Degradable copolyester with adjustable shelf life and degradation rate and main chain containing double bonds as well as preparation method and application of degradable copolyester

By introducing carbon-carbon double bond dibasic acids into the degradable polyester, the content of maleic acid and fumaric acid is regulated, and the problem of difficult regulation of degradation rate and shelf life in the prior art is solved, and the problem of different environments is realized controllable degradation and stable thermodynamic properties.

CN119019665APending Publication Date: 2024-11-26NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI

Patent Information

Application Number
CN202411112042.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The degradation rate of existing degradable polyester materials in non-compost environments is reduced, and the shelf life and degradation rate are difficult to regulate.

Method used

By introducing dibasic acids or their esterides containing carbon-carbon double bonds, the relative content of maleic acid and fumaric acid is controlled, and the three-dimensional structure of copolyester is regulated by the esterification reaction and polycondensation process to achieve shelf life and degradation rate. Adjustable.

Benefits of technology

The shelf life and degradation rate that can be adjusted in different environments is obtained, and the stable thermodynamic and mechanical properties of the material is maintained, and it is suitable for a variety of plastic products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019665A_ABST
    Figure CN119019665A_ABST
Patent Text Reader

Abstract

The invention discloses degradable copolyester with a main chain containing double bonds and adjustable shelf life and degradation rate as well as a preparation method and application of the degradable copolyester. The structural formula of the degradable copolyester with the double bonds in the main chain is as follows: # imgabs0 #,-R1-comprises a structural unit of cyclic dibasic acid or an ester thereof,-O-R2-O-comprises a structural unit of dihydric alcohol,-R3-comprises a structural unit of dibasic acid with double bonds or an ester thereof, and-R3-comprises a structural unit of dibasic acid with double bonds or an ester thereof; m and n are any integer from 1 to 5, and x is any integer from 15 to 200. The degradable copolyester material provided by the invention has good crystallization capacity, mechanical property and gas property, and can be widely applied to plastic products, the shelf life and degradation rate of the degradable copolyester material can be regulated and controlled along with the change of cis-trans content in a double-bond structure, and by utilizing the excellent controllable degradation property of degradable polyester, the degradable copolyester material can be widely applied to plastic products. The plastic pollution problem can be effectively solved, and the requirements of different application scenes for the shelf life and the degradation rate are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a main chain double-bond degradable copolyester with adjustable shelf life and degradation rate, and a preparation method and application thereof. Background Art

[0002] Degradable polyester materials in traditional technology include polylactic acid (PLA), polybutylene terephthalate adipate (PBAT), polybutylene succinate (PBS), etc. Although these degradable polyesters can achieve a high degradation rate in a composting environment, based on the hydrophobic properties of polyesters, once these degradable polyesters flow into natural environments such as oceans, rivers, and soil, their degradation rates will drop significantly. The shelf life of existing biodegradable polyesters is short and cannot be regulated, and the biodegradation rate only changes according to composting conditions. Maleic acid and fumaric acid are a pair of cis-trans isomers with different carbon-carbon double bond configurations. They are both aliphatic dibasic acids and can be used as degradation units in fat-aromatic copolyesters to enhance degradation capabilities. For maleic acid and fumaric acid polyesters, the stereostructure also plays a key role in determining the physical and chemical properties of the final polymer. Due to the influence of factors such as segment rigidity and steric hindrance in the stereostructure on the ester bond hydrolysis process, cis-maleic acid provides a faster degradation rate than trans-fumaric acid units. Therefore, by controlling the relative content of maleic acid and fumaric acid, the three-dimensional structure of the copolyester can be precisely regulated, thereby achieving regulation of the shelf life and degradation ability through polymerization methods.

[0003] However, the key challenge is to prevent maleic acid from transforming into a more stable fumaric acid during the polyester melt polycondensation process. The key factors affecting the rate of this transformation are the reaction temperature and reaction time. Under low temperature conditions, it is expected that the cis-trans isomerization process can be greatly curbed, thereby more accurately controlling the relative content of fumaric acid and maleic acid in the copolyester. Summary of the invention

[0004] The main purpose of the present invention is to provide a main chain double bond-containing degradable copolyester with adjustable shelf life and degradation rate and a preparation method thereof, so as to overcome the shortcomings of the prior art.

[0005] Another object of the present invention is to provide the application of the main chain double bond-containing degradable copolyester with adjustable shelf life and degradation rate.

[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0007] The embodiment of the present invention provides a main chain double bond-containing degradable copolyester with adjustable shelf life and degradation rate, and its structural formula is shown in formula (1):

[0008]

[0009] Among them, -R1- includes structural units of cyclic dibasic acids and / or cyclic dibasic acid esters, -O-R2-O- includes structural units of diols, and -R3- includes structural units of dibasic acids containing double bonds and / or dibasic acid esters containing double bonds; m is any integer from 1 to 5, n is any integer from 1 to 5, and x is any integer from 15 to 200.

