Cycloolefin polymer and preparation method thereof
The reaction conditions are controlled during the preparation of cycloolefin polymers through the ruthenium catalyst, and the problems of wide molecular weight distribution and poor optical performance are solved, thereby achieving economical, efficient and controllable preparation of cycloolefin polymers with good performance.
Patent Information
- Application Number
- CN202411515210.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-10-29
AI Technical Summary
During the preparation process, cycloolefin polymers have problems such as wide molecular weight distribution and poor optical properties. In particular, the high cost of Ru-based catalysts and the excessive viscosity of the polymerization system lead to uncontrollable quality.
The cycloolefin polymer is prepared by using a ruthenium catalyst. The ring-opening polymerization and hydrogenation reaction are carried out by preheating the cycloolefin monomer, chain transfer agent and catalyst solution, and the reaction conditions are controlled to obtain polymers with controllable molecular weight and good optical properties. .
The cycloolefin polymer with good performance is achieved economically, efficiently and controllable, the amount of Ru-based catalyst is used, the production cost is reduced, and the molecular weight is narrow, the thermal stability and optical performance are improved.
Smart Images

Figure CN119019649A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a cycloolefin polymer and a preparation method thereof, belonging to the field of cycloolefin polymers. Background Art
[0002] Cyclic olefin polymer, referred to as COP, is a polymer material obtained by ring-opening polymerization of cycloolefin monomers and then hydrogenation. It has the advantages of high light transmittance, low birefringence, high water vapor barrier, etc., and has good application prospects in the fields of optical lenses, medical packaging, electronic devices, etc. However, due to factors such as the preparation process of cycloolefin polymers, cycloolefin polymers generally have defects such as wide molecular weight distribution and poor optical properties.
[0003] For example, the catalysts used for the ring-opening polymerization of cycloolefins mainly include W, Mo-based catalysts and Ru-based catalysts. For example, the patent document with publication number CN1186080A discloses a method for preparing cycloolefin polymers using a ruthenium-based catalyst (Ru-based catalyst), and the polymerization and hydrogenation are simultaneously completed using the Ru-based catalyst; the patent document with publication number CN117417512A discloses a method for preparing cycloolefin polymers using W and Mo-based catalysts, and the obtained cycloolefin polymers can be used in the field of medical packaging; the patent document with publication number CN117050276A discloses a method for preparing a tetracyclo[6.2.1.13,6.02,7]dodec-4ene ring-opening polymer, using a W-based catalyst as a ring-opening polymerization catalyst and a Ru-based catalyst as a hydrogenation catalyst.
[0004] Compared with W and Mo catalysts, Ru catalysts have better tolerance to water, oxygen and functional groups (for example, as described in the following non-patent literature: Kong Yong, Yang Xiaohua, Wang Lin, et al. Research Progress in Ring-Opening Metathesis Polymerization [J]. Science, Technology and Engineering, 2015, 15(30): 71-78), and can be used for both polymerization and hydrogenation processes, which greatly reduces the difficulty and cost of operation. However, the high cost of Ru catalysts limits their industrial application, and although Ru catalysts are extremely active, too little addition of Ru catalysts will result in too high viscosity of the polymerization system, making the polymerization process difficult to control, and too wide a molecular weight distribution of the polymer, making the quality of the polymer uncontrollable. Even if a large amount of chain transfer agent is added, it is difficult to completely solve the above problems. Summary of the invention
[0005] The present invention provides a cycloolefin polymer and a preparation method thereof. The method uses a ruthenium-based catalyst (Ru-based catalyst) to prepare the cycloolefin polymer, and can obtain a cycloolefin polymer with controllable molecular weight, narrow molecular weight distribution, and good optical properties, thereby realizing economical, efficient, and controllable preparation of the cycloolefin polymer with good performance.
[0006] The invention provides a method for preparing a cycloolefin polymer, comprising the following steps: respectively preparing a solution of a cycloolefin polymer monomer, a solution of a chain transfer agent, and a solution of a ruthenium-based catalyst; respectively preheating the solution of the cycloolefin polymer monomer, the solution of the chain transfer agent, and the solution of the ruthenium-based catalyst to 45-200° C.; mixing the preheated solution of the cycloolefin polymer monomer, the solution of the chain transfer agent, and the solution of the ruthenium-based catalyst to obtain a mixed solution, and subjecting the mixed solution to a ring-opening polymerization reaction at 45-250° C., wherein the time for the ring-opening polymerization reaction is 5-65 minutes; after the ring-opening polymerization reaction is completed, adding a hydrogen source to the mixed solution for a hydrogenation reaction, wherein the time for the hydrogenation reaction is 6-12 hours; after the hydrogenation reaction is completed, sequentially adding a terminator, an adsorbent, and a poor solvent to the mixed solution to separate and obtain the cycloolefin polymer.
[0007] Optionally, the cycloolefin polymer monomer includes one or more of the compound represented by formula (1) and the compound represented by formula (2): Formula (1) Formula (2), In the formula (1), R 1 ~R 4 are independently selected from a hydrogen atom, a halogen atom, an alkyl group having 1 to 15 carbon atoms, a cycloalkyl group, an aryl group having 6 to 10 carbon atoms with a substituent, or a substituent containing a first heteroatom; in the formula (2), R 5 ~R 6 are each independently selected from an alkyl group having 1 to 15 carbon atoms, a substituted or unsubstituted aryl group having 6 to 10 carbon atoms, or a substituent containing a second heteroatom, R 7 is selected from an alkyl group having 1 to 15 carbon atoms, a substituted or unsubstituted aryl group having 6 to 12 carbon atoms, or a substituent containing a third heteroatom, R 8 ~R 9 Each is independently selected from a hydrogen atom, a halogen atom, an alkyl group having 1 to 15 carbon atoms, a substituted or unsubstituted aryl group having 6 to 10 carbon atoms, or a substituent containing a fourth heteroatom; And / or, the chain transfer agent includes olefins and / or halogenated olefins having a carbon number of 3 to 30; and / or, the concentration of the cycloolefin polymer monomer in the solution of the cycloolefin polymer monomer is 0.001 to 10 mol / L; and / or, the concentration of the chain transfer agent in the solution of the chain transfer agent is 0.001 to 10 mol / L; and / or, the concentration of ruthenium element in the solution of the ruthenium-based catalyst is 0.001 to 10 mol / L.
[0008] Optionally, in the formula (1), R 1 and R 2are combined with each other to form a ring; and / or, in the formula (1), the first heteroatom includes one or more of a silicon atom, a nitrogen atom, and an oxygen atom; and / or, in the formula (2), the second heteroatom includes one or more of a silicon atom, a nitrogen atom, and an oxygen atom; the third heteroatom includes one or more of a silicon atom, a nitrogen atom, and an oxygen atom; the fourth heteroatom includes one or more of a silicon atom, a nitrogen atom, and an oxygen atom.
[0009] Optionally, the compound represented by formula (1) includes tetracyclododecene, 8-methyltetracyclododecene, 8-ethyltetracyclododecene, 8-isopropyltetracyclododecene, 8-n-butyltetracyclododecene, 8-isobutyltetracyclododecene, 8-cyclopentyltetracyclododecene, 8-cyclohexyltetracyclododecene, 8-chlorotetracyclododecene, 8-bromotetracyclododecene, 8-methoxytetracyclododecene, 8-carbonyltetracyclododecene, 8-hydroxytetracyclododecene, 8-carboxytetracyclododecene, 8-aminotetracyclododecene, 8-phenoxytetracyclododecene, 8 One or more of cyanotetracyclododecene, 8-phenyltetracyclododecene, 12-methyltetracyclododecene, 12-phenoxytetracyclododecene, and 12-chlorotetracyclododecene; and / or, the compound represented by formula (2) includes 5-norbornene-2,3-dicarboxylic anhydride, 5-norbornene-2,3-dicarboximide, methyl-5-norbornene-2,3-dicarboxylic anhydride, ethyl-5-norbornene-2,3-dicarboxylic anhydride, isopropyl-5-norbornene-2,3-dicarboxylic anhydride, isobutyl-5-norbornene-2,3-dicarboxylic anhydride, cyclohexyl-5-norbornene-2,3-dicarboxylic anhydride, methyl-5-norbornene-2,3-dicarboxylic anhydride, One or more of norbornene-2,3-dicarboximide, ethyl-5-norbornene-2,3-dicarboximide, isopropyl-5-norbornene-2,3-dicarboximide, isobutyl-5-norbornene-2,3-dicarboximide, N-hydroxy-5-norbornene-2,3-dicarboximide, N-phenyl-5-norbornene-2,3-dicarboximide, N-benzyl-5-norbornene-2,3-dicarboximide, N-naphthyl-5-norbornene-2,3-dicarboximide, norbornene-2,3-dicarboximido tert-butyl carbonate, norbornene-2,3-dicarboximido p-nitrobenzyl carbonate; And / or, the chain transfer agent includes one or more of aliphatic olefins, aromatic olefins, and halogenated olefins; the aliphatic olefins include one or more of 1-pentene, 2-pentene, 1-hexene, 2-hexene, 4-octene, 1-octene, and 1-heptene; the aromatic olefins include one or more of styrene, triphenylethylene, 4-phenyl-1-butene, and 6-phenyl-1-hexene; the halogenated olefins include one or more of 4-bromo-1-butene, 2-bromo-2-butene, 6-bromo-1-hexene, 5,6-dibromo-1-hexene, 6-chloro-1-hexene, and 8-chloro-1-octene.
[0010] Optionally, in the mixed solution, the molar ratio of the cycloolefin polymer monomer to the ruthenium element is 1:(1×10 -5 ~5×10 -4 ); and / or, in the mixed solution, the molar ratio of the cycloolefin polymer monomer to the chain transfer agent is 1: (1×10 -4 ~5×10 -2 ); and / or, the temperature of the ring-opening polymerization reaction is greater than or equal to the preheating temperature; and / or, the pressure of the ring-opening polymerization reaction is 0.1 to 5 MPa.
