer drive recovery rate. At the same time, the polymer is an emulsion, has a fast dissolution rate, and is easy to apply on site.

[0005] The present invention provides a salt-resistant emulsion polymer. The salt-resistant emulsion polymer is prepared by an inverse emulsion polymerization reaction of an aqueous phase material including a monomer A, a monomer B and a monomer C, wherein the monomer A is a monomer having a structure shown in formula (a), the monomer B is a monomer having a structure shown in formula (b), and the monomer C is a monomer having a structure shown in formula (c).

[0006] Wherein, R1, R2 and R3 are each independently selected from -H or C1-C4 alkyl; R4, R5 and R6 are each independently selected from -H or C1-C4 alkyl; X is selected from H+, K+, Na+ or NH4+; n is an integer of 7-15; R7, R8 and R9 are each independently selected from C1-C2 alkyl.

[0007] The molar ratio of monomer A, monomer B and monomer C is (15-50): (5-10): 1;

[0008] The viscosity average molecular weight of the polymer is 1 million to 10 million;

[0009] Preferably, the polymer is polymerized by monomer A, monomer B and monomer C in a certain ratio, and the monomer A forms the main skeleton of the polymer after polymerization. Preferably, in the monomer A shown in formula (a), R1, R2 and R3 are each independently selected from -H or a C1-C4 alkyl group.

[0010] Preferably, after the monomer B is polymerized with the monomer A and the monomer C, -SO3- side groups and -(CH2)n-CH3 long-chain side groups are formed in the polymer molecular chain structure. Specifically, the monomer B has a molecular structure shown in formula (b), R4, R5 and R6 are each independently selected from -H or C1-C4 alkyl, X is selected from H+, K+, Na+ or NH4+, and n is an integer of 5-15; the hydrophilicity and strong charge of the -SO3- group make the polymer have better water solubility and hydrolysis resistance; because the -(CH2)n-CH3 group has a longer flexible molecular chain structure, on the one hand, the rotation radius of the polymer molecular chain is increased, the friction and physical entanglement between molecules are enhanced, and the viscosity of the polymer is increased; on the other hand, the flexibility of the polymer molecular chain is increased. Since the greater the flexibility of the molecular chain, the more significant the viscoelasticity, therefore, the displacement performance of the polymer is improved.

[0011] Preferably, after the monomer C is polymerized with the monomer A and the monomer B, a six-membered ring structure side group is formed in the polymer molecular chain structure. Specifically, the monomer C has a molecular structure shown in formula (c), and R7, R8 and R9 are each independently selected from a C1-C2 alkyl group. Due to the rigid structure of the six-membered ring molecule, the salt resistance of the polymer is effectively improved, and at the same time, the linearity of the polymer molecular chain is improved, so that when the polymer solution is driven in the formation, the better linear molecular structure is easier to pass through the small-sized rock pores and roaring channels, so that the sweep efficiency of the polymer solution is effectively improved, and the recovery rate is improved.

[0012] The polymer contains functional groups such as -SO3- groups, -(CH2)n-CH3 long-chain side groups and hexacyclic groups. The viscoelasticity and rigidity of the polymer are enhanced, and the polymer has good salt resistance. The polymer is prepared into a polymer saline solution with a polymer concentration of 1500 mg / L and a mineralization of 2400-6000 mg / L. The apparent viscosity of the polymer saline solution at 45°C is 10-40 mPa·s.

[0013] The present invention also provides a method for preparing a salt-resistant emulsion polymer, comprising the following steps:

[0014] 1) Prepare aqueous phase materials

[0015] The aqueous phase material includes monomer A, monomer B, monomer C and water, wherein the mass ratio of monomer A, monomer B and monomer C is (60-80): (15-30): (5-10); the mass ratio of the solid matter contained in the above-mentioned mixed system to deionized water is 40-50%: 50-60%;

[0016] 2) Prepare oil phase materials

[0017] The oil phase material comprises an organic solvent, a first emulsifier and a second emulsifier, and the mass ratio of the organic solvent, the first emulsifier and the second emulsifier is 100:(1.5-3):(3-8);

[0018] 3) mixing and emulsifying the aqueous phase material obtained in step 1) and the oil phase material obtained in step 2) to obtain a monomer emulsion;

[0019] 4) introducing nitrogen into the monomer emulsion obtained in step 3) to deoxygenate, and performing a polymerization reaction in the presence of an initiator to obtain an emulsion polymer;

[0020] 5) adding sodium hydroxide to the emulsion polymer obtained in step 4), wherein the mass ratio of the emulsion polymer system to the sodium hydroxide is 100:(2-3); heating the emulsion system to 85-95° C. and keeping the temperature for 2-4 hours to obtain a salt-resistant emulsion polymer for oil displacement.

