Retarder for high-temperature-resistant oil well cement as well as preparation method and application of retarder
Through cluster polymerization of unsaturated carboxylic acid monomers and ammonium salt cationic monomers and compounding of ethylenediaminetetramethylphosphonate, the surface adsorption capacity and hydration delay effect of the retarder are improved, and the solution is to solve the problem of The existing anti-high temperature retarder is not thickened for insufficient time at ultra-high temperatures, and the efficient compression strength of cement stone has been improved.
Patent Information
- Application Number
- CN202310600293.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-25
AI Technical Summary
The existing anti-high temperature retarder has insufficient thickening time at high temperature and limited molecular chain temperature resistance, which cannot meet the cementing needs under ultra-high temperature bottom well conditions.
Unsaturated carboxylic acid monomer, 2-methyl-2-acrylamidopropanesulfonic acid and ammonium salt cationic monomers are used for cluster polymerization to generate sulfonic acid-carboxylic acid polymerization with cationic clusters on the molecular chain. and sodium ethylenediaminetetramethylphosphonate is compounded on the molecular chain to improve the adsorption capacity and hydration delay on the surface of cement particles.
The prepared retarder was extended to 343-600 minutes at 240°C, and the compressive strength of the cement stone reached more than 26.2MPa, meeting the construction requirements of ultra-high temperature cementing.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to a retarder for high temperature resistant oil well cement and a preparation method and application thereof. Background Art
[0002] With the advancement of drilling technology and the continuous deepening of oilfield exploration and development, the number of high-temperature deep wells and ultra-deep wells with bottom hole temperatures exceeding 200°C has gradually increased. The complex well conditions of deep wells and ultra-deep wells have brought new challenges to cementing technology, and also put forward higher performance requirements for cementing working fluid, namely cement slurry technology and its admixtures. Cementing is the process of lowering casing into the wellbore and pumping cementing fluid into the annulus between the casing and the wellbore through the casing. The cementing fluid is usually cement slurry. After the cementing fluid is replaced in place, the pump is stopped and solidified until the cementing fluid solidifies. Cementing mainly plays the role of protecting and supporting casing and isolating oil and gas layers, and is the basic guarantee for safe and efficient development of oil and gas. In order to ensure the safe construction of cementing, retarders are generally added to cement slurry. At present, the commonly used high temperature retarders are mostly synthetic polymers, which can make the thickening time of cement slurry 1 to 2 hours longer than the pumping construction time.
[0003] Yan Siming, Wu Yanan, Yang Shengyue, Yang Shen, Wang Yongji, Tang Bao. Synthesis and performance evaluation of high temperature retarder AMCT [J]. Fine Chemicals, 2017, 34(05): 562-568. A high temperature retarder (AMCT) was synthesized using sodium methyl methacrylate sulfonate (MAS), hydrophilic long chain olefin monomer (CL), acrylic acid (AA) and allyl trimethyl ammonium chloride (TMAAC) as raw materials. The maximum applicable temperature can only reach 200 °C.
[0004] Patent CN109824822B uses carboxylic acid monomers, ammonium salt cationic monomers and sulfonate monomers to prepare high temperature retarders, and the applicable temperature range is only 50-180°C.
[0005] Patent CN109824823B uses carboxylic acid monomers, ammonium salt cationic monomers, sulfonate monomers and N,N-dimethylacrylamide to prepare high temperature resistant retarders, and the maximum applicable temperature can only reach 220°C.
[0006] Patent CN111662409B obtains a high-temperature oil well cement retarder by polymerizing 2-acrylamide-2-methylpropane sulfonic acid, unsaturated carboxylic acid monomers, steric hindrance functional monomers and cationic functional monomers through aqueous solution. The maximum applicable temperature can only reach 150°C. It can inhibit the "bulging" and "core-wrapping" phenomena of cement slurry in the temperature range of 120-150°C, and does not affect the strength development of cement stone. The comprehensive performance of cement slurry is good.
[0007] Feng Dejie, Yang Qizhen, Cao Chengzhang. Synthesis and performance study of large temperature difference retarder for oil well cement [J]. Synthetic Chemistry, 2023, 31(02): 93-100. A large temperature difference retarder for oil well cement was synthesized using 2-methyl-2-acrylamidopropanesulfonic acid (AMPS), acrylic acid (AA), methacryloyloxyethyltrimethylammonium chloride (DMC) and long-chain quaternary ammonium salt (DBrC) as monomers, which can only meet the large temperature difference cementing construction requirements of 60-150℃.
[0008] Wu Yanhua. Synthesis of high temperature resistant zwitterionic oil well cement retarder and study on its retarding mechanism, Synthetic Chemistry, 2023, 31(2), 101-108. A high temperature resistant zwitterionic polymer oil well cement retarder HFB-2 was synthesized by aqueous solution polymerization reaction using acrylamide (AM), 2-acrylamide-2-methylpropanesulfonic acid (AMPS), maleic anhydride (MAH) and dimethyldiallylammonium chloride (DMDAAC) as polymerization monomers. The maximum applicable temperature can only reach 220°C.