[0011] Optionally, the hydrogen source includes hydrogen and / or hydrazine compounds; the hydrazine compounds include one or more of hydrazine, phenylhydrazine, formic hydrazide, acetic hydrazide, valeryl hydrazide, hexyl hydrazide, benzenesulfonyl hydrazide, p-toluenesulfonyl hydrazide, and phenylmethylsulfonyl hydrazide; and / or, the temperature of the hydrogenation reaction is -10 to 210°C, and the pressure of the hydrogenation reaction is 0.05 to 15 MPa.
[0012] Optionally, the terminator includes an olefin with a carbon number of 3 to 30 containing a sixth heteroatom, wherein the sixth heteroatom includes one or more of an oxygen atom, a nitrogen atom, a silicon atom, a sulfur atom, and a halogen atom; and / or, the adsorbent includes one or more of thiourea resin, activated carbon, silica gel, diatomaceous earth, and alumina; and / or, the poor solvent includes one or more of an alcohol solvent, an aldehyde ketone solvent, an ether solvent, and a phenol solvent; the alcohol solvent includes one or more of methanol, ethanol, isopropanol, ethylene glycol, and n-butanol; the aldehyde ketone solvent includes one or more of acetone, methyl acetone, bromoacetone, propionaldehyde, and isobutyraldehyde; the ether solvent includes one or more of ethyl ether, methyl ethyl ether, dibutyl ether, and tetrahydrofuran; the phenol solvent includes one or more of phenol, o-cresol, and propofol.
[0013] Optionally, the terminator includes one or more of 1,1-diethoxyethylene, 1-bromo-2-ethoxyethylene, methoxyethylene, ethoxyethylene, 2-methoxypropylene, 3,3-dimethoxypropylene, 3-methoxyacrylic acid, ethyl propylene ether, and 3-ethoxyacrylic acid; and / or, after the hydrogenation reaction is terminated, the terminator, the adsorbent and the poor solvent are sequentially added to the mixed solution, and the process of separating and obtaining the cycloolefin polymer includes: after the hydrogenation reaction is terminated, the terminator is added to the mixed solution, and the temperature of the mixed solution is controlled to be 45 to 250° C., and the temperature of the mixed solution is controlled to be greater than or equal to the temperature of the ring-opening polymerization reaction, and after 1 to 60 minutes; the adsorbent is added thereto to remove the ruthenium catalyst; and then the poor solvent is added thereto dropwise to make the The cycloolefin polymer is precipitated and separated to obtain the cycloolefin polymer; wherein the molar ratio of the terminator to the ruthenium element in the mixed solution is (1-100):1; and / or, after the hydrogenation reaction is terminated, the terminator, the adsorbent and the poor solvent are sequentially added to the mixed solution to separate the cycloolefin polymer. The process includes: after the hydrogenation reaction is terminated, the terminator solution, the adsorbent and the poor solvent solution are sequentially added to the mixed solution to separate the cycloolefin polymer; wherein the concentration of the terminator in the terminator solution is 0.001-10 mol / L; the poor solvent solution includes a pH adjuster, and the pH adjuster includes one or more of hydrochloric acid, sulfuric acid, lactic acid, acetic acid, sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide and potassium carbonate.
[0014] The present invention also provides a cycloolefin polymer obtained according to the preparation method described above.
[0015] Optionally, the cycloolefin polymer has a glass transition temperature of 100 to 300° C., a hydrogenation rate of unsaturated bonds of not less than 95%, and a refractive index of 1.5 to 2.1.
[0016] The present invention provides a cycloolefin polymer and a preparation method thereof. The cycloolefin polymer is prepared by preheating a solution of a cycloolefin polymer monomer, a solution of a chain transfer agent and a solution of a ruthenium catalyst respectively, and then mixing them to carry out a ring-opening polymerization reaction, a hydrogenation reaction and the like. This is beneficial to reducing the amount of the ruthenium catalyst without affecting the quality of the cycloolefin polymer, and is helpful to reducing production costs, thereby obtaining a cycloolefin polymer with controllable molecular weight, narrow molecular weight distribution, good thermal stability and good optical properties, thereby realizing economical, efficient and controllable preparation of a cycloolefin polymer with good performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1is a high temperature gel permeation chromatogram of the cycloolefin polymer obtained in Example 1 (the left ordinate dNf / dLogM refers to the number distribution of polymer chains in different molecular weight ranges, the abscissa LogM refers to the logarithmic value of the molecular weight, and the right ordinate SCB / 1000TC refers to the number of short chain branches per 1000 carbon atoms); Figure 2 It is a high temperature gel permeation chromatogram of the cycloolefin polymer obtained in Comparative Example 1 (the left ordinate dNf / dLogM refers to the number distribution of polymer chains in different molecular weight ranges, the abscissa LogM refers to the logarithmic value of the molecular weight, and the right ordinate SCB / 1000TC refers to the number of short chain branches per 1000 carbon atoms). DETAILED DESCRIPTION
[0018] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] The embodiment of the present invention provides a method for preparing a cycloolefin polymer, comprising the following steps: respectively preparing a solution of a cycloolefin polymer monomer, a solution of a chain transfer agent, and a solution of a ruthenium-based catalyst; respectively preheating the solution of the cycloolefin polymer monomer, the solution of the chain transfer agent, and the solution of the ruthenium-based catalyst to 45 to 200° C.; mixing the preheated solution of the cycloolefin polymer monomer, the solution of the chain transfer agent, and the solution of the ruthenium-based catalyst to obtain a mixed solution, and subjecting the mixed solution to a ring-opening polymerization reaction at 45 to 250° C., wherein the time for the ring-opening polymerization reaction is 5 to 65 minutes; after the ring-opening polymerization reaction is completed, adding a hydrogen source to the mixed solution for a hydrogenation reaction, wherein the time for the hydrogenation reaction is 6 to 12 hours; after the hydrogenation reaction is completed, sequentially adding a terminator, an adsorbent, and a poor solvent to the mixed solution to separate and obtain a cycloolefin polymer.
[0020] According to the inventor's research and analysis: preheating the solution of cycloolefin polymer monomer, the solution of chain transfer agent, and the solution of ruthenium catalyst (Ru catalyst) to 45-200°C respectively, and then mixing the above three preheated solutions for ring-opening polymerization reaction, is beneficial to reduce the amount of ruthenium catalyst without affecting the quality of cycloolefin polymer, which helps to reduce production costs, and at the same time obtain cycloolefin polymers with controllable molecular weight, narrow molecular weight distribution, and good optical properties, thereby realizing economical, efficient and controllable preparation of cycloolefin polymers with good performance.
[0021] The process of preparing the solution of the cycloolefin polymer monomer may at least include the following process: dissolving the cycloolefin polymer monomer in an inert solvent at room temperature (eg, 12-40° C.) to obtain the solution of the cycloolefin polymer monomer.
[0022] The process of preparing the chain transfer agent solution may at least include the following process: dissolving the chain transfer agent in an inert solvent at room temperature (eg, 12-40° C.) to obtain the chain transfer agent solution.
[0023] The process of preparing the solution of the ruthenium-based catalyst may at least include the following process: dissolving the ruthenium-based catalyst in an inert solvent at room temperature (eg, 12-40° C.) to obtain the solution of the ruthenium-based catalyst.
[0024] The above-mentioned process of preparing the solution of cycloolefin polymer monomer, the solution of chain transfer agent and the solution of ruthenium catalyst can be carried out under the protection of inert gas. In specific implementation, a flask can be used as a container and the above-mentioned preparation process can be carried out in a glove box.
[0025] The embodiment of the present invention does not particularly limit the above-mentioned inert solvent. The above-mentioned inert solvent only needs to be a solvent that can dissolve or disperse the cycloolefin polymer and does not affect various reactions such as the ring-opening polymerization reaction. For example, the inert solvent may include one or more of aliphatic hydrocarbons, alicyclic hydrocarbons, aromatic hydrocarbons, halogenated aliphatic hydrocarbons, nitrogen-containing hydrocarbons, and ethers. Specifically, the aliphatic hydrocarbons may include one or more of pentane, hexane, heptane, 2,4-dimethylpentane, and 3-methylhexane, the alicyclic hydrocarbons may include one or more of cyclopentane, cyclohexane, cycloheptane, cyclodecane, methylcyclohexane, and cyclooctane, the aromatic hydrocarbons may include one or more of benzene, toluene, xylene, and butylbenzene, the halogenated aliphatic hydrocarbons may include one or more of dichloromethane, chloroform, and 1,2-dichloroethane, the nitrogen-containing hydrocarbons may include one or more of nitromethane, nitrobenzene, and acetonitrile, the ethers may include one or more of ethyl ether, dibutyl ether, and tetrahydrofuran, preferably, the above-mentioned inert solvent may include one or more of toluene, xylene, pentane, hexane, cyclopentane, and cyclohexane.
[0026] The concentration of the cycloolefin polymer monomer in the solution of the cycloolefin polymer monomer may be 0.001 to 10 mol / L, for example, 0.001 mol / L, 0.01 mol / L, 1 mol / L, 2 mol / L, 3 mol / L, 5 mol / L, 7 mol / L, 9 mol / L, 10 mol / L or a range consisting of any two thereof, preferably 0.01 to 5 mol / L.
[0027] The concentration of the chain transfer agent in the solution of the chain transfer agent can be 0.001 to 10 mol / L, for example, 0.001 mol / L, 0.01 mol / L, 1 mol / L, 2 mol / L, 3 mol / L, 5 mol / L, 7 mol / L, 9 mol / L, 10 mol / L or a range consisting of any two thereof, preferably 0.01 to 5 mol / L.
[0028] The concentration of ruthenium element in the solution of the above-mentioned ruthenium-based catalyst can be 0.001~10 mol / L, for example, 0.001 mol / L, 0.01 mol / L, 1 mol / L, 2 mol / L, 3 mol / L, 5 mol / L, 7 mol / L, 9 mol / L, 10 mol / L or a range composed of any two of them, preferably 0.01~5 mol / L.