[0010] In some embodiments, the structural unit containing a double-bond dibasic acid and / or a double-bond dibasic acid ester is selected from at least one of the following structures:

[0011]

[0012] The embodiment of the present invention also provides a method for preparing a main chain double-bond degradable copolyester with adjustable shelf life and degradation rate, which comprises:

[0013] (1) mixing a cyclic dibasic acid and / or a cyclic dibasic acid ester, a double-bond dibasic acid and / or a double-bond dibasic acid ester, a diol, and an esterification catalyst to form a first mixed system, and subjecting the first mixed system to an esterification reaction or an ester exchange reaction;

[0014] (2) mixing the product obtained in step (1) with a polymerization inhibitor and a polycondensation aid, and performing a polycondensation reaction to obtain a high molecular weight double bond-containing biodegradable copolyester preliminary product;

[0015] (3) heating the reaction system of step (2) and continuing the post-polycondensation reaction to obtain a main chain double-bond degradable copolyester with adjustable shelf life and degradation rate.

[0016] The embodiment of the present invention also provides a main chain double bond-containing degradable copolyester with adjustable shelf life and degradation rate, which is prepared by the above-mentioned preparation method.

[0017] The embodiment of the present invention also provides the use of the aforementioned main chain double bond-containing degradable copolyester with adjustable shelf life and degradation rate in plastic products.

[0018] Compared with the prior art, the beneficial effects of the present invention include:

[0019] The present invention provides a degradable copolyester material with controllable shelf life and degradation rate and stable comprehensive thermodynamic properties, which has good crystallization ability, mechanical properties and gas properties, and can be widely used in plastic products such as mulch films, fishing nets, plastic containers, packaging materials, drug sustained-release carriers and human implant components. In addition, its shelf life and degradation rate can be regulated as the cis-trans content in the double bond structure changes. By utilizing the excellent controllable degradation performance of degradable polyester, the problem of plastic pollution can be effectively addressed, and the requirements for shelf life and degradation rate in different application scenarios can be met. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 This is a H-NMR spectrum curve of the degradable polyester containing double bonds in the main chain prepared in Example 1 of the present invention;

[0022] Figure 2 is a DSC curve diagram of the main chain double bond-containing degradable polyester prepared in Example 1 of the present invention;

[0023] Figure 3 It is a stress-strain curve diagram of the degradable polyester containing double bonds in the main chain prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0024] In view of the problems existing in the above-mentioned prior art, after long-term research and a large number of experiments, the inventors of this case proposed a main chain double bond-containing degradable copolyester with adjustable shelf life and degradation rate and a preparation method thereof; the main chain double bond-containing degradable copolyester not only has stable and excellent mechanical properties and heat resistance, but can also be widely used in plastic products. Its shelf life and degradation rate can be regulated with the change of the cis and trans content in the double bond structure, thereby meeting the requirements of different application scenarios for the stability and degradation rate of degradable materials.

[0025] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0026] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used in the specification of the present invention herein are only for the purpose of describing specific implementation methods or embodiments and are not intended to limit the present invention.

[0027] As one aspect of the technical solution of the present invention, the structural formula of a main chain degradable copolyester containing double bonds with adjustable shelf life and degradation rate is shown in formula (1):

[0028]

[0029] Among them, -R1- includes structural units of cyclic dibasic acids and / or cyclic dibasic acid esters, -O-R2-O- includes structural units of diols, and -R3- includes structural units of dibasic acids containing double bonds and / or dibasic acid esters containing double bonds; wherein m, n, and x are all integers, m=1-5, n=1-5, and x=15-200.

[0030] In some embodiments, the molar ratio of -R1- to -R3- is 3:2 to 2:3.

[0031] The present invention introduces a structural unit (-R3-) of a dibasic acid or its esterification product containing a carbon-carbon double bond (-C=C-) into a molecular chain segment of a degradable polyester, which can synergize with a structural unit (-R1-) of a cyclic dibasic acid or its esterification product and a structural unit (-O-R2-O-) of a diol. On the one hand, the dibasic acid containing a carbon-carbon double bond is located in an amorphous region of the degradable copolyester, so that the change of its cis-trans isomers has little effect on the melting point, crystallization rate and mechanical properties of the copolyester, thereby maintaining the thermal and mechanical properties of the stability of the degradable copolyester. On the other hand, the difference in the stereo configuration of the dibasic acid of the cis-trans structure leads to different hydrolysis rates, the hydrolysis ability of the trans-fumaric acid structure is poor, and the hydrolysis rate of the cis-maleic acid is faster. This difference makes it possible to achieve different hydrolysis rates by regulating the relative content of the cis-trans structure, thereby achieving different shelf lives and degradation times under the same environment. By precisely controlling the polycondensation reaction conditions such as temperature and vacuum degree during the staged polycondensation process, the relative content of cis and trans structures can be precisely controlled, thereby achieving precise control of the shelf life and degradation rate of the copolyester material while retaining stable thermodynamic properties.