[0021] Preferably, in the method for preparing the polymer, the initiator can be a conventional initiator for free radical polymerization, such as a redox system initiator, a peroxide initiator, or an azo initiator. The mass ratio of the initiator to the monomer A is 1:(10-1000).

[0022] Preferably, the azo initiator can be selected from at least one of azobisisobutyronitrile, azobisisovaleronitrile, azobisisoheptanenitrile, dimethyl azobisisobutyrate, azobisisopropylimidazoline, azobisisobutylamidine hydrochloride, azobisisopropylimidazoline hydrochloride, azoisobutylcyanamide, azobiscyclohexylcarbonitrile and azobiscyanovaleric acid.

[0023] Preferably, the peroxide initiator can be selected from at least one of hydrogen peroxide, ammonium persulfate, sodium persulfate, potassium persulfate, benzoyl peroxide and tert-butyl benzoyl peroxide.

[0024] Preferably, the redox system initiator may be selected from at least one of sulfate-sulfite, persulfate-thiourea, persulfate-thiosulfate and ammonium persulfate-fatty amine.

[0025] Preferably, the polymerization reaction temperature is 20°C-50°C, the pH value is 4-11, and the reaction time is 1-24h.

[0026] Preferably, the organic solvent can be selected from at least one of white oil, kerosene, hexane, petroleum ether, acetone, toluene, dichloromethane and chloroform.

[0027] Preferably, the first emulsifier can be selected from at least one of Span20, Span60 and Span80, and the second emulsifier can be selected from at least one of fatty alcohol polyoxyethylene ether, alkylphenol polyoxyethylene polyoxypropylene ether, alkylamine polyoxyethylene ether, fatty amide polyoxyethylene ether, sorbitan fatty acid ester, glyceryl monostearate, glyceryl monolaurate and glyceryl monooleate.

[0028] The present invention provides a salt-resistant emulsion polymer and a preparation method thereof. The polymer has the following beneficial effects:

[0029] The salt-resistant emulsion polymer and its preparation method, on the one hand, increase the rotation radius of the polymer molecular chain, enhance the friction and physical entanglement between molecules, and improve the viscosity of the polymer; on the other hand, increase the flexibility of the polymer molecular chain. Since the greater the flexibility of the molecular chain, the more significant the viscoelasticity, the displacement performance of the polymer is improved, the polymer has good salt resistance, and can better improve the polymer flooding recovery rate. At the same time, the polymer is an emulsion, has a fast dissolution speed, and is convenient for on-site application. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 It is a schematic diagram of the molecular structure of the present invention;

[0031] Figure 2 This is a data table of viscosity test of the polymer of the present invention in salt water;

[0032] Figure 3 The evaluation result of the shear resistance of the 1500 mg / L salt-resistant emulsion polymer aqueous solution of the present invention (unit: mPa·s);

[0033] Figure 4 The time-viscosity relationship curve of the 1500 mg / L salt-resistant emulsion polymer aqueous solution of the present invention at different shear rates;

[0034] Figure 5 The evaluation result of the shear resistance of the 2000 mg / L salt-resistant emulsion polymer aqueous solution of the present invention (unit: mPa·s);

[0035] Figure 6 The time-concentration relationship curve of the 2000 mg / L salt-resistant emulsion polymer of the present invention at different shear rates;

[0036] Figure 7 This is the oil displacement data curve of the salt-resistant emulsion polymer KR1 of the present invention;

[0037] Figure 8 This is the 19 million HPAM oil displacement data curve of the present invention;

[0038] Fig. 9 This is a statistical table of oil displacement experiment results of the present invention. DETAILED DESCRIPTION

[0039] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0040] See also Figure 1-Figure 9 , Example 1: Preparation of a salt-resistant emulsion polymer:

[0041] Prepare the aqueous phase material: weigh 1000 kg of deionized water and add it into the reactor. Add 1000 kg of acrylamide while stirring until it is completely dissolved. Then add 120 kg of 2-acrylamidododecyl sodium sulfonate and 40 kg of 4-acryloylmorpholine.

[0042] Prepare oil phase materials: weigh 1000 kg of white oil and add it into the emulsifier, add 40 kg of Span 80 and 20 kg of oil ester strong emulsifier, and stir evenly;

[0043] Emulsification: Add all the oil phase materials into the water phase materials, stir and emulsify to form an emulsion;

[0044] Emulsion polymerization: add 0.8 kg of azobisisobutyronitrile as initiator; pass nitrogen through the material system for 35 minutes to remove dissolved oxygen in the water; add 20 g of sodium bisulfate and 25 g of ammonium persulfate to initiate the reaction, and keep warm for 4 hours;

[0045] Hydrolysis: 112 kg of solid sodium hydroxide was added to the reaction kettle under stirring, the temperature was raised to 90° C., and the temperature was kept for 2 h to obtain the salt-resistant emulsion polymer KR1 for oil displacement.