[0009] Yu Yongjin, Xue Yucheng, Xia Xiujian, Wang Chengwen, Liu Huiting, Meng Renzhou, Chen Zehua, Liu Bonuo. Research and development and evaluation of a 240℃ ultra-high temperature cementing retarder [J]. Natural Gas Industry, 2023, 43(03): 107-112. A new type of quaternary ultra-high temperature zwitterionic retarder (HTRP) was prepared by using strong adsorption cationic monomers (CP-22) and unsaturated carboxylic acids and other high temperature resistant monomers. The cement slurry thickening time reached 401min at an ultra-high temperature cycle temperature of 240℃. However, the inventors believe that: in this scheme, the cationic monomers are directly polymerized with other monomers, and the cations are dispersed in the molecular chain, and the adsorption performance is not as expected.
[0010] In patent CN109503781B, an aqueous solution of itaconic acid and 2-acrylamido-2-methylpropanesulfonic acid is mixed with an inorganic non-metallic material and a silane coupling agent, and reacted in the presence of an initiator to obtain an inorganic-organic polymer oil well cement retarder, which is applicable only at a maximum temperature of 230°C.
[0011] Peng Zhigang, Zhang Bojian, Feng Qian, Huang Renguo, Zhang Jian, Liu Gaofeng. Preparation and properties of polymer intercalated montmorillonite composite high temperature retarder [J]. Journal of the Chinese Ceramic Society, 2018, 46(08): 1087-1094. An organic-inorganic composite high temperature retarder (HTR-5) was synthesized by solution polymerization in situ intercalation method with 2-acrylamido-2-methylpropanesulfonic acid (AMPS), acrylic acid (AA), diallyldimethylammonium chloride (DMDAAC) as monomers and montmorillonite as active polymer filler. The applicable temperature range can only reach 150-180℃.
[0012] In summary, the currently commonly used high temperature retarders are mostly synthetic high molecular polymers, but the temperature resistance of polymer molecular chains is limited. Summary of the invention
[0013] In order to solve at least one of the above technical problems and increase the selection space of retarders for oil well cement to be suitable for more application scenarios, the present invention provides a retarder for high temperature resistant oil well cement with good temperature resistance and a preparation method thereof.
[0014] As one aspect of the present invention, it relates to a retarder for high temperature resistant oil well cement, the retarder comprising a sulfonic acid-carboxylic acid polymer with cationic clusters on the molecular chain generated by polymerization of an unsaturated carboxylic acid monomer, 2-methyl-2-acrylamidopropanesulfonic acid and an ammonium salt cationic monomer in the form of clusters; the mass ratio of the ammonium salt cationic monomer, the unsaturated carboxylic acid monomer and the 2-methyl-2-acrylamidopropanesulfonic acid is 17:(19-30):(52-64).
[0015] In a specific embodiment, the retarder further comprises sodium ethylenediaminetetramethylenephosphonate.
[0016] Furthermore, the mass of the sodium ethylenediaminetetramethylenephosphonate accounts for 15-30% of the mass of the sulfonic acid-carboxylic acid polymer with cationic clusters on the molecular chain.
[0017] In a specific embodiment, the unsaturated carboxylic acid monomer is selected from one of itaconic acid, maleic acid, fumaric acid and acrylic acid.
[0018] In a specific embodiment, the ammonium salt cationic monomer is selected from methacryloyloxyethyl trimethyl ammonium chloride or acryloyloxyethyl trimethyl ammonium chloride.
[0019] As another aspect of the present invention, it relates to a method for preparing the above-mentioned retarder for high-temperature oil well cement, wherein the method uses cluster distribution to distribute ammonium salt cationic monomers in the molecular structure of the sulfonic acid-carboxylic acid polymer with cationic clusters on the molecular chain.
[0020] Specifically, the following steps are included:
[0021] S1. Preparation of Solution A
[0022] Add water to dissolve the ammonium salt cationic monomer, and dropwise add a portion of the aqueous solution of the initiator under stirring. After the dropwise addition is completed, heat the reaction to obtain solution A;
[0023] S2. Preparation of Solution B
[0024] Under heating and stirring conditions, water is added to dissolve the unsaturated carboxylic acid monomer and 2-methyl-2-acrylamidopropanesulfonic acid, and the pH value of the solution is adjusted to obtain a solution B;
[0025] S3. Preparation of polymer
[0026] The solution B prepared by S2 is stirred at a constant temperature, and after the temperature is raised, it is added to the solution A prepared by S1, and the remaining aqueous solution of the initiator is added dropwise while stirring continuously, and refluxed to obtain a sulfonic acid-carboxylic acid polymer with cationic clusters on the molecular chain;
[0027] S4. Preparation of retarder
[0028] After the polymer obtained in S3 is cooled to room temperature, sodium ethylenediaminetetramethylenephosphonate is added and stirred evenly to obtain a retarder;
[0029] The aqueous solution of the initiator described in S1 or S3 refers to the solution prepared by dissolving the initiator in water accounting for 60% of the mass of the ammonium salt cationic monomer.