[0032] At the same time, the present invention reasonably designs the relative content of the structural unit (-R1-) and the structural unit (-R3-), maintains the content of cyclic dibasic acid in the total dibasic acid in the aliphatic aromatic copolyester material at 40%-60%, which is within the biodegradable composition range, and ensures that the adjustment of the cis-trans structure content of the dibasic acid does not affect the intrinsic biodegradability; the present invention reasonably selects short-chain aliphatic diols with strong crystallization ability to ensure that the main chain double-bond degradable copolyester has good crystallization ability, thereby having good thermal properties, mechanical properties and gas barrier properties, and has obvious performance advantages compared with commercial PBAT, PBS and other degradable materials.

[0033] Specifically, the reason why the double-bond copolyesters with different cis-trans contents in the present invention can maintain stable thermal properties and mechanical properties is that the thermal properties, crystallization ability and mechanical properties of the aliphatic-aromatic copolyesters are mainly affected by the content of the aromatic chain segments and the average chain segment length; and the double-bond dibasic acid, as an aliphatic dibasic acid, is mainly located in the aliphatic chain and amorphous region of the copolyester, and the change of its cis-trans structure does not affect the crystallization ability of the copolyester, thereby having little effect on the thermal properties, mechanical properties and other aspects of the copolyester.

[0034] Specifically, the reason why the present invention can accurately control the shelf life and storage stability of the copolyesters containing double bonds with different cis-trans contents is that the different spatial configurations of cis double-bond dibasic acids and trans double-bond dibasic acids lead to significant differences in the spatial steric hindrance of the ester bond hydrolysis process, which is reflected in the phenomenon of shelf life and degradation process that cis double-bond dibasic acid esters have a shorter shelf life and a faster degradation rate; while trans double-bond dibasic acid esters have a longer shelf life and a slower degradation rate.

[0035] In some embodiments, the structural unit containing a double bond dibasic acid and / or a double bond dibasic acid ester is selected from at least one of the following structures:

[0036]

[0037] Specifically, the main chain of the degradable copolyester containing double bonds has a cis structure and / or a trans structure; the cis structure is maleic acid and its esters; the trans structure is fumaric acid and its esters.

[0038] In some embodiments, the relative content of cis- and trans-structures in the main chain degradable copolyester containing double bonds can be precisely controlled according to the polymerization conditions and raw material ratio, wherein the content of cis-structure is 10% to 90%, and correspondingly, the content of trans-structure in the main chain degradable copolyester containing double bonds is 10% to 90%.

[0039] In order to further coordinate the thermal stability of the structural units of the dibasic acid or its esters with carbon-carbon double bonds (-C=C-), so that they meet the requirements of lower melt condensation temperature, so that the prepared polyester has a suitable melting point and crystallization rate, thereby giving the degradable polyester better heat resistance and mechanical properties.

[0040] In some embodiments, the structural unit of the cyclic dibasic acid and / or cyclic dibasic acid ester is a structural unit of a cyclic dibasic acid or its ester with better crystallization ability. Specifically, the structural unit of the cyclic dibasic acid and / or cyclic dibasic acid ester is selected from at least one of the following structures:

[0041]

[0042] In order to further coordinate the structural units of the dibasic acid or its esters containing carbon-carbon double bonds (-C=C-) and the structural units of the cyclic dibasic acid or its esters, diol units with stronger chain segment crystallization ability are used, thereby improving the overall crystallization ability of the copolyester and better achieving the regulation of the comprehensive properties of the polyester such as heat resistance, crystallization properties, and mechanical properties. The structural units of the diols are selected from the structural units of diols with 2 to 10 carbon atoms.

[0043] In some embodiments, the diol includes at least one of ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, octanediol, decanediol, and the like.

[0044] Among them, the diols can all give the copolyester good crystallization ability, and the aliphatic diols with different chain lengths can not only adjust the glass transition strength and tensile toughness of the polyester, but also reduce the chain segment steric hindrance of the polyester to increase the degradation rate of the polyester. The diol can be preferably selected from at least one of ethylene glycol, butanediol, hexanediol, octanediol, etc.