[0046] Example 2: Preparation of a salt-resistant emulsion polymer for oil displacement:

[0047] Prepare the aqueous phase material: weigh 1000 kg of deionized water and add it into the reactor. Add 1000 kg of acrylamide while stirring until it is completely dissolved. Then add 150 kg of 2-acrylamidododecyl sodium sulfonate and 40 kg of 4-acryloylmorpholine.

[0048] Prepare oil phase materials: weigh 1000 kg of white oil and add it into the emulsifier, add 40 kg of Span 80 and 20 kg of oil ester strong emulsifier, and stir evenly;

[0049] Emulsification: Add all the oil phase materials into the water phase materials, stir and emulsify to form an emulsion;

[0050] Emulsion polymerization: add 0.8 kg of azobisisobutyronitrile as initiator; pass nitrogen through the material system for 35 minutes to remove dissolved oxygen in the water; add 25 g of sodium bisulfate and 30 g of ammonium persulfate to initiate the reaction, and keep warm for 4 hours;

[0051] Hydrolysis: Add 112 kg of sodium hydroxide into the reactor, raise the temperature to 90°C, and keep it warm for 2 hours to obtain the salt-resistant emulsion polymer KR2 for oil displacement.

[0052] Example 3: Preparation of a salt-resistant emulsion polymer for oil displacement:

[0053] Prepare the aqueous phase material: weigh 1000 kg of deionized water and add it into the reactor. Add 1000 kg of acrylamide while stirring until it is completely dissolved. Then add 200 kg of 2-acrylamidododecyl sodium sulfonate and 40 kg of 4-acryloylmorpholine.

[0054] Prepare oil phase materials: weigh 1000 kg of white oil and add it into the emulsifier, add 40 kg of Span 80 and 20 kg of oil ester strong emulsifier, and stir evenly;

[0055] Emulsification: Add all the oil phase materials into the water phase materials, stir and emulsify to form an emulsion;

[0056] Emulsion polymerization: add 0.8 kg of azobisisobutyronitrile as initiator; pass nitrogen through the material system for 35 minutes to remove dissolved oxygen in the water; add 30 g of sodium bisulfate and 35 g of ammonium persulfate to initiate the reaction, and keep warm for 4 hours;

[0057] Hydrolysis: Add 112 kg of sodium hydroxide into the reactor, raise the temperature to 90°C, and keep the temperature for 2 hours to obtain the salt-resistant emulsion polymer KR3 for oil displacement.

[0058] Example 4: Test of salt resistance of polymers: Salt-resistant emulsion polymers KR1, KR2, KR3 and commercially available oil displacement agent LH1 were respectively mixed with saline water with a salinity of 2410 mg / L (2410 mg of NaCl dissolved in 1L of water) and simulated sewage of 6000 mg / L (5861 mg of NaCl and 139 mg of CaCl2 dissolved in 1L of water) to prepare polymer brine solutions with a polymer concentration of 1500 mg / L. The apparent viscosity of the above polymer brine solutions was measured using a Brookfield DV-II viscometer with a 0# rotor at a speed of 6 rpm and a temperature of 45°C. The results are shown in Figure 2 .

[0059] Depend on Figure 2 It can be seen that the salt-resistant emulsion polymers KR1, KR2 and KR3 provided by the present invention have a relatively low molecular weight and exhibit good salt resistance in saline water with a salinity of 2410 mg / L and simulated sewage with a salinity of 6000 mg / L. Under the same conditions, the apparent viscosity of the salt water solution of the comparison sample ordinary polyacrylamide product LH1 polymer is lower, and the salt resistance of the salt-resistant emulsion polymers KR1, KR2 and KR3 is significantly better than that of ordinary polyacrylamide products.