[0030] In a specific embodiment, in S1, the reaction temperature is 60-65°C, and the reaction time is 0.5-1h.
[0031] In a specific embodiment, in S2, the pH value of the solution B is 2-4.
[0032] In a specific embodiment, in S3, the temperature is raised to 60-70°C and then added to the solution A prepared in S1.
[0033] In a specific embodiment, in S3, the reflux reaction time is 6 to 8 hours.
[0034] In a specific embodiment, the mass of the initiator is 1.5% to 3% of the mass of the ammonium salt cationic monomer.
[0035] Furthermore, the initiator is selected from ammonium persulfate or potassium persulfate.
[0036] As another aspect of the present invention, it relates to a cementing cement slurry, wherein the above-mentioned retarder for high temperature resistant oil well cement is used in the cementing fluid.
[0037] As another aspect of the present invention, it relates to an oil and gas well cementing process, wherein the oil and gas well cementing process uses the above-mentioned cementing slurry.
[0038] The present invention develops an ultra-high temperature retarder from the perspective of improving the adsorption capacity of molecular chains on the surface of cement particles, forms cation clusters on the generated polymer molecular chains, transforms the dispersed distribution of cations in the molecular chains into clustered distribution, and increases the adsorption capacity of molecular chains on the surface of cement particles. 2+ The ability of sodium ethylenediaminetetra(methylenephosphonic acid) to hinder the formation of calcium hydroxide crystal nuclei in cement slurry, further delaying the hydration of cement slurry.
[0039] The retarder prepared by the present invention has a temperature resistance of 240°C. When the retarder is added in an amount of 2% to 4%, the thickening time of the cement slurry at 240°C is between 343 and 600 minutes. After the cement slurry system is cured for 24 hours, the compressive strength of the cement stone reaches more than 26.2 MPa, which can meet the requirements of ultra-high temperature cementing.
[0040] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention are realized and obtained by the structures particularly pointed out in the description and claims. DETAILED DESCRIPTION
[0041] In order to better understand the above technical solution, the above technical solution will be described in detail below in combination with specific implementation methods. The sources of materials mainly involved in the embodiments of the present invention are shown in Table 1 below, and other materials not shown are conventional commercial products.
[0042] Table 1: Material source description
[0043]
[0044] In addition, the 191230 high and low temperature dual cylinder pressurized thickener used in the embodiment of the present invention is from Liaoning Bestray Petroleum Equipment Manufacturing Co., Ltd., and the 4265 ultrasonic cement stone strength analyzer used is from the American Qiandele Instrument Company.
[0045] The inventors have continuously optimized the composition and preparation method of the retarder material through a large number of experimental studies, and provided Examples 1 to 8.
[0046] Example 1
[0047] The retarder of this embodiment is prepared by the following steps:
[0048] S1. Preparation of Solution A
[0049] 17 g of methacryloyloxyethyl trimethylammonium chloride (DMC, ammonium salt cationic monomer) was dissolved in 30 g of deionized water, and a 50 wt % aqueous solution of ammonium persulfate was added dropwise at a stirring speed of 200 r / min. After the addition was completed, the temperature was raised to 65° C. and the reaction was carried out for 0.5 h to obtain solution A;
[0050] S2. Preparation of Solution B
[0051] 29 g of itaconic acid (IA) and 54 g of 2-methyl-2-acrylamidopropanesulfonic acid (AMPS) were dissolved in 136 g of deionized water, and after stirring at 45° C. for 15 min, a saturated sodium hydroxide solution was used to adjust the pH of the solution to 3 to obtain a solution B;
[0052] S3. Preparation of polymer
[0053] The solution B prepared in S2 was stirred at 45°C for 30 minutes, and then the temperature was raised to 65°C and added to the solution A prepared in S2. The remaining 50 wt% of the aqueous solution of ammonium persulfate was added dropwise at a stirring speed of 200 r / min, and the mixture was refluxed for 8 hours to obtain a sulfonic acid-carboxylic acid polymer with cationic clusters on the molecular chain.
[0054] S4. Preparation of retarder
[0055] After the polymer in S3 is cooled to room temperature, 15% of the mass of the polymer is added with sodium ethylenediaminetetramethylenephosphonate and stirred evenly to obtain a retarder;
[0056] The aqueous solution of the initiator described in S1 and / or S3 is prepared by dissolving 0.51 g of ammonium persulfate (initiator) in 10.2 g of deionized water.
[0057] The retarder prepared in this example has a viscosity of 480 mPa·s and a relative molecular weight of 19820.