[0029] In some embodiments, the cycloolefin polymer monomer includes one or more of the compound represented by formula (1) and the compound represented by formula (2): Formula (1) Formula (2), In formula (1), R 1 ~R 4 are independently selected from a hydrogen atom, a halogen atom, an alkyl group having 1 to 15 carbon atoms, a cycloalkyl group, an aryl group having 6 to 10 carbon atoms and a substituent group containing a first heteroatom; in formula (2), R 5 ~R 6 are each independently selected from an alkyl group having 1 to 15 carbon atoms, a substituted or unsubstituted aryl group having 6 to 10 carbon atoms, or a substituent containing a second heteroatom, R 7 is selected from an alkyl group having 1 to 15 carbon atoms, a substituted or unsubstituted aryl group having 6 to 12 carbon atoms, or a substituent containing a third heteroatom, R 8 ~R 9 Each is independently selected from a hydrogen atom, a halogen atom, an alkyl group having 1 to 15 carbon atoms, a substituted or unsubstituted aryl group having 6 to 10 carbon atoms, or a substituent containing a fourth heteroatom. In the system of the preparation method of the embodiment of the present invention, the cycloolefin polymer monomer can ensure that a cycloolefin polymer with controllable molecular weight, narrow molecular weight distribution, and good optical properties is obtained under the premise of using a small amount of ruthenium-based catalyst.
[0030] In formula (1), R 1 , R 2 They may be combined to form a ring or not; the first heteroatom may include one or more of a silicon atom, a nitrogen atom, and an oxygen atom. In formula (2), the second heteroatom, the third heteroatom, and the fourth heteroatom each independently include one or more of a silicon atom, a nitrogen atom, and an oxygen atom.
[0031] Specifically, the compound represented by the above formula (1) may include tetracyclododecene, 8-methyltetracyclododecene, 8-ethyltetracyclododecene, 8-isopropyltetracyclododecene, 8-n-butyltetracyclododecene, 8-isobutyltetracyclododecene, 8-cyclopentyltetracyclododecene, 8-cyclohexyltetracyclododecene, 8-chlorotetracyclododecene, 8-bromotetracyclododecene, 8-methoxytetracyclododecene, 8-carbonyltetracyclododecene, 8-hydroxytetracyclododecene, 8-carboxytetracyclododecene, 8-aminotetracyclododecene, 8-phenoxytetracyclododecene, 8-hydroxy- ... One or more of cyanotetracyclododecene, 8-phenyltetracyclododecene, preferably one or more of tetracyclododecene, 8-methyltetracyclododecene, 8-ethyltetracyclododecene, -isopropyltetracyclododecene, 8-n-butyltetracyclododecene, 8-isobutyltetracyclododecene, 8-phenyltetracyclododecene, 12-methyltetracyclododecene, 12-phenoxytetracyclododecene, and 12-chloro-tetracyclododecene.
[0032] Among them, the structural formula of 8-methyltetracyclododecene is shown in formula (1-1), the structural formula of tetracyclododecene is shown in formula (1-2), the structural formula of 8-chloro-tetracyclododecene is shown in formula (1-3), the structural formula of 8-phenoxytetracyclododecene is shown in formula (1-4), the structural formula of 12-methyltetracyclododecene is shown in formula (1-5), the structural formula of 12-phenoxytetracyclododecene is shown in formula (1-6), and the structural formula of 12-chloro-tetracyclododecene is shown in formula (1-7).
[0033] The compound represented by formula (2) may include 5-norbornene-2,3-dicarboxylic anhydride, 5-norbornene-2,3-dicarboximide, methyl-5-norbornene-2,3-dicarboxylic anhydride, ethyl-5-norbornene-2,3-dicarboxylic anhydride, isopropyl-5-norbornene-2,3-dicarboxylic anhydride, isobutyl-5-norbornene-2,3-dicarboxylic anhydride, cyclohexyl-5-norbornene -2,3-dicarboxylic anhydride, methyl-5-norbornene-2,3-dicarboximide, ethyl-5-norbornene-2,3-dicarboximide, isopropyl-5-norbornene-2,3-dicarboximide, isobutyl-5-norbornene-2,3-dicarboximide, N-hydroxy-5-norbornene-2,3-dicarboximide, N-phenyl-5-norbornene-2,3-dicarboximide One or more of amine, N-benzyl-5-norbornene-2,3-dicarboximide, N-naphthyl-5-norbornene-2,3-dicarboximide, norbornene-2,3-dicarboxyimino tert-butyl carbonate, norbornene-2,3-dicarboxyimino p-nitrobenzyl carbonate, preferably 5-norbornene-2,3-dicarboxylic anhydride, 5-norbornene-2,3-dicarboximide , methyl-5-norbornene-2,3-dicarboxylic anhydride, methyl-5-norbornene-2,3-dicarboximide, ethyl-5-norbornene-2,3-dicarboximide, N-phenyl-5-norbornene-2,3-dicarboximide, N-benzyl-5-norbornene-2,3-dicarboximide, and one or more of N-naphthyl-5-norbornene-2,3-dicarboximide.
[0034] Wherein, the structural formula of N-phenyl-5-norbornene-2,3-dicarboximide is shown in formula (2-1), and the structural formula of 5-norbornene-2,3-dicarboxylic anhydride is shown in formula (2-2).
[0035] Formula (2-1) Formula (2-2) In some embodiments, the ruthenium-based catalyst can be prepared according to the following process: 1 g of Grubbs second-generation catalyst [CAS: 246047-72-3] (Adamas Reagent Co., Ltd., purity 98%) is dissolved in 50 mL of dichloromethane (Adamas Reagent Co., Ltd., purity 99.9%) to obtain a first mixed solution; 1Dissolve in 30 mL of dichloromethane to prepare a solution to obtain a second mixed solution; then, mix the first mixed solution and the second mixed solution at 40°C, add 0.1 g of cuprous chloride (Adamas Reagent Co., Ltd., 98%), stir and react for 5 hours, let stand overnight at -30°C, and then filter to obtain a solid ruthenium catalyst. Among them, ligand B can be prepared according to the following process 1 : In a glove box, 1 g of 2-isopropoxystyrene (Sinopharm Chemical Reagent Co., Ltd., 97%) was dissolved in 10 mL of toluene to obtain a third mixed solution; 0.1 g of anhydrous aluminum chloride (Sinopharm Chemical Reagent Co., Ltd., 98%) was added to the third mixed solution, and then methyl chloride gas (Shanghai Weichuang Standard Gas Co., Ltd., 99%) was introduced to react for 3 h to obtain a reaction solution; then, the above reaction solution was added dropwise to 0.7 g of metallic lithium (Sinopharm Chemical Reagent Co., Ltd., 99%) at -78°C to obtain a toluene solution containing alkyl lithium; 2 mL of the toluene solution containing alkyl lithium was taken and added dropwise to 3 g of 3,5-dibromopyridine (Adamas Reagent Co., Ltd. (adamas), 98%), stirred for reaction for 3 h, and then recrystallized at -30°C, and the precipitated solid was the ligand B used. 1 .
[0036] In other embodiments, the ruthenium-based catalyst can be prepared according to the following process: 1 g of the second-generation grubbs catalyst [CAS: 246047-72-3] (Adamas Reagent Co., Ltd. (Adamas), 98%) is dissolved in 60 mL of toluene (Adamas Reagent Co., Ltd. (Adamas), 99.5%) to obtain a fourth mixed solution; in addition, ligand A is dissolved in 45 mL of toluene to obtain a fifth mixed solution; then the fourth mixed solution and the fifth mixed solution are mixed at room temperature, stirred for reaction for 10 hours, and then an equal volume of n-hexane (Fischer Scientific International Inc. (Fischer Scientific International Inc. (Fischer Scientific International Inc. (Fischer Scientific International Inc. (Fischer Scientific International Inc. (Fischer Scientific International Inc. (Fischer Scientific International Inc. (Fischer Scientific International Inc. (Fischer Scientific International Inc. Scientific), HPLC), and placed at -30°C overnight, then filtered to collect the precipitated solid; the precipitated solid was dissolved in 80 mL of dichloromethane to prepare a sixth mixed solution; ligand B was dissolved in 30 mL of dichloromethane to prepare a seventh mixed solution, then the sixth mixed solution and the seventh mixed solution were mixed at 40°C, and then 0.1 g of cuprous chloride was added, stirred for reaction for 8 hours, and then allowed to stand at -30°C overnight, filtered, and the obtained solid was the ruthenium catalyst; Wherein, ligand A may include 1,3-bis(2,4,6-triisopropylphenyl)imidazole (Sinopharm Chemical Reagent Co., Ltd., 98%); ligand B may be prepared according to the following process: in a glove box, 1.3 g of 2-methoxystyrene (Sinopharm Chemical Reagent Co., Ltd., 97%) is dissolved in 10 mL of toluene to obtain an eighth mixed solution, and then 0.1 g of anhydrous aluminum chloride (Sinopharm Chemical Reagent Co., Ltd., 98%) is added to the eighth mixed solution, and then methyl chloride gas (Shanghai Weichuang Standard Gas Co., Ltd., 99%) is introduced, and the reaction is carried out for 3 hours to obtain a reaction solution, and the above reaction solution is added dropwise to 0.7 g of metallic lithium (Sinopharm Chemical Reagent Co., Ltd., 99%) at -78°C to obtain a toluene solution containing alkyl lithium, and 2 mL of the toluene solution containing alkyl lithium is added dropwise to 3 g of 3,5-dibromopyridine, and after stirring for 5 hours, it is recrystallized at -30°C to precipitate a solid, namely ligand B; Alternatively, ligand A may include 1,3-bis(2,4,6-triisopropylphenyl)imidazole (Sinopharm Chemical Reagent Co., Ltd., 98%); ligand B may be prepared according to the following process: 1 g of 2-isopropoxystyrene (Sinopharm Chemical Reagent Co., Ltd., 97%) is dissolved in 10 mL of toluene to obtain a ninth mixed solution, 0.1 g of anhydrous aluminum chloride (Sinopharm Chemical Reagent Co., Ltd., 98%) is added to the ninth mixed solution, and then methyl chloride gas (Shanghai Weichuang Standard Gas Co., Ltd., 99%) is introduced, and the reaction is carried out for 3 hours to obtain a reaction solution, and the reaction solution is added dropwise to 0.7 g of metallic lithium (Sinopharm Chemical Reagent Co., Ltd., 99%) at -78°C to obtain a toluene solution