Wet-process low-temperature pressing color-changing polyurethane resin and preparation process thereof

By introducing a new chain extender 1,6-hexanediol and optimized formula technology, the problem of traditional wet polyurethane resin requiring dry veneer to achieve low-temperature hot-blasting discoloration is solved, and the color change effect is achieved under 130℃, reducing the reduction of color change effect The production cost and defective rate are improved, and the practicality of the product is improved.

CN119019640APending Publication Date: 2024-11-26FUJIAN YUANFA RESIN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411328703.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The production of traditional wet polyurethane resin requires dry veneer to achieve low-temperature hot pressing and discoloration, which increases production costs and unnecessary steps, making it difficult to meet the needs of special purposes.

Method used

A new chain extender 1,6-hexanediol was introduced. By optimizing the formulation process and mixing it with the original chain extender, the two-step synthesis method is adopted to ensure that the wet low-temperature hot-cold discoloration effect is achieved under 130℃, reducing the Production difficulty and time.

Benefits of technology

The effect of pressing and discoloration under 130℃ is achieved, which protects product integrity, reduces defective rates, improves product practicality and yield rates, and does not increase production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019640A_ABST
    Figure CN119019640A_ABST
Patent Text Reader

Abstract

The wet-process low-temperature pressing color-changing polyurethane resin is prepared from the following raw materials in parts by mass: 105 parts of polyester polyol PEBA-2000, 105 parts of polyester polyol PEDA-2000, 4 parts of ethylene glycol (EG), 16 parts of a chain extender 1, 6-hexanediol, 75 parts of MDI (Diphenyl Diisocyanate), 700 parts of DMF (Dimethyl Formamide), 0.5 part of an end-capping reagent, 0.8 part of a stabilizer, 0.05 part of a catalyst, 0.5 part of an antioxidant and 5 parts of a penetrating agent. According to the invention, a special chain extender is introduced, the chain extender and an original chain extender form a mixed chain extender through a process for optimizing a formula, and the wet-process polyurethane resin meeting the low-temperature pressing discoloring requirement can be produced without increasing the production difficulty through a process adjustment and addition method.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chemical materials, and specifically to an innovative synthesis method for wet-process pressed polyurethane resin by introducing a novel chain extender by changing a synthesis process, and is suitable for manufacturing wet-process low-temperature pressed color-changing polyurethane resin in the synthetic leather industry. Background Art

[0002] As a kind of widely used polymer material, the optimization of the performance of polyurethane resin has always been the focus of research and development in the chemical industry. In the production of traditional wet-process polyurethane resin, in order to print some LOGOs, it must be realized after dry-process veneer. For some special-purpose wet-process bases, its cheap production use undoubtedly adds a lot of unnecessary costs. In response to the requirements of this special field, a polyurethane resin for making wet-process bases is developed, which can directly achieve the effect of 130° low-temperature pressing and discoloration without dry-process veneer. It can help downstream customers save the cost of the entire dry-process veneer and achieve the same low-temperature pressing effect. The present invention has important industrial value and market prospects. Summary of the invention

[0003] The purpose of the present invention is to introduce a new chain extender, and through the process of optimizing the formula, this chain extender and the original chain extender are combined to form a mixed chain extender. Through our process adjustment and addition method, the production difficulty is not increased, and a wet-process polyurethane resin that meets the requirements of low-temperature pressing and discoloration can be produced.

[0004] In order to achieve the above object, the present invention adopts the following technical solution: A wet-process low-temperature pressing color-changing polyurethane resin, wherein the raw materials used include, by mass, 105 parts of polyester polyol PEBA-2000, 105 parts of polyester polyol PEDA-2000, 4 parts of ethylene glycol EG, 16 parts of chain extender 1,6-hexanediol, 75 parts of MDI, 700 parts of DMF, 0.5 parts of end-capping agent, 0.8 parts of stabilizer, 0.05 parts of catalyst, 0.5 parts of antioxidant, and 5 parts of penetrant.

[0005] Preferably, the capping agent is methanol.

[0006] Preferably, the catalyst is an organic bismuth catalyst.

[0007] Preferably, the antioxidant is a hindered phenol antioxidant.

[0008] Preferably, the stabilizer is malic acid.

[0009] Preferably, the penetrant is a fatty alcohol polyoxyethylene ether product.