[0058] Example 2
[0059] The retarder of this embodiment is prepared by the following steps:
[0060] S1. Preparation of Solution A
[0061] 17 g of acryloyloxyethyl trimethylammonium chloride (DAC, ammonium salt cationic monomer) was dissolved in 30 g of deionized water, and a 50 wt % aqueous solution of potassium persulfate was added dropwise at a stirring speed of 200 r / min. After the addition was completed, the temperature was raised to 60° C. and the reaction was carried out for 1 hour to obtain a solution A;
[0062] S2. Preparation of Solution B
[0063] 19 g of maleic acid (MA) and 64 g of 2-methyl-2-acrylamidopropanesulfonic acid (AMPS) were dissolved in 136 g of deionized water, and after stirring at 45° C. for 15 min, a saturated sodium hydroxide solution was used to adjust the pH of the solution to 2.4 to obtain a solution B;
[0064] S3. Preparation of polymer
[0065] The solution B prepared in S2 was stirred at 45°C for 30 minutes, and then the temperature was raised to 60°C and added to the solution A prepared in S2. The remaining 50 wt% of the aqueous solution of potassium persulfate was added dropwise at a stirring speed of 200 r / min, and the mixture was refluxed for 6.5 hours to obtain a sulfonic acid-carboxylic acid polymer with cationic clusters on the molecular chain.
[0066] S4. Preparation of retarder
[0067] After the polymer in S3 is cooled to room temperature, 20% of the mass of the polymer is added with sodium ethylenediaminetetramethylenephosphonate and stirred evenly to obtain a retarder;
[0068] The aqueous solution of the initiator described in S1 and / or S3 is prepared by dissolving 0.31 g of potassium persulfate (initiator) in 10.2 g of deionized water.
[0069] The retarder prepared in this example has a viscosity of 600 mPa·s and a relative molecular weight of 30215.
[0070] Example 3
[0071] The retarder of this embodiment is prepared by the following steps:
[0072] S1. Preparation of Solution A
[0073] 17 g of methacryloyloxyethyl trimethylammonium chloride (DMC, ammonium salt cationic monomer) was dissolved in 30 g of deionized water, and a 50 wt % aqueous solution of ammonium persulfate was added dropwise at a stirring speed of 200 r / min. After the addition was completed, the temperature was raised to 65° C. and the reaction was carried out for 0.6 h to obtain solution A;
[0074] S2. Preparation of Solution B
[0075] 20 g of fumaric acid (FA) and 60 g of 2-methyl-2-acrylamidopropanesulfonic acid (AMPS) were dissolved in 136 g of deionized water, and after stirring at 45° C. for 15 min, a saturated sodium hydroxide solution was used to adjust the pH of the solution to 4 to obtain a solution B;
[0076] S3. Preparation of polymer
[0077] The solution B prepared in S2 was stirred at 45°C for 30 minutes, and then the temperature was raised to 70°C and added to the solution A prepared in S2. The remaining 50 wt% of the aqueous solution of ammonium persulfate was added dropwise at a stirring speed of 200 r / min, and the mixture was refluxed for 7.5 hours to obtain a sulfonic acid-carboxylic acid polymer with cationic clusters on the molecular chain.
[0078] S4. Preparation of retarder
[0079] After the polymer in S3 is cooled to room temperature, 30% of the mass of the polymer is added with sodium ethylenediaminetetramethylenephosphonate and stirred evenly to obtain a retarder;
[0080] The aqueous solution of potassium persulfate described in S1 and / or S3 is prepared by dissolving 0.34 g of ammonium persulfate (initiator) in 10.2 g of deionized water.
[0081] The retarder prepared in this example has a viscosity of 422 mPa·s and a relative molecular weight of 12589.
[0082] Example 4
[0083] The retarder of this embodiment is prepared by the following steps:
[0084] S1. Preparation of Solution A
[0085] 17 g of acryloyloxyethyl trimethylammonium chloride (DAC, ammonium salt cationic monomer) was dissolved in 30 g of deionized water, and a 50 wt % aqueous solution of potassium persulfate was added dropwise at a stirring speed of 200 r / min. After the addition was completed, the temperature was raised to 62° C. and the reaction was carried out for 0.8 h to obtain solution A;
[0086] S2. Preparation of Solution B
[0087] 30 g of acrylic acid (AA) and 64 g of 2-methyl-2-acrylamidopropanesulfonic acid (AMPS) were dissolved in 136 g of deionized water, and after stirring at 45° C. for 15 min, a saturated sodium hydroxide solution was used to adjust the pH of the solution to 2.5 to obtain a solution B;
[0088] S3. Preparation of polymer
[0089] The solution B prepared in S2 was stirred at 45°C for 30 minutes, and then the temperature was raised to 63°C and added to the solution A prepared in S2. The remaining 50 wt% of the aqueous solution of potassium persulfate was added dropwise at a stirring speed of 200 r / min, and the mixture was refluxed for 6 hours to obtain a sulfonic acid-carboxylic acid polymer with cationic clusters on the molecular chain.
[0090] S4. Preparation of retarder
[0091] After the polymer in S3 is cooled to room temperature, 25% of the mass of the polymer is added with sodium ethylenediaminetetramethylenephosphonate and stirred evenly to obtain a retarder;
[0092] The aqueous solution of potassium persulfate described in S1 and / or S3 is prepared by dissolving 0.37 g of potassium persulfate (initiator) in 10.2 g of deionized water.
[0093] The retarder prepared in this example has a viscosity of 570 mPa·s and a relative molecular weight of 27153.