containing alkyl lithium, 2 mL of the toluene solution containing alkyl lithium is added dropwise to 3 g of 3,5-dibromopyridine, and after stirring for 3 hours, it is recrystallized at -30°C to precipitate a solid as ligand B; Alternatively, ligand A may include 1,3-bis(2,4,6-triisopropylphenyl)imidazole (Sinopharm Chemical Reagent Co., Ltd., 98%); ligand B may be prepared according to the following process: 1 g of 2-isopropoxystyrene (Sinopharm Chemical Reagent Co., Ltd., 97%) is dissolved in 10 mL of toluene to obtain a tenth mixed solution, 0.1 g of anhydrous aluminum chloride (Sinopharm Chemical Reagent Co., Ltd., 98%) is added to the tenth mixed solution, and then 0.3 g of 1-chlorobutanol-2-one (Adamas Reagent Co., Ltd. (Adamas), 98%) is added, and the mixture is reacted for 3 h to obtain a reaction solution, and then the reaction solution is added dropwise to 0.7 g of metallic lithium (Sinopharm Chemical Reagent Co., Ltd., 99%) at -78°C to obtain a toluene solution containing alkyl lithium, 2.5 mL of the toluene solution containing alkyl lithium is added dropwise to 3 g of 3,5-dibromopyridine, and the mixture is stirred for reaction for 3 h, and then recrystallized at -30°C to precipitate a solid as ligand B; Alternatively, ligand A may include tricyclohexylphosphine (Adamas Reagent Co., Ltd., 98%); ligand B may be prepared according to the following process: 1 g of 2-isopropoxystyrene (Sinopharm Chemical Reagent Co., Ltd., 97%) is dissolved in 10 mL of toluene to obtain an eleventh mixed solution, 0.1 g of anhydrous aluminum chloride (Sinopharm Chemical Reagent Co., Ltd., 98%) is added to the eleventh mixed solution, and then 0.5 mL of tert-butyl chloride (Adamas Reagent Co., Ltd., 99%) is added, and the reaction is carried out for 3 hours to obtain a reaction solution; then, the reaction solution is added dropwise to 0.7 g of metallic lithium (Sinopharm Chemical Reagent Co., Ltd., 99%) at -78°C to obtain a toluene solution containing alkyl lithium, 1.5 mL of the toluene solution containing alkyl lithium is added dropwise to 3 g of 3,5-dibromopyridine, and after stirring for 6 hours, it is recrystallized at -30°C to precipitate a solid as ligand B; Alternatively, ligand A may include 1,3-bis(2,4,6-triisopropylphenyl)imidazole (Sinopharm Chemical Reagent Co., Ltd., 98%); ligand B may be prepared according to the following process, 1 g of 2-isopropoxystyrene (Sinopharm Chemical Reagent Co., Ltd., 97%) is dissolved in 10 mL of toluene to obtain a twelfth mixed solution, 0.1 g of anhydrous aluminum chloride (Sinopharm Chemical Reagent Co., Ltd., 98%) is added to the twelfth mixed solution, and then 0.5 mL of tert-butyl chloride (Adamas Reagent Co., Ltd. (adamas), 99%) is added, and the reaction is carried out for 3 hours to obtain a reaction solution; then, the above reaction solution is added dropwise to 0.7 g of metallic lithium (Sinopharm Chemical Reagent Co., Ltd., 99%) at -78°C to obtain a toluene solution containing alkyl lithium, 1.5 mL of the toluene solution containing alkyl lithium is added dropwise to 3 g of 3,5-dibromopyridine, and after stirring for 7 hours, it is recrystallized at -30°C to precipitate a solid as ligand B.
[0037] It is understandable that the quality of raw materials and reaction conditions in the above-mentioned process of preparing ruthenium-based catalysts are average values.
[0038] The preparation process of the ruthenium-based catalyst in the embodiment of the present invention is not limited to the above process.
[0039] The above-mentioned ruthenium catalyst can be supported on a carrier to form a supported catalyst. In this case, the ruthenium catalyst does not need to be prepared into a solution, and can be directly added to the mixed solution (for example, directly added to the reactor). The carrier of the supported catalyst can include one or more of activated carbon, silica gel, diatomaceous earth, and aluminum oxide.
[0040] In some embodiments, the chain transfer agent includes olefins and / or halogenated olefins having 3 to 30 carbon atoms, and the olefins may include aliphatic olefins and / or aromatic olefins.
[0041] The above-mentioned aliphatic olefins may include one or more of 1-pentene, 2-pentene, 1-hexene, 2-hexene, 4-octene, 1-octene, and 1-heptene; the aromatic olefins may include one or more of styrene, triphenylethylene, 4-phenyl-1-butene, and 6-phenyl-1-hexene; the halogenated olefins may include one or more of 4-bromo-1-butene, 2-bromo-2-butene, 6-bromo-1-hexene, 5,6-dibromo-1-hexene, 6-chloro-1-hexene, and 8-chloro-1-octene.
[0042] Preferably, the chain transfer agent may include aliphatic olefins and / or aromatic olefins.
[0043] Preheating the solution of cycloolefin polymer monomer, the solution of chain transfer agent and the solution of ruthenium catalyst to 45-200°C, for example, 45°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 120°C, 150°C, 200°C or a range consisting of any two of them, preferably 50-80°C, helps to reduce the amount of ruthenium catalyst (Ru catalyst) used, while ensuring that cycloolefin polymers with narrow molecular weight distribution, good thermal stability and optical properties are obtained, that is, while reducing costs, ensuring that products with excellent performance (cycloolefin polymers) are obtained. The reason for this is that when the preheating temperature is higher than 200°C, the ruthenium catalyst may be deactivated, and when the preheating temperature is lower than 45°C, polymers may precipitate from the solvent, resulting in a wider molecular weight distribution of the final product (cycloolefin polymer).
[0044] In some embodiments, the preheated cycloolefin polymer monomer solution, the chain transfer agent solution, and the ruthenium catalyst solution are mixed in a molar ratio of cycloolefin polymer monomer, chain transfer agent, and ruthenium element of 1:(1×10 -4 ~5×10 -2 ): (1×10 -5 ~5×10 -4 ) are mixed to obtain a mixed solution. That is, in the mixed solution, the molar ratio of the cycloolefin polymer monomer, the chain transfer agent, and the ruthenium element is 1: (1×10 -4 ~5×10 -2 ): (1×10 -5 ~5×10 -4 ), preferably 1: (3×10 -4 ~8×10 -4 ): (5×10 -5 ~1×10 -4 ).
[0045] In the mixed solution, the molar ratio of the cycloolefin polymer monomer to the ruthenium element can be 1:(1×10 -5 ~5×10 -4 ).
[0046] In the mixed solution, the molar ratio of the cycloolefin polymer monomer to the chain transfer agent can be 1:(1×10 -4 ~5×10 -2 ).
[0047] In a specific implementation, the preheated cycloolefin polymer monomer solution, chain transfer agent solution, and ruthenium catalyst solution can be added into a reaction kettle (eg, a reaction kettle substituted with nitrogen three times) and mixed to obtain a mixed solution.
[0048] Next, the mixed solution is subjected to a ring-opening polymerization reaction at 45 to 250° C., and the time of the ring-opening polymerization reaction is 5 to 65 minutes. For example, the temperature of the ring-opening polymerization reaction may be 45° C., 50° C., 60° C., 80° C., 100° C., 120° C., 150° C., 200° C., 250° C., or a range consisting of any two thereof, preferably 50 to 100° C., and the time of the ring-opening polymerization reaction may be 5 minutes, 10 minutes, 20 minutes, 30 minutes, 40 minutes, 50 minutes, 55 minutes, 56 minutes, 57 minutes, 58 minutes, 59 minutes, 60 minutes, 61 minutes, 62 minutes, 63 minutes, 64 minutes, 65 minutes, or a range consisting of any two thereof.
[0049] In specific implementation, the temperature of the above-mentioned ring-opening polymerization reaction should be greater than or equal to (i.e. not lower than) the above-mentioned preheating temperature to avoid the precipitation of the product (polymer) of the ring-opening polymerization reaction, which may lead to the problem of a broadening of the molecular weight distribution of the final product (cycloolefin polymer), thereby ensuring that a cycloolefin polymer with a narrow molecular weight distribution, good thermal stability and optical properties is obtained.
[0050] In some embodiments, the pressure of the ring-opening polymerization reaction may be 0.1-5 MPa, for example, 0.1 MPa, 0.5 MPa, 1 MPa, 2 MPa, 3 MPa, 4 MPa, 5 MPa or a range consisting of any two thereof, preferably 0.1-2 MPa.
[0051] After the ring-opening polymerization reaction is completed, a hydrogen source is added to the mixed solution for hydrogenation reaction. The hydrogenation reaction time is 6 to 12 hours, for example, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours or a range consisting of any two of them.
[0052] The above-mentioned preheating, mixing and ring-opening polymerization processes can all be carried out under the protection of inert gas.
[0053] The hydrogen source includes hydrogen and / or hydrazine compounds. For example, after the ring-opening polymerization reaction is completed, hydrogen can be introduced into the mixed solution for hydrogenation reaction; and / or, after the ring-opening polymerization reaction is completed, hydrazine compounds can be added (or introduced) into the mixed solution for hydrogenation reaction.
[0054] The hydrazine compound may include one or more of hydrazine, phenylhydrazine, formic hydrazide, acetic hydrazide, valeryl hydrazide, hexyl hydrazide, benzenesulfonyl hydrazide, p-toluenesulfonyl hydrazide and phenylmethylsulfonyl hydrazide.
[0055] During the above hydrogenation reaction, a hydrogenation catalyst may be added to the mixed solution to improve the efficiency of the hydrogenation reaction (the reaction activity of various reactants in the hydrogenation reaction).