[0010] The preparation process of the wet low-temperature pressing color-changing polyurethane resin comprises the following steps: (1) After preheating 180 parts of DMF, 105 parts of PEBA-2000 and 105 parts of PEDA-2000 to 45°C, slowly add 26 parts of MDI and maintain the reaction at 75°C for 2 hours; proceed to the second step, continue to add 180 parts of DMF, 0.5 parts of antioxidant, 4 parts of EG, and 16 parts of 1,6-hexanediol, mix and stir evenly, add 49 parts of MDI, maintain the reaction at 75°C for 2 hours, and finally add 0.05 parts of catalyst, react at 75°C for 1 hour, and increase the viscosity at a constant rate to a constant value; (2) When the viscosity of the prepolymer reaches 300,000 cps / 75°C, 340 parts of DMF solvent are gradually added in proportion to control the reaction rate to ensure sufficient chain extension and viscosity increase; (3) After the reaction is completed, add 0.5 parts of end-capping agent, 0.8 parts of stabilizer, and 5 parts of penetrant, and stir to disperse evenly; (4) The final product is subjected to a aging treatment to form a high-performance polyurethane resin product.

[0011] Beneficial effects: 1. The chain extender 1,6-hexanediol introduced in the present invention has a higher price than the original ethylene glycol material. Since the proportion used in the formula is very small, the cost increase is limited. Due to the particularity of this type of finished resin, the selling price is much higher than that of ordinary resins. Therefore, the increased cost does not affect the promotion and profit of the product.

[0012] 2. From the comparison of the two formulas, it can be seen that this new invention method does not increase the difficulty of production and does not prolong the production time.

[0013] 3. Through this invention, the wet-process bass produced can achieve the color-changing effect of pressing at 130°C, and can well protect the integrity after pressing. Compared with the ordinary bass that requires pressing conditions of 180°C or even 200°C, it protects the bass well and reduces the defective rate. Moreover, the logo after pressing is bright and clear, and it is very practical.

[0014] 4. After production verification, the output rate of qualified finished products after the modified formula process is equivalent to that of the original formula process. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The color changing effects of the three colors of group A in the embodiment of the present invention are shown below; Figure 2 The color changing effects of the three colors of group B in the embodiment of the present invention are shown below: Figure 3 This is the color change effect of the three colors of group C in the embodiment of the present invention. DETAILED DESCRIPTION

[0016] In order to make the above features and advantages of the present invention more clearly understood, the following embodiments are given for detailed description. The methods of the present invention are all conventional methods in the art unless otherwise specified.

[0017] Example 1 1. Raw material composition: The polyurethane resin formula of the present invention mainly includes the following components: - Polyol (Component A): The most commonly used polyester polyols in the market are PEBA2000 molecular weight and PEDA2000 molecular weight bifunctional polyols. These two polyols are widely representative and typical; PEBA2000 is a 2000 molecular weight polyol polymerized from adipic acid, ethylene glycol and 1,4-butanediol; PEDA2000 is a 2000 molecular weight polyol polymerized from adipic acid, ethylene glycol and diethylene glycol.

[0018] - Isocyanate (component B): 4,4'-diphenylmethane diisocyanate (MDI) -Chain extender (component C): Ethylene glycol (EG) and our new chain extender 1,6-hexanediol (1,6-HD) - Catalyst: Organic bismuth catalyst - Solvent: dimethylformamide (DMF) - Special additives: end-capping agent (methanol), stabilizer (malic acid), antioxidant (hindered phenol), penetrant (fatty alcohol polyoxyethylene ether) 2. Synthesis and test methods: formula: Two formulations were set to verify the effectiveness of the present invention. Formulation 1 selected the variety with the largest market usage as a reference comparison variety. Formulation 2, based on Formulation 1, changed the conventional one-step synthesis into a two-step synthesis, added a new chain extender, and then compared the pressing and discoloration effects. The same test was conducted in three groups: Formula 1: This is the mainstream formula used in the market.

[0019] Formula 2: This is an innovative and improved formula after calculation. If the new chain extender is added directly, the base produced by downstream customers will lose thickness too seriously and cannot be used at all. Therefore, we add a bulk polymerization reaction. First, the polyol reacts with MDI to increase its chain length, and then our new chain extender 1,6-HD is mixed with EG evenly, and then reacted with MDI to increase viscosity. The polyurethane resin produced can fully meet the production needs of downstream customers. Customers do not need to change any conditions. Use it with the original conditions to produce wet-process base that changes color at 130°C.

[0020] Synthesis process: Synthesis process of formula 1 - Add DMF, component A, component C and antioxidant into the reactor according to the indicated amount of the formula, preheat to 45°C, slowly add component B in batches, maintain the reaction at 75°C for 4 hours, then add the catalyst and react at 75°C for 1 hour, and increase the viscosity at a constant rate to a constant value.

