Hydroxyl modified solid epoxy resin with controllable content and high activity and preparation method thereof
Through the preparation method of inorganic solvents, the high active hydroxyl content of solid epoxy resin is adjusted, and the problems of poor reactivity and insufficient heat exogenous are solved, and the preparation of high active epoxy resin is achieved, which meets the requirements of the coating industry and is environmentally friendly and suitable for large-scale processes. Large-scale production.
Patent Information
- Application Number
- CN202310608183.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-25
- Publication Date
- 2024-11-26
AI Technical Summary
The existing solid epoxy resin has poor reactivity and insufficient heat exogenous capacity, which cannot meet the coating anti-cathode peeling inspection standards, and the use of solvents in the process increases energy consumption and is not conducive to environmental protection.
By quantitatively adjusting the content of high-active hydroxyl groups on the surface of solid epoxy resin, using the preparation method of inorganic solvents, the synergistic action of curing agent and water improves the reaction activity, and controlling the reaction process to achieve the preparation of highly active hydroxyl-modified solid epoxy resin. .
The prepared epoxy resin has a viscosity of ≤4000mPa·s at 150°C, a hydrolyzed glycidyl group content of ≥16%, and an exothermic capacity of ≥50J/g. It meets the performance requirements of the coating industry, and has a simple process without organic waste liquid, which is suitable for industrial production. .
Smart Images

Figure BDA0004251625370000071 
Figure FDA0004251625360000021 
Figure FDA0004251625360000022
Abstract
Description
Technical Field
[0001] The invention relates to a hydroxyl-modified resin, in particular to a content-controllable high-activity hydroxyl-modified solid epoxy resin and a preparation method thereof, belonging to the field of epoxy resin material preparation. Background Art
[0002] With the development of my country's petroleum and chemical industry, a large number of pipeline projects have been started one after another, which has greatly promoted the development of pipeline anti-corrosion and the demand for heavy-duty anti-corrosion powder coatings has been increasing.
[0003] Epoxy powder coating is a kind of thermosetting functional coating. It forms a hard coating that cannot be melted after being heated, and the coating has good fluidity, so it has good decorative properties, excellent corrosion resistance, mechanical properties, and bonding properties. After testing, its bonding shear strength is more than 40 times higher than that of petroleum asphalt and tar coatings. However, with the development of the industry and the improvement of the coating anti-cathode stripping test standard, the solid epoxy resin produced by the existing process has poor reactivity and low heat release, and cannot meet the coating anti-cathode stripping test standard.
[0004] Wu Xige disclosed a high glass transition temperature and high toughness modified solid epoxy resin and its preparation method in patent CN104788648A, pointing out that the solid epoxy resin is prepared by using modifiers such as nitrile rubber and polyurethane. The epoxy coating prepared by the solid epoxy resin has a maximum glass transition temperature of 178°C and its toughness is improved.
[0005] Philip Carlberg disclosed a method for producing solid epoxy resin in patent CN103554431A, pointing out that a reaction solvent containing both aldehyde groups and alcohol groups is added to a reaction mixture of an aromatic hydroxyl-containing compound, epihalohydrin and an inorganic hydroxide to prepare the solid epoxy resin, and the method requires distillation to recover the solvent.
[0006] In summary, the existing solid epoxy resin production technology has not improved the low reactivity and insufficient heat release of solid epoxy resin, and solvents are still used in the process, which not only increases energy consumption but is also not conducive to environmental protection. Summary of the invention
[0007] In view of the problems existing in the prior art, the present invention provides a solid epoxy resin modified with a controllable content of highly active hydroxyl groups. Based on the synergistic effect between the components, the present invention quantitatively adjusts the content of highly active hydroxyl groups in the solid epoxy resin to obtain a highly active reactive solid epoxy resin. According to tests, the epoxy resin provided by the present invention has a viscosity of ≤4000 mPa·s at 150°C, a hydrolyzed glycidyl content of ≥16%, and a heat release of ≥50 J / g, which can meet the performance requirements of the coating industry.
[0008] The second object of the present invention is to provide a method for preparing a solid epoxy resin modified with a controllable content of highly active hydroxyl groups. This method controls the fluidity and molecular weight of the product by a curing agent without using an organic solvent, and then quantitatively regulates the active hydroxyl content on the surface of the epoxy resin under the synergistic effect of water, thereby greatly improving the reaction activity of the solid epoxy resin. This method has a simple process, does not generate organic waste liquid, is friendly to the ecological environment, and is suitable for large-scale industrial production.