[0056] The above-mentioned hydrogenation catalyst can be selected to use a heterogeneous catalyst or a homogeneous catalyst. The above-mentioned heterogeneous catalyst can include a heterogeneous catalyst prepared by loading one or more metals of nickel, palladium, platinum, rhodium, and ruthenium on a carrier, such as nickel / silicon dioxide, ruthenium / diatomaceous earth, palladium / carbon, palladium / silicon dioxide, nickel / carbon, nickel / alumina, platinum / silicon dioxide, platinum / carbon, palladium / alumina, ruthenium / carbon, ruthenium / alumina, nickel / diatomaceous earth, and ruthenium / silicon dioxide. The above-mentioned homogeneous catalyst may include one or more of a catalyst composed of a transition metal compound and an organic aluminum compound, a catalyst composed of a metallocene compound and an organic alkali metal compound, a catalyst composed of a transition metal compound and an organic magnesium compound, and a noble metal carbene catalyst. For example, the catalyst composed of a transition metal compound and an organic aluminum compound may be selected from nickel acetate / triisobutylaluminum, cobalt acetate / trimethylaluminum, nickel acetylacetonate / triethylaluminum or cobalt acetylacetonate / triisobutylaluminum, the catalyst composed of a metallocene compound and an organic alkali metal compound may be selected from dichlorodipentadienyltitanium / tert-butyllithium or dichlorodipentadienyltitanium / n-butyllithium, the catalyst composed of a transition metal compound and an organic magnesium compound may be selected from tetrabutoxytitanate / dimethylmagnesium or tetrabutoxytitanate / diethylmagnesium, and the noble metal carbene catalyst may be selected from bis(triphenylphosphine)palladium dichloride, chlorohydrocarbonyltris(triphenylphosphine)ruthenium, chlorohydrocarbonylbis(tricyclohexylphosphine)ruthenium, bis(tricyclohexylphosphine)benzylideneruthenium dichloride or tris(triphenylphosphine)rhodium chloride.
[0057] In particular, when a heterogeneous catalyst is used as the hydrogenation catalyst, the hydrogenation catalyst can be separated and recovered by filtering or other means after the hydrogenation reaction (hydrogenation reaction) is completed, so as to facilitate reuse. It is understandable that the conditions of the hydrogenation reaction (hydrogenation reaction) are different depending on the selected hydrogenation catalyst system.
[0058] In some embodiments, the temperature of the hydrogenation reaction is -10 to 210°C, for example, -10°C, -5°C, 0°C, 10°C, 50°C, 100°C, 150°C, 200°C, 210°C or a range composed of any two thereof, preferably -5 to 200°C, and further preferably 25 to 190°C.
[0059] In some embodiments, the pressure of the hydrogenation reaction is 0.05 to 15 MPa, for example, 0.05 MPa, 0.1 MPa, 0.5 MPa, 1 MPa, 2 MPa, 5 MPa, 6 MPa, 7 MPa, 8 MPa, 9 MPa, 10 MPa, 12 MPa, 13 MPa, 14 MPa, 15 MPa or a range composed of any two thereof, preferably 0.1 to 10 MPa, and more preferably 0.5 to 8 MPa.
[0060] After the hydrogenation reaction is completed, a terminator, an adsorbent and a poor solvent are sequentially added to the mixed solution. In the process of separating the cycloolefin polymer, the terminator serves to terminate the ring-opening polymerization reaction and the hydrogenation reaction (i.e., the formation reaction of the cycloolefin polymer) to ensure that the cycloolefin polymer with a narrow molecular weight distribution, good thermal stability and optical properties is obtained. The adsorbent serves to remove the ruthenium catalyst. The poor solvent needs to have good compatibility with the aforementioned inert solvent (the solvent for the ring-opening polymerization reaction and the hydrogenation reaction) and be immiscible with the cycloolefin polymer, so as to facilitate the precipitation of the cycloolefin polymer from the solution and to facilitate the separation of the cycloolefin polymer.
[0061] The terminator may include an olefin having 3 to 30 carbon atoms and containing a sixth heteroatom, wherein the sixth heteroatom may include one or more of an oxygen atom, a nitrogen atom, a silicon atom, a sulfur atom, and a halogen atom, and may specifically include one or more of 1,1-diethoxyethylene, 1-bromo-2-ethoxyethylene, methoxyethylene, ethoxyethylene, 2-methoxypropylene, 3,3-dimethoxypropylene, 3-methoxyacrylic acid, ethyl propylene ether, and 3-ethoxypropylene. The amount of the terminator added may be 1 to 100 times, preferably 10 to 50 times, of the amount of the ruthenium catalyst.
[0062] The above-mentioned adsorbent generally uses a solid adsorbent with a large specific surface area and insoluble in the above-mentioned inert solvent (solvent for ring-opening polymerization reaction and hydrogenation reaction), for example, it may include one or more of thiourea resin, activated carbon, silica gel, diatomaceous earth, and alumina. In specific implementation, after the above-mentioned adsorbent fully adsorbs the ruthenium-based catalyst, the adsorbent can be removed (separated) by filtration, leaving a supernatant (supernatant) without the catalyst; then, a poor solvent is added to the supernatant or the supernatant is added dropwise to the poor solvent to promote the precipitation of the cycloolefin polymer (forming a white suspension), and then the cycloolefin polymer is separated.
[0063] The above-mentioned poor solvent may include one or more of alcohol solvents (for example, one or more of methanol, ethanol, isopropanol, ethylene glycol, and n-butanol), aldehyde ketone solvents (for example, one or more of acetone, acetone aldehyde, bromoacetone, propionaldehyde, and isobutyraldehyde), ether solvents (for example, one or more of ethyl ether, methyl ethyl ether, dibutyl ether, and tetrahydrofuran), and phenol solvents (for example, one or more of phenol, o-cresol, and propofol), preferably alcohol solvents (for example, one or more of methanol, ethanol, and isopropanol). The amount of the above-mentioned poor solvent added may exceed the required amount, which is conducive to the precipitation of cycloolefin polymers.
[0064] In some embodiments, after the hydrogenation reaction is completed, a terminator, an adsorbent and a poor solvent are sequentially added to the mixed solution, and the process of isolating the cycloolefin polymer includes: after the hydrogenation reaction is terminated, a terminator is added to the mixed solution, and the temperature of the mixed solution is controlled to be 45 to 250°C, and the temperature of the mixed solution is controlled to be greater than or equal to (not lower than) the temperature of the ring-opening polymerization reaction, and after 1 to 60 minutes; an adsorbent is added thereto to remove the ruthenium catalyst; and then a poor solvent is added thereto to precipitate the cycloolefin polymer, and the cycloolefin polymer is separated; wherein the molar ratio of the terminator to the ruthenium element in the mixed solution is (1 to 100):1. In the above process, the temperature of the mixed solution is controlled to be 45-250°C, for example, 45°C, 50°C, 60°C, 70°C, 90°C, 100°C, 150°C, 200°C, 250°C or a range consisting of any two thereof, preferably 50-100°C, and the temperature of the mixed solution is maintained and controlled to be greater than or equal to the temperature of the ring-opening polymerization reaction, while ensuring that the terminator fully exerts the effect of the termination reaction and avoiding the precipitation problem of the hydrogenation reaction product, thereby avoiding affecting the molecular weight of the final product (cycloolefin polymer), ensuring that a cycloolefin polymer with a narrow molecular weight distribution, good thermal stability and optical properties is obtained; further, the temperature of the above mixed solution is controlled at 45-250°C and maintained for 1-60min, for example, 1min, 10min, 20min, 30min, 40min, 50min, 60min or a range consisting of any two thereof, preferably 5-30min, to ensure that the ring-opening polymerization reaction and the hydrogenation reaction (i.e., the formation reaction of the cycloolefin polymer) are completely terminated.
[0065] The terminator can be directly added to the mixed solution (such as a reactor), or it can be dissolved in an organic solvent to prepare a terminator solution, and the terminator solution is added to the mixed solution. For example, after the hydrogenation reaction is terminated, the terminator, the adsorbent and the poor solvent are sequentially added to the mixed solution to separate the cycloolefin polymer. The process may include: after the hydrogenation reaction is terminated, the terminator solution, the adsorbent and the poor solvent solution are sequentially added to the mixed solution to separate the cycloolefin polymer. The above-mentioned organic solvent only needs to be able to dissolve or disperse the terminator and not affect the structure of the product (polymer) of the ring-opening polymerization reaction and the hydrogenation reaction. For example, one or more of aliphatic hydrocarbons, alicyclic hydrocarbons, aromatic hydrocarbons, halogenated aliphatic hydrocarbons, and ethers can be used. The above-mentioned aliphatic hydrocarbons may include one or more of pentane, hexane, and heptane. The above-mentioned alicyclic hydrocarbons may include one or more of cyclopentane, cyclohexane, cyclodecane, hexahydroindene cyclohexane, and cyclooctane. The aromatic hydrocarbons may include one or more of benzene, toluene, and xylene. The halogenated aliphatic hydrocarbons may include one or more of dichloromethane, chloroform, and 1,2-dichloroethane. The nitrogen-containing hydrocarbons may include one or more of nitromethane, nitrobenzene, and acetonitrile. The ethers may include one or more of diethyl ether and tetrahydrofuran.
[0066] The concentration of the terminator in the above-mentioned terminator solution can be 0.001 to 10 mol / L, for example, 0.001 mol / L, 0.01 mol / L, 0.1 mol / L, 1 mol / L, 2 mol / L, 4 mol / L, 6 mol / L, 8 mol / L, 10 mol / L or a range consisting of any two of them, preferably 0.01 to 5 mol / L.
[0067] The poor solvent solution may include a pH adjuster, which can adjust the pH value and further regulate the solubility of impurities to achieve the purpose of removing impurities from the cycloolefin polymer.
[0068] The pH regulator includes an acidic substance and / or an alkaline substance. The acidic substance may include one or more of hydrochloric acid, sulfuric acid, lactic acid, and acetic acid, preferably hydrochloric acid and / or lactic acid; the alkaline substance may include one or more of sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide, and potassium carbonate, preferably sodium hydroxide and / or sodium carbonate.
[0069] The embodiment of the present invention further provides a cycloolefin polymer, which is obtained according to the above preparation method.
[0070] In some embodiments, the glass transition temperature of the cycloolefin polymer is 100-300° C., preferably 100-200° C., and more preferably 140-155° C., indicating that the cycloolefin polymer has good thermal stability.
[0071] In some embodiments, the hydrogenation rate of unsaturated bonds of the cycloolefin polymer is not less than 95%, preferably above 95%, more preferably above 98%, further preferably above 99.5%, and particularly preferably above 99.8%, indicating that the cycloolefin polymer has good light transmittance.