[0094] Example 5
[0095] The retarder of this embodiment is prepared by the following steps:
[0096] S1. Preparation of Solution A
[0097] 17 g of methacryloyloxyethyl trimethylammonium chloride (DMC, ammonium salt cationic monomer) was dissolved in 30 g of deionized water, and a 50 wt % aqueous solution of ammonium persulfate was added dropwise at a stirring speed of 200 r / min. After the addition was completed, the temperature was raised to 63° C. and the reaction was carried out for 1 hour to obtain a solution A;
[0098] S2. Preparation of Solution B
[0099] 25 g of itaconic acid (IA) and 52 g of 2-methyl-2-acrylamidopropanesulfonic acid (AMPS) were dissolved in 136 g of deionized water, and after stirring at 45° C. for 15 min, a saturated sodium hydroxide solution was used to adjust the pH of the solution to 3.8 to obtain a solution B;
[0100] S3. Preparation of polymer
[0101] Solution B prepared in S2 was stirred at 45°C for 30 min, then the temperature was raised to 66°C and added to solution A prepared in S2. The remaining 50 wt% of the aqueous solution of ammonium persulfate was added dropwise at a stirring speed of 200 r / min, and the mixture was refluxed for 7 h to obtain a sulfonic acid-carboxylic acid polymer with cationic clusters on the molecular chain.
[0102] S4. Preparation of retarder
[0103] After the polymer in S3 is cooled to room temperature, 18% of the mass of the polymer is added with sodium ethylenediaminetetramethylenephosphonate and stirred evenly to obtain a retarder;
[0104] The aqueous solution of the initiator described in S1 and / or S3 is prepared by dissolving 0.48 g of ammonium persulfate (initiator) in 10.2 g of deionized water.
[0105] The retarder prepared in this example has a viscosity of 750 mPa·s and a relative molecular weight of 43256.
[0106] Example 6
[0107] The retarder of this embodiment is prepared by the following steps:
[0108] S1. Preparation of Solution A
[0109] 17 g of acryloyloxyethyl trimethylammonium chloride (DAC, ammonium salt cationic monomer) was dissolved in 30 g of deionized water, and a 50 wt % aqueous solution of potassium persulfate was added dropwise at a stirring speed of 200 r / min. After the addition was completed, the temperature was raised to 61° C. and the reaction was carried out for 0.5 h to obtain solution A;
[0110] S2. Preparation of Solution B
[0111] 19 g of maleic acid (MA) and 52 g of 2-methyl-2-acrylamidopropanesulfonic acid (AMPS) were dissolved in 136 g of deionized water, and after stirring at 45° C. for 15 min, a saturated sodium hydroxide solution was used to adjust the pH of the solution to 2.2 to obtain a solution B;
[0112] S3. Preparation of polymer
[0113] Solution B prepared in S2 was stirred at 45°C for 30 min, then the temperature was raised to 68°C and added to solution A prepared in S2. The remaining 50 wt% of the aqueous solution of potassium persulfate was added dropwise at a stirring speed of 200 r / min, and the mixture was refluxed for 6 h to obtain a sulfonic acid-carboxylic acid polymer with cationic clusters on the molecular chain.
[0114] S4. Preparation of retarder
[0115] After the polymer in S3 is cooled to room temperature, 28% of the mass of the polymer is added with sodium ethylenediaminetetramethylenephosphonate and stirred evenly to obtain a retarder;
[0116] The aqueous solution of potassium persulfate described in S1 and / or S3 is prepared by dissolving 0.29 g of potassium persulfate (initiator) in 10.2 g of deionized water.
[0117] The retarder prepared in this example has a viscosity of 534 mPa·s and a relative molecular weight of 23565.
[0118] Example 7
[0119] The retarder of this embodiment is prepared by the following steps:
[0120] S1. Preparation of Solution A
[0121] 17 g of methacryloyloxyethyl trimethylammonium chloride (DMC, ammonium salt cationic monomer) was dissolved in 30 g of deionized water, and a 50 wt % aqueous solution of ammonium persulfate was added dropwise at a stirring speed of 200 r / min. After the addition was completed, the temperature was raised to 64° C. and the reaction was carried out for 0.9 h to obtain solution A;
[0122] S2. Preparation of Solution B
[0123] 24 g of fumaric acid (FA) and 60 g of 2-methyl-2-acrylamidopropanesulfonic acid (AMPS) were dissolved in 136 g of deionized water, and after stirring at 45° C. for 15 min, a saturated sodium hydroxide solution was used to adjust the pH of the solution to 3.5 to obtain a solution B;
[0124] S3. Preparation of polymer
[0125] The solution B prepared in S2 was stirred at 45°C for 30 minutes, and then the temperature was raised to 62°C and added to the solution A prepared in S2. The remaining 50 wt% of the aqueous solution of ammonium persulfate was added dropwise at a stirring speed of 200 r / min, and the mixture was refluxed for 7.5 hours to obtain a sulfonic acid-carboxylic acid polymer with cationic clusters on the molecular chain.