[0009] To achieve the above technical objectives, the present invention provides a method for preparing a highly active hydroxyl-modified solid epoxy resin with controllable content. The method comprises the following steps: preheating a reaction kettle, removing air, adding a liquid epoxy agent, a curing agent, water and a catalyst to carry out a condensation reaction, and removing water after the reaction to obtain the solid epoxy resin; the liquid epoxy agent is a liquid epoxy resin having at least one glycidyl group per molecule; the curing agent is a compound having at least one phenolic hydroxyl group per molecule; the catalyst is any catalyst that can catalyze the ortho-position reaction between epoxy groups and phenolic hydroxyl groups; the molar ratio of the liquid epoxy agent to the curing agent is 1.2 to 30:1; the amount of the catalyst added is 0.1 to 10 mmol / mol per equivalent of epoxide in the liquid epoxy agent; and the amount of water added is 1.1 to 1.5 times the molar amount of the remaining epoxy groups after the liquid epoxy agent reacts with the curing agent.
[0010] The preparation method provided by the present invention does not use organic solvents throughout the entire process, and the reaction progress is controlled by controlling the reaction temperature and the addition ratio between the raw materials. The reaction temperature and the amount of curing agent added directly affect the fluidity of the phase during the reaction and the molecular weight of the resulting product. With the synergistic use of water, the directional regulation of the active hydroxyl groups on the surface of the epoxy resin is achieved. The overall process does not generate organic waste liquid and waste gas, and the resulting product has high reactivity, meeting the performance requirements of the downstream coating industry.
[0011] As a preferred solution, the molar ratio of the liquid epoxy agent to the curing agent is 1.4 to 10: 1. The amount of the liquid epoxy agent and the curing agent must be strictly implemented in accordance with the above requirements. If the amount of curing agent added is too low, the molecular weight of the obtained product is too low, and it is still in liquid state and difficult to form; while if the amount of curing agent added is too high, not only the molecular weight and viscosity of the product are too large, but also the surface hydroxylation modification process of the epoxy resin is affected, the contact between the resin and water is reduced, and the product cannot obtain enough active hydrolyzable hydroxyl groups, resulting in a significant decrease in the reaction activity and reaction heat of the epoxy resin.
[0012] As a preferred solution, the molar ratio of the liquid epoxy agent to the catalyst is 1 mol: 0.2-6 mmol.
[0013] As a preferred solution, the molar amount of water is 1.2 to 1.3 times the molar amount of the remaining epoxy group after the liquid epoxy agent reacts with the curing agent. The amount of water used must be strictly in accordance with the above requirements. In the present invention, water is used as a hydroxyl modifier on the surface of the epoxy resin. The greater the amount of water used, the greater the hydrolysis effect. However, the epoxy resin and water belong to different physical phases. Therefore, during the contact process, some water will not be able to participate in the hydroxylation reaction. Therefore, the amount of water used must be greater than the theoretical addition amount to ensure that the epoxy groups on the resin are completely hydrolyzed to obtain highly active hydroxyl groups.
[0014] As a preferred solution, the preheating temperature of the reactor is 85-95°C.
[0015] As a preferred solution, the method of excluding air from the reactor is: using nitrogen to completely remove air and then nitrogen sealing for 3 to 8 minutes.
[0016] As a preferred solution, the conditions of the condensation reaction are: temperature of 100-250° C. and time of 0.5-2.5 h.
[0017] As a preferred solution, the water removal method is one of vacuum stripping, high-temperature evaporation and inert gas purging.
[0018] As a preferred embodiment, the liquid epoxy agent is at least one of polyvalent aliphatic glycidyl ether, cycloaliphatic glycidyl ether, aromatic compound glycidyl ether and polyvalent carboxylic acid glycidyl ester.
[0019] As a preferred embodiment, the curing agent is at least one of aliphatic, cycloaliphatic and aromatic compounds having at least two phenolic hydroxyl groups.
[0020] As a preferred solution, the catalyst is at least one of a quaternary phosphorus compound, an ammonium compound and a halide.
[0021] As a preferred solution, the liquid epoxy agent is at least one of Formulas 1 to 3;
[0022] Formula 1:
[0023] Formula 2:
[0024] Formula 3:
[0025] In formulas 1 to 3: A is a divalent hydrocarbon group having 1 to 8 carbon atoms; X is hydrogen, bromine, chlorine or a hydrocarbon group having 1 to 8 carbon atoms; X' is hydrogen, bromine, chlorine or a hydrocarbon group having 1 to 8 carbon atoms; the value of n is 0 or 1; the value of n' is ≤0.9; the value of n" is 0.001 to 5. More preferably, in formulas 1 to 3: the value of n' is 0.001 to 0.15, and the value of n" is 0.1 to 2.5. Since the overall reaction process of the present invention does not contain an organic solvent, the fluidity of the liquid epoxy agent must be strictly required. The larger the values of n' and n", the worse the fluidity of the epoxy agent, and the effective contact area will be greatly reduced in the subsequent reaction process. In addition, the fluidity of the epoxy agent gradually decreases as the curing reaction proceeds. Therefore, the uniform dispersion of each material must be ensured by the fluidity of the liquid epoxy group at the initial stage of the reaction to ensure the controllability and uniformity of the hydroxyl groups in the subsequent product.