[0072] In some embodiments, the refractive index of the cycloolefin polymer is 1.5 to 2.1, preferably, the refractive index is 1.52 to 1.6, and more preferably, the refractive index is 1.54 to 1.56. The cycloolefin polymer has good optical properties.
[0073] The present invention is described in more detail below through specific embodiments.
[0074] The petroleum raw materials in each embodiment and comparative example can be purchased commercially or prepared according to conventional methods in the art.
[0075] The ruthenium-based catalysts used in Comparative Examples 1 and 2 are both commercial catalysts, which can be purchased from Adamas Reagent Co., Ltd. (ADAMAS), and the purity is 98%.
[0076] The ruthenium catalyst I can be prepared according to the following process: 1 g of Grubbs second generation catalyst [CAS: 246047-72-3] (Adamas Reagent Co., Ltd., purity 98%) is dissolved in 50 mL of dichloromethane (Adamas Reagent Co., Ltd., purity 99.9%) to obtain a first mixed solution; 1 Dissolve in 30 mL of dichloromethane to prepare a solution to obtain a second mixed solution; then, mix the first mixed solution and the second mixed solution at 40°C, add 0.1 g of cuprous chloride (Adamas Reagent Co., Ltd., 98%), stir and react for 5 hours, let stand overnight at -30°C, and then filter to obtain a solid, namely, ruthenium-based catalyst I. Among them, ligand B can be prepared according to the following process 1: In a glove box, 1 g of 2-isopropoxystyrene (Sinopharm Chemical Reagent Co., Ltd., 97%) was dissolved in 10 mL of toluene to obtain a third mixed solution; 0.1 g of anhydrous aluminum chloride (Sinopharm Chemical Reagent Co., Ltd., 98%) was added to the third mixed solution, and then methyl chloride gas (Shanghai Weichuang Standard Gas Co., Ltd., 99%) was introduced to react for 3 h to obtain a reaction solution; then, the above reaction solution was added dropwise to 0.7 g of metallic lithium (Sinopharm Chemical Reagent Co., Ltd., 99%) at -78°C to obtain a toluene solution containing alkyl lithium; 2 mL of the toluene solution containing alkyl lithium was taken and added dropwise to 3 g of 3,5-dibromopyridine (Adamas Reagent Co., Ltd. (adamas), 98%), stirred for reaction for 3 h, and then recrystallized at -30°C, and the precipitated solid was the ligand B used. 1 .
[0077] Ruthenium catalysts II to VI can be prepared according to the following process: 1 g of Grubbs second generation catalyst [CAS: 246047-72-3] (Adamas Reagent Co., Ltd. (Adamas), 98%) is dissolved in 60 mL of toluene (Adamas Reagent Co., Ltd. (Adamas), 99.5%) to obtain a fourth mixed solution; in addition, ligand A is dissolved in 45 mL of toluene to obtain a fifth mixed solution; then the fourth mixed solution and the fifth mixed solution are mixed at room temperature, stirred for reaction for 10 hours, and then an equal volume of n-hexane (Fischer Scientific International Inc. (Fischer Scientific International Inc. (Fischer Scientific International Inc. (Fischer Scientific International Inc. (Fischer Scientific International Inc. (Fischer Scientific International Inc. (Fischer Scientific International Inc. (Fischer Scientific International Inc. (Fischer Scientific International Inc. Scientific), HPLC), and placed at -30°C overnight, then filtered to collect the precipitated solid; the precipitated solid was dissolved in 80 mL of dichloromethane to prepare a sixth mixed solution; ligand B was dissolved in 30 mL of dichloromethane to prepare a seventh mixed solution, then the sixth mixed solution and the seventh mixed solution were mixed at 40°C, and then 0.1 g of cuprous chloride was added, stirred for reaction for 8 hours, and then allowed to stand at -30°C overnight, filtered, and the obtained solid was ruthenium-based catalysts II to VI; Wherein, the ligand A corresponding to the ruthenium catalyst II may include 1,3-bis(2,4,6-triisopropylphenyl)imidazole (Sinopharm Chemical Reagent Co., Ltd., 98%); the ligand B corresponding to the ruthenium catalyst II may be prepared by referring to the following process: in a glove box, 1.3 g of 2-methoxystyrene (Sinopharm Chemical Reagent Co., Ltd., 97%) is dissolved in 10 mL of toluene to obtain an eighth mixed solution, and then 0.1 g of anhydrous aluminum chloride (Sinopharm Chemical Reagent Co., Ltd.) is added to the eighth mixed solution. Company, 98%), and then introduce chloromethane gas (Shanghai Weichuang Standard Gas Co., Ltd., 99%), react for 3 hours to obtain a reaction solution, add the above reaction solution drop by drop into 0.7g of metallic lithium (Sinopharm Chemical Reagent Co., Ltd., 99%) at -78°C to obtain a toluene solution containing alkyl lithium, take 2mL of the toluene solution containing alkyl lithium and add dropwise to 3g of 3,5-dibromopyridine, stir and react for 5 hours, and then recrystallize at -30°C to precipitate a solid, which is the ligand B corresponding to the ruthenium-based catalyst II.
[0078] The ligand A corresponding to the ruthenium catalyst III includes 1,3-bis(2,4,6-triisopropylphenyl)imidazole (Sinopharm Chemical Reagent Co., Ltd., 98%); the ligand B corresponding to the ruthenium catalyst III can be prepared by referring to the following process: 1 g of 2-isopropoxystyrene (Sinopharm Chemical Reagent Co., Ltd., 97%) is dissolved in 10 mL of toluene to obtain a ninth mixed solution, and 0.1 g of anhydrous aluminum chloride (Sinopharm Chemical Reagent Co., Ltd., 98%) is added to the ninth mixed solution. , then introduce chloromethane gas (Shanghai Weichuang Standard Gas Co., Ltd., 99%), react for 3 hours to obtain a reaction solution, add the above reaction solution dropwise into 0.7 g of metallic lithium (Sinopharm Chemical Reagent Co., Ltd., 99%) at -78°C to obtain a toluene solution containing alkyl lithium, take 2 mL of the toluene solution containing alkyl lithium and add dropwise into 3 g of 3,5-dibromopyridine, stir and react for 3 hours, and then recrystallize at -30°C to precipitate a solid which is the ligand B corresponding to the ruthenium-based catalyst III.
[0079] The ligand A corresponding to the ruthenium catalyst IV may include 1,3-bis(2,4,6-triisopropylphenyl)imidazole (Sinopharm Chemical Reagent Co., Ltd., 98%); the ligand B corresponding to the ruthenium catalyst IV may be prepared by referring to the following process: 1 g of 2-isopropoxystyrene (Sinopharm Chemical Reagent Co., Ltd., 97%) is dissolved in 10 mL of toluene to obtain a tenth mixed solution, 0.1 g of anhydrous aluminum chloride (Sinopharm Chemical Reagent Co., Ltd., 98%) is added to the tenth mixed solution, and then 0.3 g of 1-Chlorobutanol-2-one (Adamas Reagent Co., Ltd. (Adamas), 98%), react for 3 hours to obtain a reaction solution, then, at -78 ° C, the above reaction solution was added dropwise to 0.7 g of metallic lithium (Sinopharm Chemical Reagent Co., Ltd., 99%) to obtain a toluene solution containing alkyl lithium, 2.5 mL of the toluene solution containing alkyl lithium was added dropwise to 3 g of 3,5-dibromopyridine, stirred for reaction for 3 hours, and then recrystallized at -30 ° C. The precipitated solid was the ligand B corresponding to the ruthenium catalyst IV.
[0080] The ligand A corresponding to the ruthenium catalyst V may include tricyclohexylphosphine (Adamas Reagent Co., Ltd. (adamas), 98%); the ligand B corresponding to the ruthenium catalyst V may be prepared by referring to the following process: 1 g of 2-isopropoxystyrene (Sinopharm Chemical Reagent Co., Ltd., 97%) is dissolved in 10 mL of toluene to obtain an eleventh mixed solution, 0.1 g of anhydrous aluminum chloride (Sinopharm Chemical Reagent Co., Ltd., 98%) is added to the eleventh mixed solution, and then 0.5 mL of chlorine is added. tert-Butane (Adamas Reagent Co., Ltd. (Adamas), 99%), react for 3 hours to obtain a reaction solution; then, the reaction solution was added dropwise into 0.7 g of metallic lithium (Sinopharm Chemical Reagent Co., Ltd., 99%) at -78°C to obtain a toluene solution containing alkyl lithium, 1.5 mL of the toluene solution containing alkyl lithium was added dropwise into 3 g of 3,5-dibromopyridine, and the reaction was stirred for 6 hours, and then recrystallized at -30°C to precipitate a solid which was the ligand B corresponding to the ruthenium-based catalyst V.
[0081] The ligand A corresponding to the ruthenium catalyst VI may include 1,3-bis(2,4,6-triisopropylphenyl)imidazole (Sinopharm Chemical Reagent Co., Ltd., 98%); the ligand B corresponding to the ruthenium catalyst VI may be prepared by referring to the following process: 1 g of 2-isopropoxystyrene (Sinopharm Chemical Reagent Co., Ltd., 97%) is dissolved in 10 mL of toluene to obtain a twelfth mixed solution, 0.1 g of anhydrous aluminum chloride (Sinopharm Chemical Reagent Co., Ltd., 98%) is added to the twelfth mixed solution, and then 0. 5mL of tert-butyl chloride (Adamas Reagent Co., Ltd., 99%) was reacted for 3h to obtain a reaction solution; then, the reaction solution was added dropwise to 0.7g of metallic lithium (Sinopharm Chemical Reagent Co., Ltd., 99%) at -78°C to obtain a toluene solution containing alkyl lithium, 1.5mL of the toluene solution containing alkyl lithium was added dropwise to 3g of 3,5-dibromopyridine, and the reaction was stirred for 7h, and then recrystallized at -30°C to precipitate a solid which was the ligand B corresponding to the ruthenium-based catalyst VI.