[0021] - After prepolymerization to a suitable viscosity (300,000 cps / 75°C), gradually add solvent in proportion to control the reaction rate to ensure sufficient chain extension and viscosity increase.

[0022] - After the reaction is completed, add special additives (capping agent, stabilizer, penetrant) and disperse evenly by stirring.

[0023] - The final product is cured to form a high-performance polyurethane resin product.

[0024] The synthesis process of formula 2 - Preheat DMF and component A polyol to 45°C according to the indicated amount in the formula, then slowly add component B and maintain the reaction at 75°C for 2 hours. After completion, continue to add the indicated amount of DMF, antioxidant and component C (two mixed chain extenders), stir evenly after adding, add component B, maintain the reaction at 75°C for 2 hours, then add the catalyst, react at 75°C for 1 hour, and increase the viscosity at a constant rate to a constant value.

[0025] - After prepolymerization to a suitable viscosity (300,000 cps / 75°C), gradually add solvent in proportion to control the reaction rate to ensure sufficient chain extension and viscosity increase.

[0026] - After the reaction is completed, add special additives (capping agent, stabilizer, penetrant) and disperse evenly by stirring at low speed.

[0027] - The final product is cured to form a high-performance polyurethane resin product.

[0028] Processing: -Take 100 parts of the synthesized polyurethane resin, add 20 parts of wood powder and 10 parts of calcium carbonate powder (CaCO3), 80 parts of DMF solvent, and stir at high speed. -Let it stand for 5 minutes and use a centrifuge to remove air bubbles from the prepared slurry -Use 120 coating rods to evenly coat the base fabric - Place in 20% DMF aqueous solution to form -After forming, put it into the oven for drying -Crop - Select three colors that are easy to identify, set the pressing machine at 130℃, and compare the color change effect after pressing. The results are as follows Figure 1-Figure 3 shown.

[0029] Depend on Figure 1-Figure 3 The comparison clearly shows that the resin production method of the present invention is completely capable of changing color under 130°C pressing conditions, and the color changing effect is remarkable, and the logo is clear and bright.

[0030] The above content constitutes the basic framework and technical details of the present invention, which aims to fill the gap in the unique field of wet process resin. All equivalent changes and modifications made according to the scope of the patent application of the present invention shall fall within the scope of the present invention.

Claims

1. A wet low temperature pressing color changing polyurethane resin, characterized in that: The raw materials used include, by mass, 105 parts of polyester polyol PEBA-2000, 105 parts of polyester polyol PEDA-2000, 4 parts of ethylene glycol EG, 16 parts of chain extender 1,6-hexanediol, 75 parts of MDI, 700 parts of DMF, 0.5 parts of end capping agent, 0.8 parts of stabilizer, 0.05 parts of catalyst, 0.5 parts of antioxidant and 5 parts of penetrant.

2. The wet low temperature pressing color changing polyurethane resin according to claim 1, characterized in that: The end-capping agent is methanol.

3. The wet low temperature pressing color changing polyurethane resin according to claim 1, characterized in that: The catalyst is an organic bismuth catalyst.

4. The wet low temperature pressing color changing polyurethane resin according to claim 1, characterized in that: The antioxidant is a hindered phenol antioxidant.

5. The wet low temperature pressing color changing polyurethane resin according to claim 1, characterized in that: The stabilizer is malic acid.

6. The wet low temperature pressing color changing polyurethane resin according to claim 1, characterized in that: The penetrant is a fatty alcohol polyoxyethylene ether product.

7. The process for preparing the wet low temperature pressing color-changing polyurethane resin according to claim 1, characterized in that: The following steps are involved: (1) After preheating 180 parts of DMF, 105 parts of PEBA-2000 and 105 parts of PEDA-2000 to 45°C, slowly add 26 parts of MDI and maintain the reaction at 75°C for 2 hours; then continue to add 180 parts of DMF, 0.5 parts of antioxidant, 4 parts of EG, and 16 parts of 1,6-hexanediol, mix and stir evenly, add 49 parts of MDI, maintain the reaction at 75°C for 2 hours, then add 0.05 parts of catalyst, react at 75°C for 1 hour, and increase the viscosity at a constant rate to a constant value; (2) When the viscosity of the prepolymer reaches 300,000 cps / 75°C, 340 parts of DMF solvent are gradually added in proportion to control the reaction rate to ensure sufficient chain extension and viscosity increase; (3) After the reaction is completed, add 0.5 parts of end-capping agent, 0.8 parts of stabilizer, and 5 parts of penetrant, and stir to disperse evenly; (4) The final product is subjected to a aging treatment to form a high-performance polyurethane resin product.