[0026] As a preferred solution, the curing agent is at least one of Formulas 4 to 6;
[0027] Formula 4:
[0028] Formula 5:
[0029] Formula 6:
[0030] In formulae 4 to 6: A is a divalent hydrocarbon group having 1 to 8 carbon atoms; X is hydrogen, bromine, chlorine or a hydrocarbon group having 1 to 8 carbon atoms; X' is hydrogen, bromine, chlorine or a hydrocarbon group having 1 to 8 carbon atoms; the value of n is 0 or 1; the value of n' is ≤0.9; the value of n" is 0.001 to 5.
[0031] As a preferred embodiment, the catalyst is at least one of ethyltriphenylphosphonium chloride, ethyltriphenylphosphonium bromide, methyltriphenylphosphonium iodide, ethyltriphenylphosphonium acetate, ethyltriphenylphosphonium diacetate, tetrabutylphosphonium chloride, tetrabutylphosphonium bromide, tetrabutylphosphonium iodide, tributylphosphonium acetate, tetrabutylphosphonium diacetate, benzyltrimethylammonium chloride, tetramethylammonium hydroxide, Lewis acid, boron trifluoride, tin chloride, aluminum chloride, ferric chloride bromide dealumination, zinc chloride, silicon tetrachloride and titanium tetrachloride.
[0032] As a preferred solution, the water removal method is vacuum stripping, and the conditions are: vacuum degree is 10-50 kPa, temperature is 150-200° C., and time is 0.4-0.6 h.
[0033] The present invention also provides a highly active hydroxyl-modified solid epoxy resin with controllable content, obtained by any of the above-mentioned preparation methods, wherein each molecule of the solid epoxy resin contains at least one hydrolyzed glycidyl group, and the structure of the glycidyl group is Formula 9;
[0034] Formula 9:
[0035] As a preferred solution, the viscosity of the solid epoxy resin is ≤4000 mPa·s, the hydrolyzed glycidyl content is ≥16%, and the heat release is ≥50 J / g.
[0036] Compared with the prior art, the beneficial effects of the technical solution of the present invention are:
[0037] 1) The hydroxyl-modified solid epoxy resin provided by the present invention is based on the synergistic effect between the components, and the content of highly active hydroxyl groups on the surface of the solid epoxy resin is quantitatively adjusted to obtain a highly active reactive solid epoxy resin. According to tests, the epoxy resin provided by the present invention has a viscosity of ≤4000 mPa·s at 150°C, a hydrolyzed glycidyl content of ≥16%, and a heat release of ≥50 J / g, which can meet the performance requirements of the coatings industry.
[0038] 2) In the preparation method of the hydroxyl-modified solid epoxy resin provided by the present invention, the fluidity and molecular weight of the product are controlled by a curing agent without using an organic solvent, and the active hydroxyl content on the surface of the epoxy resin is quantitatively controlled under the synergistic effect of water, thereby greatly improving the reaction activity of the solid epoxy resin; the method has a simple process, does not generate organic waste liquid, is friendly to the ecological environment, and is suitable for large-scale industrial production. DETAILED DESCRIPTION
[0039] The present invention is illustrated by the following examples, which are not intended to limit the scope or implementation of the present invention.
[0040] In the following examples, the viscosity was measured using the NDJ-8S type produced by Shanghai Precision Scientific Instrument Co., Ltd.; the heat release was measured using the American Perkin Elmer Q2000 liquid gel permeation chromatograph (GPC); and the softening point was measured using a METTLER TOLEDO DP70 softening point tester. All indicators were measured according to the Q / SH 1085 007-2020 standard.
[0041] Example 1
[0042] Preheat the reactor to 90±5℃ and introduce 20m 3 / h of N2, after keeping nitrogen blanket for 5 minutes, 736g of bisphenol A diglycidyl ether with an epoxy equivalent weight (EEW) of about 184, 264g of bisphenol A and 50g of water were added, and 0.5g of ethyl triphenylphosphine diacetate solution catalyst was used as a catalyst for the reaction between epoxy resin and bisphenol A to prepare a series of high molecular weight epoxy resins. The reaction was continued at 140°C for 2 hours, and then unreacted water was removed by vacuum stripping at 190°C for about 30 minutes. The physical and chemical properties of the obtained products are shown in Table 1.