[0082] Example 1 This embodiment provides a method for preparing a cycloolefin polymer, comprising: 1) Dissolve 5 g of 8-methyltetracyclododecene in 100 mL of cyclohexane to obtain a solution of cycloolefin polymer monomer; dissolve 0.12 g of ruthenium catalyst III in 100 mL of cyclohexane to obtain a solution of ruthenium catalyst; dissolve 0.14 g of 1-octene in 200 mL of cyclohexane to obtain a solution of chain transfer agent; 2) preheating the above-mentioned cycloolefin polymer monomer solution, chain transfer agent solution, and ruthenium catalyst solution at 70° C. for 30 minutes respectively; 3) Under normal pressure, 25 mL of the preheated cycloolefin polymer monomer solution, 45 mL of the preheated chain transfer agent solution, and 1.1 mL of the preheated ruthenium catalyst solution were mixed to obtain a mixed solution, and the mixed solution was stirred at 70° C. for 60 minutes to perform a ring-opening polymerization reaction; 4) After the ring-opening polymerization reaction is completed, hydrogen is introduced into the mixed solution for hydrogenation reaction at 180°C and 0.8MPa for 12h; 5) After the hydrogenation reaction is completed, 20 mL of a mixed solution of vinyl ether and cyclohexane (the volume ratio of vinyl ether to cyclohexane is 1:4) is added to the above mixed solution, and stirred at 80°C for 15 min; then 5 g of thiourea resin is added to the mixed solution, and after stirring for 10 min, the solution is filtered to obtain a supernatant; the supernatant is added dropwise to 1.5 L of acetone to form a white suspension, and the white suspension is filtered to obtain a cycloolefin polymer.
[0083] Comparative Example 1 This comparative example provides a method for preparing a cycloolefin polymer, comprising: 1) 1.25 g of 8-methyltetracyclododecene, 0.05 g of 1-octene, and 12 mg of 1,3-bis(2,4,6-trimethylphenyl)-2-(imidazolidinylidene)(dichlorobenzylidene)(tricyclohexylphosphine)ruthenium were dissolved in 70 mL of cyclohexane to obtain a mixed solution, and the mixed solution was stirred at 70° C. for 60 min to perform a ring-opening polymerization reaction; 2) After the ring-opening polymerization reaction is completed, hydrogen is introduced into the mixed solution for hydrogenation reaction at 150°C and 0.8 MPa for 10 hours; 3) After the hydrogenation reaction is completed, 20 mL of a mixed solution of vinyl ether and cyclohexane (the volume ratio of vinyl ether to cyclohexane is 1:4) is added to the above mixed solution, and stirred at room temperature for 15 minutes; then 5 g of thiourea resin is added to the mixed solution, and after stirring for 10 minutes, the solution is filtered to obtain a supernatant; the supernatant is added dropwise to 1.5 L of acetone to form a white suspension, and the white suspension is filtered to obtain a cycloolefin polymer.
[0084] Comparative Example 2 This comparative example provides a method for preparing a cycloolefin polymer, comprising: 1) 1.25 g of 8-methyltetracyclododecene, 0.36 g of N-phenyl-5-norbornene-2,3-dicarboximide, 0.05 g of 1-octene, and 12 mg of 1,3-bis(2,4,6-trimethylphenyl)-2-(imidazolidinylidene)(dichlorobenzylidene)(tricyclohexylphosphine)ruthenium were dissolved in 70 mL of cyclohexane to obtain a mixed solution, and the mixed solution was stirred at 70° C. for 60 min to perform a ring-opening polymerization reaction; 2) After the ring-opening polymerization reaction is completed, hydrogen is introduced into the mixed solution for hydrogenation reaction at 150°C and 0.8 MPa for 10 hours; 3) After the hydrogenation reaction is completed, 5 mL of a mixed solution of vinyl ether and cyclohexane (the volume ratio of vinyl ether to cyclohexane is 1:4) is added to the above mixed solution, and stirred at room temperature for 15 minutes; then 5 g of thiourea resin is added to the mixed solution, stirred for 10 minutes, and filtered to obtain a supernatant; the supernatant is added dropwise into 1.5 L of acetone to form a white suspension, and the white suspension is filtered to obtain a cycloolefin polymer.
[0085] Comparative Example 3 This comparative example provides a method for preparing a cycloolefin polymer, comprising: 1) Dissolve 5 g of 8-methyltetracyclododecene in 100 mL of cyclohexane to obtain a solution of cycloolefin polymer monomer; dissolve 0.12 g of ruthenium catalyst III in 100 mL of cyclohexane to obtain a solution of ruthenium catalyst; dissolve 0.14 g of 1-octene in 200 mL of cyclohexane to obtain a solution of chain transfer agent; 2) preheating the above-mentioned cycloolefin polymer monomer solution, chain transfer agent solution, and ruthenium catalyst solution at 30° C. for 30 minutes respectively; 3) Under normal pressure, 25 mL of a cycloolefin polymer monomer solution, 45 mL of a chain transfer agent solution, and 1.1 mL of a ruthenium catalyst solution were mixed to obtain a mixed solution, and the mixed solution was stirred at 70° C. for 60 min to perform a ring-opening polymerization reaction; 4) After the ring-opening polymerization reaction is completed, hydrogen is introduced into the mixed solution for hydrogenation reaction at 180°C and 0.8MPa for 12h; 5) After the hydrogenation reaction is completed, 20 mL of a mixed solution of vinyl ether and cyclohexane (the volume ratio of vinyl ether to cyclohexane is 1:4) is added to the above mixed solution, and stirred at 80°C for 15 min; then 5 g of thiourea resin is added to the mixed solution, and after stirring for 10 min, the solution is filtered to obtain a supernatant; the supernatant is added dropwise to 1.5 L of acetone to form a white suspension, and the white suspension is filtered to obtain a cycloolefin polymer.
[0086] Referring to the process of Example 1, the preparation of cycloolefin polymers of Examples 2 to 22 and Comparative Examples 3 to 8 was performed respectively. The cycloolefin polymer monomers, the concentration of cycloolefin polymer monomers in the solution of cycloolefin polymer monomers, the ruthenium-based catalyst, the concentration of ruthenium in the solution of the ruthenium-based catalyst, the chain transfer agent, the concentration of the chain transfer agent in the solution of the chain transfer agent, the molar ratio of the cycloolefin polymer monomers to the chain transfer agent in the mixed solution, the molar ratio of the cycloolefin polymer monomers to the ruthenium in the mixed solution, the inert solvent, etc. of each Example and Comparative Examples 3 to 8 are summarized in Tables 1, 2 and 3; the preheating temperature and time, the temperature and time of the ring-opening polymerization reaction, the hydrogen source, the temperature, pressure and time of the hydrogenation reaction, the terminator and the temperature and time of the termination reaction, the adsorbent, the poor solvent, etc. of each Example and Comparative Examples 3 to 8 are summarized in Tables 4 and 5.
[0087] Table 1
[0088] Table 2
[0089] Table 3
[0090] Table 4
[0091] Table 5
[0092] Test example 1. The following parameters of the above embodiments and comparative examples were tested: 1) The weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight distribution (PDI) of the cycloolefin polymer were measured by high temperature gel permeation chromatography, using 1,2,4-trichlorobenzene as the mobile phase and narrow distribution polystyrene as the standard. The specific results are shown in Tables 6 and 7; wherein the high temperature gel permeation chromatograms of the cycloolefin polymers of Example 1 and Comparative Example 1 are shown in Tables 6 and 7, respectively. Figure 1 and Figure 2 ( Figure 1 and Figure 2 Where A refers to the number distribution curve of polymer chains in different molecular weight ranges, and B refers to the number curve of short chain branches per 1000 carbon atoms in the polymer chain in different molecular weight ranges).
[0093] 2) The glass transition temperature of the cycloolefin polymer was measured using a differential scanning calorimeter (DSC) at a heating rate of 20°C / min. The specific results are shown in Tables 6 and 7; 3) The hydrogenation rate of the cycloolefin polymer was measured by H-NMR spectroscopy, and deuterated chloroform was selected as the solvent. The specific results are shown in Tables 6 and 7; 4) The refractive index of the cycloolefin polymer was measured by a precision refractometer. The cycloolefin polymer was made into a 4 mm thick sheet sample. The light source was a He lamp (wavelength 587.6 nm). The refractive index at 25°C was measured. The specific results are shown in Tables 6 and 7. 5) The light transmittance of the cycloolefin polymer was measured by a spectrophotometer. The cycloolefin polymer was made into a 3 mm thick sheet. The test wavelength was 430 nm. The specific results are shown in Tables 6 and 7. 6) Calculate the unit dosage of ruthenium catalyst (ruthenium catalyst / cycloolefin monomer): Use ICP-AES (RF power 1150 W; auxiliary gas flow rate 0.5 L / min; nebulizing gas flow rate 0.75 L / min; cooling water flow rate 12 L / min; peristaltic pump speed 50 r / min) to detect the content of ruthenium in the ruthenium catalyst solution, and use the content of ruthenium to express the dosage of ruthenium catalyst. Then, divide the content of ruthenium (the dosage of ruthenium catalyst) by the dosage of cycloolefin monomer (molar ratio) to obtain the unit dosage of ruthenium catalyst (ruthenium catalyst / cycloolefin monomer).
[0094] 2. Test results Table 6 Properties of Cycloolefin Polymers of Examples 1 to 16
[0095] Table 7 Properties of Cycloolefin Polymers of Examples 17-22 and Comparative Examples 1-8
[0096] Data Analysis: By adopting the method for preparing cycloolefin polymers in the embodiment of the present invention, it is possible to obtain cycloolefin polymers with narrow molecular weight distribution, good thermal stability and optical properties under the premise of using a small amount of ruthenium-based catalyst (Ru-based catalyst) (judged by combining the conversion rate and the amount of ruthenium-based catalyst used), thereby greatly reducing the cost and obtaining cycloolefin polymers with excellent performance, thereby achieving economical, efficient and controllable preparation of cycloolefin polymers with good performance.