[0060] Ordinary polyacrylamide is dissolved in a saline solution. Due to the repulsive effect of salt ions on the ionic groups on the polymer molecular chain, the increase in salt ion concentration causes the polymer molecular chain to be further compressed and curled, and the fluid mechanics volume is greatly reduced, and the macroscopic performance is that the viscosity is greatly reduced. Since the polymer molecular chain of the present invention contains functional groups such as flexible long-chain groups and six-membered ring structures, the polymer molecular radius is increased, and the ability of the polymer molecule to resist salt ion compression is improved. The molecular chain is not easy to curl in high-concentration salt water, and its viscosity value is significantly greater than the comparative polyacrylamide product with a molecular weight close to it after the salt concentration increases. In the study of the salt resistance of polymers, the introduction of rigid monomers often leads to a decrease in the water solubility of the polymer, so it is difficult to obtain a polymer that improves both water solubility and salt resistance at the same time, or at least maintains water solubility while improving salt resistance. The polymer described in the present invention better solves the contradiction between water solubility and salt resistance. The polymer of the present invention introduces functional groups such as long-chain alkyl groups, sulfonate groups, and six-membered ring structure molecules into the main molecular chain of polyacrylamide, and reasonably controls the proportion of each group in the molecular chain. On the basis of ensuring molecular linearity, the polymer molecular radius is increased, the polymer molecular chain rigidity is enhanced, and the salt resistance and oil displacement performance of the polymer are improved while ensuring that the polymer has good water solubility.

[0061] Example 5: Evaluation of shear resistance: The salt-resistant emulsion polymer KR1 was mixed with saline water with a salinity of 2410 mg / L to prepare polymer aqueous solutions with concentrations of 1500 mg / L and 2000 mg / L, and the viscosity of the salt-resistant emulsion polymer at different concentrations was measured; the viscosity of the emulsion before and after shearing was measured by a T25 high-speed homogenizer at 2000 r / min, 3000 r / min, and 5000 r / min for 60s, 180s, 300s, and 600s, and the viscosity retention rate was calculated. The results are shown in FIG. Figure 3 and Figure 4 , Figure 3 and Figure 6 shown.

[0062] 1) 1500 mg / L salt-resistant emulsion polymer aqueous solution (placed for 36 hours, initial viscosity 25.4 mPa·s)

[0063] Figure 3 , Figure 4 It shows that the 1500mg / L polymer aqueous solution prepared with the salt-resistant emulsion polymer KR1 has a viscosity retention rate of more than 90% after mechanical shearing at 2000r / min for 600s; more than 85% after mechanical shearing at 3000r / min for 600s; and 70% after mechanical shearing at 5000r / min for 600s. This shows that the salt-resistant emulsion polymer of the present application has good shear resistance and is conducive to retaining higher viscosity after shearing of the underground oil layer core.

[0064] 2) 2000 mg / L salt-resistant emulsion polymer aqueous solution (after 36 hours, initial viscosity is 55.3 mPa·s)

[0065] Figure 3 , Figure 6 The results show that after mechanical shearing at 3000 r / min, the 2000 mg / L salt-resistant emulsion polymer aqueous solution showed viscosity increase (shear thickening, small viscosity loss in underground oil layers); after mechanical shearing at 5000 r / min for 600 seconds, the viscosity retention rate was 88.0%, and the viscosity loss was small.

[0066] As can be seen from the above, the viscosity of the 1500mg / L salt-resistant emulsion polymer aqueous solution decreased at a speed of 3000r / min, and the viscosity of the 2000mg / L salt-resistant emulsion polymer aqueous solution increased at a speed of 3000r / min, indicating that for high-concentration salt-resistant emulsion polymer aqueous solutions, shear viscosity increase occurs at low speeds. The viscosity retention rate of the 1500mg / L salt-resistant emulsion polymer aqueous solution at a speed of 5000r / min is 77%; the viscosity retention rate of the 2000mg / L salt-resistant emulsion polymer aqueous solution at a speed of 5000r / min is 88%, indicating that the anti-shear performance of the salt-resistant emulsion polymer is good.

[0067] Example 5: Evaluation of oil displacement effect: An oil displacement experiment was carried out using Bailey cores (30×4.5×4.5; water-measured permeability of 100mD) to study the oil displacement effect of injecting a plug-type salt-resistant emulsion polymer. A 1800mg / L polymer aqueous solution was prepared with salt-resistant emulsion polymer KR1 (9 days of storage, viscosity of 40mPa.s), and water was injected into the core at a rate of 0.35mL / min. The water flooding was terminated when the water content was above 98%. After injecting 0.5PV of emulsion at the same injection rate, subsequent water was injected, and the experiment was terminated when the water content of the produced liquid was greater than 98%. The experimental results are as follows Figure 7 , Figure 8 What you see;

[0068] Figure 7 , Figure 8 It shows that the chemical flooding recovery rate of the salt-resistant emulsion polymer KR1 is 10.74%; the recovery rate of the salt-resistant emulsion polymer injection stage is 8.57%, and the recovery rate of the subsequent water stage is 2.17%. The injection of salt-resistant emulsion polymer has a significant pore plugging effect, which is manifested in the increase of pressure and the decrease of water content in the salt-resistant emulsion polymer injection stage. The pressure drop in the subsequent water stage is not obvious. According to the injection capacity evaluation experiment, it can be seen that the core has a certain degree of blockage. Fig. 9 It shows that compared with ordinary ultra-high molecular weight polyacrylamide of the same viscosity and molecular weight of 19 million, the pressure rise is larger, indicating that the salt-resistant emulsion polymer has a good plugging effect and a high recovery degree.