[0126] S4. Preparation of retarder
[0127] After the polymer in S3 is cooled to room temperature, ethylenediaminetetramethylenephosphonic acid sodium accounting for 26% of the mass of the polymer is added and stirred evenly to prepare a retarder;
[0128] The aqueous solution of the initiator described in S1 and / or S3 is prepared by dissolving 0.26 g of ammonium persulfate (initiator) in 10.2 g of deionized water.
[0129] The retarder prepared in this example has a viscosity of 492 mPa·s and a relative molecular weight of 20156.
[0130] Example 8
[0131] The retarder of this embodiment is prepared by the following steps:
[0132] S1. Preparation of Solution A
[0133] 17 g of acryloyloxyethyl trimethylammonium chloride (DAC, ammonium salt cationic monomer) was dissolved in 30 g of deionized water, and a 50 wt % aqueous solution of potassium persulfate was added dropwise at a stirring speed of 200 r / min. After the addition was completed, the temperature was raised to 60° C. and the reaction was carried out for 0.7 h to obtain solution A;
[0134] S2. Preparation of Solution B
[0135] 30 g of acrylic acid (AA) and 52 g of 2-methyl-2-acrylamidopropanesulfonic acid (AMPS) were dissolved in 136 g of deionized water, and after stirring at 45° C. for 15 min, a saturated sodium hydroxide solution was used to adjust the pH of the solution to 2 to obtain a solution B;
[0136] S3. Preparation of polymer
[0137] Solution B prepared in S2 was stirred at 45°C for 30 min, then the temperature was raised to 62°C and added to solution A prepared in S2. The remaining 50 wt% of the aqueous solution of potassium persulfate was added dropwise at a stirring speed of 200 r / min, and the mixture was refluxed for 6.5 h to obtain a sulfonic acid-carboxylic acid polymer with cationic clusters on the molecular chain.
[0138] S4. Preparation of retarder
[0139] After the polymer in S3 is cooled to room temperature, ethylenediaminetetramethylenephosphonic acid sodium accounting for 26% of the mass of the polymer is added and stirred evenly to prepare a retarder;
[0140] The aqueous solution of potassium persulfate described in S1 and / or S3 is prepared by dissolving 0.41 g of potassium persulfate (initiator) in 10.2 g of deionized water.
[0141] The retarder prepared in this example has a viscosity of 450 mPa·s and a relative molecular weight of 15421.
[0142] The following are comparative examples 1 to 5 prepared by the inventors by making a series of changes to the experimental conditions during experimental research.
[0143] Comparative Example 1
[0144] The retarder of this comparative example is prepared by the following steps:
[0145] Dissolve 0.51 g of ammonium persulfate (initiator) in 10.2 g of deionized water to obtain an aqueous solution of ammonium persulfate;
[0146] 17 g of methacryloyloxyethyltrimethylammonium chloride (DMC, ammonium salt cationic monomer), 29 g of itaconic acid (IA) and 54 g of 2-methyl-2-acrylamidopropanesulfonic acid (AMPS) were dissolved in 136 g of deionized water, and after stirring at 45° C. for 30 min, a saturated sodium hydroxide solution was used to adjust the pH of the solution to 3 to obtain solution A;
[0147] After the obtained solution A was heated to 65°C, all the aqueous solution of ammonium persulfate was added dropwise at a stirring speed of 200 r / min, and refluxed for 8 hours to obtain a polymer;
[0148] After the prepared polymer is cooled to room temperature, 15% of the mass of the polymer sodium ethylenediaminetetramethylenephosphonate is added to the prepared polymer and stirred evenly to prepare a retarder.
[0149] The viscosity of the retarder prepared in this comparative example is 468 mPa·s, and the relative molecular weight is 19685.
[0150] Comparative Example 2
[0151] The retarder of this comparative example is prepared by the following steps:
[0152] Dissolve 0.31 g of potassium persulfate (initiator) in 10.2 g of deionized water to obtain a potassium persulfate aqueous solution;
[0153] 17 g of acryloyloxyethyltrimethylammonium chloride (DAC, ammonium salt cationic monomer), 19 g of maleic acid (MA) and 64 g of 2-methyl-2-acrylamidopropanesulfonic acid (AMPS) were dissolved in 136 g of deionized water, and after stirring at 45° C. for 30 min, a saturated sodium hydroxide solution was used to adjust the pH of the solution to 2.4 to obtain solution A;
[0154] After the obtained solution A was heated to 60°C, all the aqueous solution of potassium persulfate was added dropwise at a stirring speed of 200 r / min, and the mixture was refluxed for 6.5 hours to obtain a polymer;
[0155] After the prepared polymer is cooled to room temperature, 20% of the mass of the polymer sodium ethylenediaminetetramethylenephosphonate is added to the prepared polymer and stirred evenly to prepare a retarder.
[0156] The retarder prepared in this comparative example has a viscosity of 591 mPa·s and a relative molecular weight of 30001.
[0157] Comparative Example 3
[0158] The difference from Example 3 is that "17 g of dimethyldiallylammonium chloride (DMDAAC)" is used to replace "17 g of methacryloyloxyethyltrimethylammonium chloride (DMC)" in S1.
[0159] The viscosity of the retarder prepared in this comparative example is 353 mPa·s, and the relative molecular weight is 10125.