[0097] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a cycloolefin polymer, It is characterized in that The following steps are involved: preparing a solution of a cycloolefin polymer monomer, a solution of a chain transfer agent, and a solution of a ruthenium-based catalyst respectively; Preheating the cycloolefin polymer monomer solution, the chain transfer agent solution, and the ruthenium catalyst solution to 45-200° C. respectively; The preheated solution of the cycloolefin polymer monomer, the solution of the chain transfer agent, and the solution of the ruthenium catalyst are mixed to obtain a mixed solution, and the mixed solution is subjected to a ring-opening polymerization reaction at 45 to 250° C. The time of the ring-opening polymerization reaction is 5 to 65 minutes; After the ring-opening polymerization reaction is completed, a hydrogen source is added to the mixed solution to carry out a hydrogenation reaction, and the hydrogenation reaction time is 6 to 12 hours; After the hydrogenation reaction is completed, a terminator, an adsorbent and a poor solvent are sequentially added to the mixed solution to separate and obtain the cycloolefin polymer.
2. The preparation method according to claim 1, It is characterized in that The cycloolefin polymer monomer includes one or more of the compound represented by formula (1) and the compound represented by formula (2): Formula (1) Formula (2), In the formula (1), R 1 ~R 4 Each is independently selected from a hydrogen atom, a halogen atom, an alkyl group having 1 to 15 carbon atoms, a cycloalkyl group, an aryl group having 6 to 10 carbon atoms having a substituent, or a substituent containing a first heteroatom; In the formula (2), R 5 ~R 6 are each independently selected from an alkyl group having 1 to 15 carbon atoms, a substituted or unsubstituted aryl group having 6 to 10 carbon atoms, or a substituent containing a second heteroatom, R 7 is selected from an alkyl group having 1 to 15 carbon atoms, a substituted or unsubstituted aryl group having 6 to 12 carbon atoms, or a substituent containing a third heteroatom, R 8 ~R 9 Each is independently selected from a hydrogen atom, a halogen atom, an alkyl group having 1 to 15 carbon atoms, a substituted or unsubstituted aryl group having 6 to 10 carbon atoms, or a substituent containing a fourth heteroatom; And / or, the chain transfer agent comprises an olefin and / or a halogenated olefin having 3 to 30 carbon atoms; and / or, the concentration of the cycloolefin polymer monomer in the solution of the cycloolefin polymer monomer is 0.001 to 10 mol / L; and / or, the concentration of the chain transfer agent in the chain transfer agent solution is 0.001 to 10 mol / L; And / or, the concentration of ruthenium element in the solution of the ruthenium-based catalyst is 0.001 to 10 mol / L.
3. The preparation method according to claim 2, It is characterized in that In the formula (1), R 1 and R 2 Combined with each other to form a ring; And / or, in the formula (1), the first heteroatom includes one or more of a silicon atom, a nitrogen atom, and an oxygen atom; And / or, in the formula (2), the second heteroatom includes one or more of a silicon atom, a nitrogen atom, and an oxygen atom; the third heteroatom includes one or more of a silicon atom, a nitrogen atom, and an oxygen atom; and the fourth heteroatom includes one or more of a silicon atom, a nitrogen atom, and an oxygen atom.
4. The preparation method according to claim 2, It is characterized in that The compound represented by formula (1) includes one or more of tetracyclododecene, 8-methyltetracyclododecene, 8-ethyltetracyclododecene, 8-isopropyltetracyclododecene, 8-n-butyltetracyclododecene, 8-isobutyltetracyclododecene, 8-cyclopentyltetracyclododecene, 8-cyclohexyltetracyclododecene, 8-chlorotetracyclododecene, 8-bromotetracyclododecene, 8-methoxytetracyclododecene, 8-carbonyltetracyclododecene, 8-hydroxytetracyclododecene, 8-carboxytetracyclododecene, 8-aminotetracyclododecene, 8-phenoxytetracyclododecene, 8-cyanotetracyclododecene, 8-phenyltetracyclododecene, 12-methyltetracyclododecene, 12-phenoxytetracyclododecene and 12-chlorotetracyclododecene; and / or, the compound represented by formula (2) includes 5-norbornene-2,3-dicarboxylic anhydride, 5-norbornene-2,3-dicarboximide, methyl-5-norbornene-2,3-dicarboxylic anhydride, ethyl-5-norbornene-2,3-dicarboxylic anhydride, isopropyl-5-norbornene-2,3-dicarboxylic anhydride, isobutyl-5-norbornene-2,3-dicarboxylic anhydride, cyclohexyl-5-norbornene-2,3-dicarboxylic anhydride, methyl-5-norbornene-2,3-dicarboximide, ethyl-5-norbornene-2,3-dicarboxylic anhydride One or more of amine, isopropyl-5-norbornene-2,3-dicarboximide, isobutyl-5-norbornene-2,3-dicarboximide, N-hydroxy-5-norbornene-2,3-dicarboximide, N-phenyl-5-norbornene-2,3-dicarboximide, N-benzyl-5-norbornene-2,3-dicarboximide, N-naphthyl-5-norbornene-2,3-dicarboximide, norbornene-2,3-dicarboximido tert-butyl carbonate, norbornene-2,3-dicarboximido p-nitrobenzyl carbonate; And / or, the chain transfer agent includes one or more of aliphatic olefins, aromatic olefins, and halogenated olefins; The aliphatic olefins include one or more of 1-pentene, 2-pentene, 1-hexene, 2-hexene, 4-octene, 1-octene, and 1-heptene; the aromatic olefins include one or more of styrene, triphenylethylene, 4-phenyl-1-butene, and 6-phenyl-1-hexene; the halogenated olefins include one or more of 4-bromo-1-butene, 2-bromo-2-butene, 6-bromo-1-hexene, 5,6-dibromo-1-hexene, 6-chloro-1-hexene, and 8-chloro-1-octene.
5. The preparation method according to claim 1, It is characterized in that In the mixed solution, the molar ratio of the cycloolefin polymer monomer to the ruthenium element is 1:(1×10 -5 ~5×10 -4 ); And / or, in the mixed solution, the molar ratio of the cycloolefin polymer monomer to the chain transfer agent is 1:(1×10 -4 ~5×10 -2 ); and / or, the temperature of the ring-opening polymerization reaction is greater than or equal to the preheating temperature; And / or, the pressure of the ring-opening polymerization reaction is 0.1-5 MPa.
6. The preparation method according to claim 1, It is characterized in that The hydrogen source includes hydrogen and / or hydrazine compounds; The hydrazine compound includes one or more of hydrazine, phenylhydrazine, formic hydrazide, acetic hydrazide, valeric hydrazide, hexanoic hydrazide, benzenesulfonyl hydrazide, p-toluenesulfonyl hydrazide and phenylmethanesulfonyl hydrazide; And / or, the temperature of the hydrogenation reaction is -10 to 210° C., and the pressure of the hydrogenation reaction is 0.05 to 15 MPa.
7. The preparation method according to claim 1, It is characterized in that The terminator includes an olefin having 3 to 30 carbon atoms and containing a sixth heteroatom, wherein the sixth heteroatom includes one or more of an oxygen atom, a nitrogen atom, a silicon atom, a sulfur atom, and a halogen atom; and / or, the adsorbent comprises one or more of thiourea resin, activated carbon, silica gel, diatomaceous earth, and alumina; And / or, the poor solvent includes one or more of alcohol solvents, aldehyde and ketone solvents, ether solvents, and phenol solvents; The alcohol solvent includes one or more of methanol, ethanol, isopropanol, ethylene glycol, and n-butanol; the aldehyde and ketone solvent includes one or more of acetone, acetone aldehyde, bromoacetone, propionaldehyde, and isobutyraldehyde; the ether solvent includes one or more of ethyl ether, methyl ethyl ether, dibutyl ether, and tetrahydrofuran; the phenol solvent includes one or more of phenol, o-cresol, and propofol.
8. The preparation method according to claim 1, It is characterized in that The terminator includes one or more of 1,1-diethoxyethylene, 1-bromo-2-ethoxyethylene, methoxyethylene, ethoxyethylene, 2-methoxypropylene, 3,3-dimethoxypropylene, 3-methoxyacrylic acid, ethyl propylene ether, and 3-ethoxyacrylic acid; And / or, after the hydrogenation reaction is terminated, the terminator, the adsorbent and the poor solvent are sequentially added to the mixed solution to separate and obtain the cycloolefin polymer, the process comprising: After the hydrogenation reaction is terminated, the terminator is added to the mixed solution, and the temperature of the mixed solution is controlled to be 45-250°C, and the temperature of the mixed solution is controlled to be greater than or equal to the temperature of the ring-opening polymerization reaction, and after 1-60 minutes; the adsorbent is added thereto to remove the ruthenium catalyst; then the poor solvent is added thereto to precipitate the cycloolefin polymer, and the cycloolefin polymer is separated; wherein the molar ratio of the terminator to the ruthenium element in the mixed solution is (1-100):1; And / or, after the hydrogenation reaction is terminated, the terminator, the adsorbent and the poor solvent are sequentially added to the mixed solution to separate and obtain the cycloolefin polymer, the process comprising: After the hydrogenation reaction is terminated, the solution of the terminator, the adsorbent and the solution of the poor solvent are sequentially added to the mixed solution to separate and obtain the cycloolefin polymer; wherein the concentration of the terminator in the solution of the terminator is 0.001 to 10 mol / L; the solution of the poor solvent includes a pH adjuster, and the pH adjuster includes one or more of hydrochloric acid, sulfuric acid, lactic acid, acetic acid, sodium hydroxide, sodium carbonate, sodium bicarbonate, potassium hydroxide and potassium carbonate.
9. A cycloolefin polymer, It is characterized in that Obtained according to the preparation method according to any one of claims 1 to 8.
10. The cycloolefin polymer according to claim 9, It is characterized in that The cycloolefin polymer has a glass transition temperature of 100 to 300° C., a hydrogenation rate of unsaturated bonds of not less than 95%, and a refractive index of 1.5 to 2.1.
Citation Information
Patent Citations
Syndiotactic crystal tetracyclic [6.2. 1.13, 6.02, 7] dodeca-4-ene ring-opening polymer hydride and preparation method thereof
CN117050276A
Cyclic olefin ring-opening polymer hydride for medical apparatus and preparation method thereof
CN117417512A
Process for production of hydrogenated ring-opened metathesis polymers
CN1186080A
Cyclic olefin polymer, method for producing same, and optical element
CN114651026A
Cycloolefin ring-opening polymer hydride as well as preparation method and application thereof
CN117510796A
Cited By
Cycloolefin polymer, colored cycloolefin polymer film as well as preparation method and application of colored cycloolefin polymer film