[0069] in conclusion:

[0070] (1) The salt-resistant emulsion polymer has good viscosity-increasing and shear resistance properties, and the viscosity retention rate is above 85% when the 1500 mg / L emulsion is rotated at 3000 r / min for 600 s;

[0071] (2) The salt-resistant emulsion polymer has good salt resistance;

[0072] (3) When the same PV number is injected, the emulsion pressure rises more significantly than that of 19 million HPAM with the same viscosity, and the oil recovery rate of the salt-resistant emulsion polymer flooding is high, indicating that the salt-resistant emulsion polymer has a good plugging effect.

[0073] Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field and related fields without creative work should fall within the scope of protection of the present invention. The structures, devices and operating methods not specifically described and explained in the present invention are implemented according to the conventional means in the field unless otherwise specified and limited.

Claims

1. A salt-resistant emulsion polymer, Features: The invention is prepared by inverse emulsion polymerization of aqueous materials including monomer A, monomer B and monomer C, wherein the molar ratio of monomer A, monomer B and monomer C is (15-50):(5-10):

1.

2. A salt-resistant emulsion polymer according to claim 1, Features: The viscosity average molecular weight of the polymer is 1 million to 10 million.

3. A salt-resistant emulsion polymer according to claim 1, Features: The polymer is prepared into a polymer salt solution with a polymer concentration of 1500 mg / L and a mineralization degree of 2400-6000 mg / L. The apparent viscosity of the polymer salt solution at 45° C. is 10-40 mPa·s.

4. A method for preparing a salt-resistant emulsion polymer, The following steps are involved: 1) preparing aqueous phase materials; The aqueous phase material includes monomer A, monomer B, monomer C and water, the mass ratio of monomer A, monomer B and monomer C is (60-80): (15-30): (5-10), and the mass ratio of the solid matter contained in the above mixed system to deionized water is 40-50%: 50-60%; 2) preparing oil phase materials; The oil phase material comprises an organic solvent, a first emulsifier and a second emulsifier, and the mass ratio of the organic solvent, the first emulsifier and the second emulsifier is 100:(1.5-3):(3-8); 3) mixing and emulsifying the aqueous phase material obtained in step 1) and the oil phase material obtained in step 2) to obtain a monomer emulsion; 4) introducing nitrogen into the monomer emulsion obtained in step 3) to deoxygenate, and performing a polymerization reaction in the presence of an initiator to obtain an emulsion polymer; 5) adding sodium hydroxide to the emulsion polymer obtained in step 4), wherein the mass ratio of the emulsion polymer system to the sodium hydroxide is 100:(2-3), heating the emulsion system to 85-95° C. and keeping the temperature for 2-6 hours to obtain a salt-resistant emulsion polymer.

5. A method for preparing a salt-resistant emulsion polymer according to claim 4, Features: The initiators include sulfate initiators, phosphate initiators, peroxide initiators and azo initiators, and the mass ratio of the initiator to monomer A is 1:(10-1000).

6. A method for preparing a salt-resistant emulsion polymer according to claim 4, Features: The polymerization reaction temperature is 20° C.-50° C., the pH value is 4-11, and the reaction time is 1-24 hours.

7. A method for preparing a salt-resistant emulsion polymer according to claim 4, Features: The organic solvent may be selected from at least one of white oil, kerosene, hexane, petroleum ether, acetone, toluene, dichloromethane and chloroform.

8. A method for preparing a salt-resistant emulsion polymer according to claim 4, Features: The first emulsifier can be selected from at least one of Span20, Span60 and Span80, and the second emulsifier can be selected from at least one of fatty alcohol polyoxyethylene ether, alkylphenol polyoxyethylene polyoxypropylene ether, alkylamine polyoxyethylene ether, fatty amide polyoxyethylene ether, sorbitan fatty acid ester, glyceryl monostearate, glyceryl monolaurate and glyceryl monooleate.

Citation Information

Cited By

  • Stain-resistant salt-tolerant polymer for oil extraction and synthesis method thereof

    CN120230247A

  • Stain-resistant and salt-resistant monomer DLCM for oil extraction and synthesis method thereof

    CN120248208A