[0043] Example 2
[0044] The reaction process of this embodiment is exactly the same as that of Example 1, the only difference being: 755.5 g of bisphenol A diglycidyl ether, 244.5 g of bisphenol A and 75 g of water. The physicochemical properties of the obtained product are shown in Table 1.
[0045] Example 3
[0046] The reaction process of this embodiment is exactly the same as that of embodiment 1, the only difference being: 755.5 g of bisphenol A diglycidyl ether, 244.5 g of bisphenol A and 93 g of water. The physicochemical properties of the obtained product are shown in Table 1.
[0047] Comparative Example 1
[0048] The reaction process of this embodiment is exactly the same as that of Example 1, the only difference being: 755.5 g of bisphenol A diglycidyl ether, 244.5 g of bisphenol A and 20 g of water. The physicochemical properties of the obtained product are shown in Table 1.
[0049] Comparative Example 2
[0050] Preheat the reactor to 90±5℃ and introduce 20m 3 / h of N2, keep nitrogen sealing for 5min, then put 714.5g of bisphenol A diglycidyl ether and 14.1g of bisphenol A2 into the reactor, add 0.41g of diacetate ethyl triphenyl phosphine solution catalyst for the first time when the temperature rises to 120℃, continue to rise to 160±5℃, maintain stirring and dissolving reaction at this temperature for 2.5 hours. After cooling the temperature to 140℃, add 71.4g of bisphenol A again, and add 0.14g of diacetate ethyl triphenyl phosphine solution for the second time after bisphenol A is completely dissolved. Heat to 180±5℃, react for 2 hours, and start sampling and analyzing the epoxy equivalent. After the epoxy equivalent analysis is qualified, the solid resin is obtained. The number of reactants and experimental results are shown in Table 1.
[0051] Comparative Example 3
[0052] This comparative example is exactly the same as comparative example 4, the only difference being that the amount of bisphenol A diglycidyl ether added is 755.5 g, the amount of bisphenol A added for the first time is 228.75 g, the amount of catalyst added for the first time is 0.43 g, the amount of bisphenol A added for the second time is 76.35 g, and the amount of catalyst added for the second time is 0.15 g.
[0053] Table 1
[0054]
[0055] Table 1 is a table of the raw material dosage and the physicochemical properties of the obtained products in Examples 1 to 3 and Comparative Examples 1 to 3. It can be seen from Examples 1 to 3 that when the amount of water used exceeds the theoretical amount, as the amount of water increases, the number of highly reactive hydroxyl groups contained in the obtained product also increases. It can be seen from Examples 2, 3 and Comparative Example 1 that if the amount of water added does not exceed the theoretical amount of water added, it is impossible to effectively quantitatively adjust the number of active hydroxyl groups in the product. Therefore, only by strictly complying with the technical solution provided by the present invention can a solid epoxy resin with high reactivity that meets the performance requirements of the downstream coating industry be obtained.
Claims
1. A method for preparing a solid epoxy resin with controllable content and high activity hydroxyl group, characterized in that: After preheating the reactor, the air is removed, and liquid epoxy agent, curing agent, water and catalyst are added to carry out condensation reaction. After the reaction is completed, water is removed to obtain; The liquid epoxy agent is a liquid epoxy resin having at least one glycidyl group per molecule; the curing agent is a compound having at least one phenolic hydroxyl group per molecule; and the catalyst is any catalyst that can catalyze the ortho-position reaction between epoxy groups and phenolic hydroxyl groups; The molar ratio of the liquid epoxy agent to the curing agent is 1.2 to 30:1; the added amount of the catalyst is 0.1 to 10 mmol / mol per equivalent of epoxide in the liquid epoxy agent; and the added amount of water is 1.1 to 1.5 times the molar amount of the remaining epoxy group after the liquid epoxy agent reacts with the curing agent.
2. The method for preparing a solid epoxy resin with controllable content and high activity hydroxyl group according to claim 1, characterized in that: The molar ratio of the liquid epoxy agent to the curing agent is 1.4-10:1; the molar ratio of the liquid epoxy agent to the catalyst is 1 mol: 0.2-6 mmol; the molar amount of water is 1.2-1.3 times the molar amount of the remaining epoxy group after the liquid epoxy agent reacts with the curing agent.