[0160] Comparative Example 4
[0161] The difference from Example 4 is that "64 g of sodium styrene sulfonate (SSS)" is used to replace "64 g of 2-methyl-2-acrylamidopropanesulfonic acid (AMPS)" in S2.
[0162] The viscosity of the retarder prepared in this comparative example is 732 mPa·s, and the relative molecular weight is 39524.
[0163] Comparative Example 5
[0164] The difference from Example 5 is that S4 is omitted.
[0165] The viscosity of the retarder prepared in this comparative example is 615 mPa·s, and the relative molecular weight is 30256.
[0166] In order to clearly understand the differences between Comparative Examples 1 to 5 and Examples 1 to 8, the inventors briefly explain them here:
[0167] In Comparative Examples 1-2, the ammonium cationic monomers did not form cationic clusters in the molecular structure of the retarder; in Comparative Examples 3-4, the same monomers were replaced; and in Comparative Example 5, no organic phosphonate was compounded.
[0168] The inventor prepared cement slurry according to "GB / T 19139-2012 Test Method for Oil Well Cement" for the retarders prepared in the above Examples 1 to 8 and Comparative Examples 1 to 5. The specific steps of the cement slurry formula are: G-grade oil well cement + 50% (cement mass) quartz sand (200 mesh) + x% (cement mass) retarder + y% water, and the liquid-to-solid ratio is 0.44.
[0169] The prepared cement slurry was tested for its thickening time according to ANSI / API Recommended Practice 10B-5.
[0170] At the same time, the inventors also tested the highest temperature that the retarder can withstand before failure. For example, the retarder effect is tested at 150°C. If the thickening curve is normal and there are no abnormal phenomena such as bulging, core encapsulation or super-retardation, the test temperature is increased to 160°C and the test is continued. This is repeated until the retarder fails. The last test temperature before the retarder fails is recorded as the test temperature (i.e., the highest temperature), and the compressive strength test results of the cement paste are tested at this test temperature. The above test results are recorded in Table 2 below.
[0171] Table 2: Retarder performance test results
[0172]
[0173] It can be seen from the data in Table 2 that the temperature resistance of the retarders prepared according to Examples 1 to 8 of the present invention can reach 240°C, and their temperature resistance is better than that of the retarders prepared in the comparative examples. Therefore, the inventors believe through data analysis that the improvement of temperature resistance is mainly due to the change of cationic monomers in the polymer molecular structure from traditional dispersed distribution to clustered distribution.
[0174] The experimental data results recorded in Table 2 show that when the retarder prepared by Examples 1 to 8 is used to prepare cement slurry, the initial consistency of the cement slurry is lower than 25Bc, and the compressive strength of the cement stone after 24 hours is greater than 26.2MPa, which meets the actual cementing requirements. Therefore, after a series of analyses, the inventor believes that when the retarder is prepared by the preparation method of the present invention, the thickening time of the cement slurry can be changed by adjusting the raw material ratio and reaction conditions.
[0175] Compared with Examples 1-2, the performance of the retarders of Comparative Examples 1-2 is generally inferior to that of the retarder materials prepared in Examples 1-2. It is inferred that the possible reason is that when preparing the retarder materials in Comparative Examples 1-2, the ammonium cationic monomers did not form cationic clusters in the molecular structure of the retarder. However, the structure of the cations in the form of clusters is more stable and not easily destroyed by high temperatures. Therefore, the retarders prepared in Examples 1-2 have stronger high temperature resistance and higher compressive strength.
[0176] Combining Comparative Example 3 and Example 3 and their test results, Comparative Example 3 uses dimethyldiallylammonium chloride with two double bonds in its molecular structure, which is easy to self-polymerize to form a ring structure during the preparation process, resulting in the inability to form a cationic cluster with copolymerization activity and effectively connect to the molecular chain of the polymer, resulting in the inability to effectively improve the temperature resistance of the polymer. Therefore, the inventors believe that when preparing the retarder, the ammonium salt cationic monomer is more recommended to use methacryloyloxyethyl trimethylammonium chloride or acryloyloxyethyl trimethylammonium chloride.
[0177] Through the performance test data in Table 2, we can also find that: Comparative Example 4 has the lowest compressive strength. Therefore, the inventors believe that the possible reason is that: Comparative Example 4 uses sodium styrene sulfonate with a rigid group when preparing the retarder, but this substance is not conducive to the stability of the cement slurry system and the development of the early strength of the cement stone.
[0178] Example 5 Compared with Comparative Example 5, an organic phosphonate is compounded. The organic phosphonate has a C—P—O bond electron ligand and can react with the Ca in cement. 2+ 、Al 3+ It forms a strong chelating structure that is not easily destroyed at high temperatures, and can synergize with the polymer to enhance the application temperature range of the retarder and its ability to inhibit hydration.
[0179] The above are only preferred feasible embodiments of the present invention, and the protection scope of the present invention is not limited thereto. Various modifications or applications made according to the above embodiments are within the protection scope of this technical solution.
[0180] Although the specific embodiments of the present invention have been described in detail, it will be understood by those skilled in the art. According to all the teachings disclosed, various modifications and replacements can be made to those details, and these changes are all within the protection scope of the present invention. The full scope of the present invention is given by the attached claims and any equivalents thereof.
Claims
1. A retarder for high temperature resistant oil well cement, characterized in that: The retarder comprises a sulfonic acid-carboxylic acid polymer with cationic clusters on the molecular chain, which is generated by polymerizing an unsaturated carboxylic acid monomer, 2-methyl-2-acrylamidopropanesulfonic acid and an ammonium salt cationic monomer in a clustered form; the mass ratio of the ammonium salt cationic monomer, the unsaturated carboxylic acid monomer and the 2-methyl-2-acrylamidopropanesulfonic acid is 17:(19-30):(52-64).
2. The retarder for high temperature resistant oil well cement according to claim 1, characterized in that: The retarder further comprises sodium ethylenediaminetetramethylenephosphonate.
3. The retarder for high temperature resistant oil well cement according to claim 2, characterized in that: The mass of the sodium ethylenediaminetetramethylenephosphonate accounts for 15-30% of the mass of the sulfonic acid-carboxylic acid polymer with cationic clusters on the molecular chain.
4. The retarder for high temperature resistant oil well cement according to claim 1, characterized in that: The unsaturated carboxylic acid monomer is selected from one of itaconic acid, maleic acid, fumaric acid and acrylic acid.
5. The retarder for high temperature resistant oil well cement according to claim 1, characterized in that: The ammonium salt cationic monomer is selected from methacryloyloxyethyl trimethyl ammonium chloride or acryloyloxyethyl trimethyl ammonium chloride.
6. A method for preparing a retarder for high temperature resistant oil well cement according to any one of claims 1 to 5, characterized in that: The method uses cluster distribution to distribute the ammonium salt cationic monomers in the molecular structure of the sulfonic acid-carboxylic acid polymer with cationic clusters on the molecular chain.
7. The method for preparing a retarder for high temperature resistant oil well cement according to claim 6, characterized in that: The following steps are involved: S1. Preparation of Solution A Add water to dissolve the ammonium salt cationic monomer, and dropwise add a portion of the aqueous solution of the initiator under stirring. After the dropwise addition is completed, heat the reaction to obtain solution A; S2. Preparation of Solution B Under heating and stirring conditions, water is added to dissolve the unsaturated carboxylic acid monomer and 2-methyl-2-acrylamidopropanesulfonic acid, and the pH value of the solution is adjusted to obtain a solution B; S3. Preparation of polymer The solution B prepared by S2 is stirred at a constant temperature, and after the temperature is raised, it is added to the solution A prepared by S1, and the remaining aqueous solution of the initiator is added dropwise while stirring continuously, and refluxed to obtain a sulfonic acid-carboxylic acid polymer with cationic clusters on the molecular chain; S4. Preparation of retarder After the polymer obtained in S3 is cooled to room temperature, sodium ethylenediaminetetramethylenephosphonate is added and stirred evenly to obtain a retarder; The aqueous solution of the initiator described in S1 or S3 refers to the solution prepared by dissolving the initiator in water accounting for 60% of the mass of the ammonium salt cationic monomer.
8. The method for preparing a retarder for high temperature resistant oil well cement according to claim 7, characterized in that: In S1, the reaction temperature is 60-65°C, and the reaction time is 0.5-1h.
9. The method for preparing a retarder for high temperature resistant oil well cement according to claim 7, characterized in that: In S2, the pH value of the solution B is 2-4.
10. The method for preparing a retarder for high temperature resistant oil well cement according to claim 7, characterized in that: In S3, the temperature is raised to 60-70°C and then added to the solution A prepared in S1.
11. The method for preparing a retarder for high temperature resistant oil well cement according to claim 7, characterized in that: In S3, the reflux reaction time is 6 to 8 hours.
12. The method for preparing a retarder for high temperature resistant oil well cement according to claim 7, characterized in that: The mass of the initiator is 1.5% to 3% of the mass of the ammonium salt cationic monomer.
13. The method for preparing a retarder for high temperature resistant oil well cement according to claim 12, characterized in that: The initiator is selected from ammonium persulfate or potassium persulfate.
14. A cementing slurry, characterized in that: The cementing slurry uses the retarder for high temperature resistant oil well cement as claimed in any one of claims 1 to 12.
15. An oil and gas well cementing process, characterized in that: The oil and gas well cementing process uses the cementing slurry as claimed in claim 13.
Citation Information
Patent Citations
High-temperature-resistant copolymer oil well cement retarder and preparation method thereof
CN104403056A
Temperature-responsive high temperature retarder suitable for oil-gas well cementation, preparation method thereof and well cementing slurry
CN109824822A
High-temperature oil well cement retarder capable of inhibiting abnormal gelling, and preparation method thereof
CN111662409A
High-temperature retarder suitable for oil and gas well cementation, preparation method thereof and cementing slurry
US20200239760A1
Cited By
Multi-element micromolecule compounded high-temperature-resistant oil well cement retarder and application thereof
CN121824004A