3. The method for preparing a solid epoxy resin with controllable content and high activity hydroxyl group according to claim 1, characterized in that: The preheating temperature of the reactor is 85-95° C., and the method of exhausting air from the reactor is: using nitrogen to exhaust air to completely remove air and then nitrogen sealing for 3-8 minutes.
4. The method for preparing a solid epoxy resin with controllable content and high activity hydroxyl group according to claim 1, characterized in that: The conditions of the condensation reaction are: temperature of 100-250° C., time of 0.5-2.5 h; the water removal method is one of vacuum stripping, high-temperature evaporation and inert gas purging.
5. The method for preparing a solid epoxy resin with controllable content and high activity hydroxyl group according to claim 1, characterized in that: The liquid epoxy agent is at least one of polyhydric aliphatic glycidyl ether, cycloaliphatic glycidyl ether, aromatic compound glycidyl ether and polyhydric carboxylic acid glycidyl ester.
6. The method for preparing a solid epoxy resin with controllable content and high activity hydroxyl group according to claim 1, characterized in that: The curing agent is at least one of aliphatic, cycloaliphatic and aromatic compounds having at least two phenolic hydroxyl groups; the catalyst is at least one of quaternary phosphorus compounds, ammonium compounds and halides.
7. The method for preparing a solid epoxy resin with controllable content and high activity hydroxyl group according to claim 1, characterized in that: The liquid epoxy agent is at least one of formulas 1 to 3; Formula 1: Formula 2: Formula 3: In formulas 1 to 3: A is a divalent hydrocarbon group having 1 to 8 carbon atoms; X is hydrogen, bromine, chlorine or a hydrocarbon group having 1 to 8 carbon atoms; X' is hydrogen, bromine, chlorine or a hydrocarbon group having 1 to 8 carbon atoms; the value of n is 0 or 1; the value of n' is ≤0.9; the value of n" is 0.001 to 5.
8. The method for preparing a solid epoxy resin with controllable content and high activity hydroxyl group according to claim 1, characterized in that: The curing agent is at least one of formulas 4 to 6; Formula 4: Formula 5: Formula 6: In formulae 4 to 6: A is a divalent hydrocarbon group having 1 to 8 carbon atoms; X is hydrogen, bromine, chlorine or a hydrocarbon group having 1 to 8 carbon atoms; X' is hydrogen, bromine, chlorine or a hydrocarbon group having 1 to 8 carbon atoms; the value of n is 0 or 1; the value of n' is ≤0.9; the value of n" is 0.001 to 5.
9. The method for preparing a solid epoxy resin with controllable content and high activity hydroxyl group according to claim 1, characterized in that: The catalyst is at least one of ethyltriphenylphosphonium chloride, ethyltriphenylphosphonium bromide, methyltriphenylphosphonium iodide, ethyltriphenylphosphonium acetate, ethyltriphenylphosphonium diacetate, tetrabutylphosphonium chloride, tetrabutylphosphonium bromide, tetrabutylphosphonium iodide, tributylphosphonium acetate, tetrabutylphosphonium diacetate, benzyltrimethylammonium chloride, tetramethylammonium hydroxide, Lewis acid, boron trifluoride, tin chloride, aluminum chloride, ferric chloride bromide dealumination, zinc chloride, silicon tetrachloride and titanium tetrachloride.
10. The method for preparing a solid epoxy resin with controllable content and high activity hydroxyl group according to claim 1, characterized in that: The water removal method is vacuum stripping, and the conditions are: vacuum degree is 10-50 kPa, temperature is 150-200° C., and time is 0.4-0.6 h.
11. A solid epoxy resin modified with a controllable content of highly active hydroxyl groups, characterized in that: The solid epoxy resin obtained by the preparation method according to any one of claims 1 to 10 contains at least one hydrolyzed glycidyl group per molecule, and the structure of the glycidyl group is Formula 9; Formula 9:
12. The highly active hydroxyl-modified solid epoxy resin with controllable content according to claim 11, characterized in that: The solid epoxy resin has a viscosity of ≤4000 mPa·s, a hydrolyzed glycidyl content of ≥16%, and a heat release of ≥50 J / g.
Citation Information
Patent Citations
Modifying method of solid epoxy resin
CN105061728A
Epoxy resin composition capable of cure at low temperature
CN1175265A
Method for preparing high molecular weight epoxy resins containing hydrolyzed epoxy groups
US4340713A
Method for preparing high molecular weight epoxy resins containing hydrolyzed epoxy groups
US4358577A
Method for preparing high molecular weight epoxy resins containing hydrolyzed glycidyl groups
WO1982001878A1