[0045] Therefore, the present invention can reasonably select the structural units of the dibasic acid or its esters of the dibasic acid containing a carbon-carbon double bond (-C=C-), the structural units of the cyclic dibasic acid or its esters, and the structural units of the diols according to the needs of different molecular structures to obtain degradable polyesters with different structural formulas.

[0046] In some more preferred embodiments, the structural formula of the degradable copolyester containing double bonds in the main chain is shown in formula (1-1):

[0047]

[0048] Here, m is any integer from 1 to 5, n is any integer from 1 to 5, y is any integer from 1 to 5, and z is any integer from 15 to 50.

[0049] In some embodiments, the main chain double bond-containing degradable copolyester has an intrinsic viscosity of 1.2-2.5 dL / g and a number average molecular weight of 40-120 KDa; according to the L*a*b* color model, the L* value is greater than 70, the a* absolute value is less than 5, and the b* absolute value is less than 7.

[0050] In some embodiments, the shelf life of the main chain double-bond-containing degradable copolyester can be controlled from 5 months to 20 months, and the degradation rate test method includes hydrolysis, enzyme degradation and composting degradation.

[0051] As one aspect of the technical solution of the present invention, a method for preparing a main chain double-bond degradable copolyester with adjustable shelf life and degradation rate comprises:

[0052] (1) mixing a cyclic dibasic acid and / or a cyclic dibasic acid ester, a double-bond dibasic acid and / or a double-bond dibasic acid ester, a diol, and an esterification catalyst to form a first mixed system, and subjecting the first mixed system to an esterification reaction or an ester exchange reaction;

[0053] (2) mixing the product obtained in step (1) with a polymerization inhibitor and a polycondensation aid, and performing a polycondensation reaction to obtain a high molecular weight double bond-containing biodegradable copolyester preliminary product;

[0054] (3) heating the reaction system of step (2) and continuing the post-polycondensation reaction to obtain a main chain double-bond degradable copolyester with adjustable shelf life and degradation rate.

[0055] In some embodiments, the esterification reaction or transesterification reaction is carried out at a temperature of 150° C. to 170° C. for a time of 4 h to 20 h in a protective atmosphere until the yield of byproduct water or methanol is at least 95%.

[0056] In some embodiments, the preparation method comprises: adding a polymerization inhibitor and a polycondensation aid to the product obtained in step (1), reducing the pressure of the reaction system to 5Pa to 200Pa, and conducting a polycondensation reaction at 170°C to 175°C, wherein the stable vacuum degree of the polycondensation reaction is less than or equal to 7Pa, and the polycondensation reaction time is 5 to 10 hours, to obtain a preliminary product of a degradable copolyester containing double bonds.

[0057] Furthermore, the number average molecular weight of the preliminary product of the double bond-containing degradable copolyester is 20 to 60 KDa, preferably 20 to 50 KDa.

[0058] In some embodiments, the preparation method comprises: heating the reaction system of step (2) to 180-185° C., continuing the post-condensation reaction, wherein the stable vacuum degree of the post-condensation reaction is less than or equal to 7 Pa, and the time of the post-condensation reaction is 0.5-3 hours, to obtain the main chain double bond-containing degradable copolyester with adjustable shelf life and degradation rate.

[0059] Among them, in one of some more preferred embodiments, a method for preparing a main chain double bond-containing degradable copolyester with adjustable shelf life and degradation rate comprises the following steps:

[0060] (1) mixing a cyclic dibasic acid or its esterified product, a double-bond dibasic acid or its esterified product, a diol and an esterification catalyst to form a first mixed system, and subjecting the first mixed system to an esterification reaction or an ester exchange reaction at 150 to 170° C. until the yield of byproduct water or methanol is at least 95%;

[0061] (2) adding a polymerization inhibitor and a polycondensation aid to the product of step (1), reducing the pressure of the reaction system to 5Pa to 200Pa, and conducting a polycondensation reaction at 170 to 175°C, wherein the stable vacuum degree of the polycondensation reaction is less than or equal to 7Pa, and the polycondensation reaction time is 5 to 10 hours, to obtain a preliminary product of a high molecular weight double-bond-containing biodegradable copolyester;

[0062] (3) The reaction system of step (2) is heated to 180-185° C., and a post-condensation reaction is continued. The stable vacuum degree of the post-condensation reaction is less than or equal to 7 Pa. The post-condensation reaction is carried out for 0.5-3 hours. The main chain degradable copolyester containing double bonds with different isomer ratios is obtained according to the post-condensation time.

[0063] In step (1), the carbon-carbon double bond dibasic acid or its esterified product can be obtained not only by a petroleum source route reaction, but also by a biomass fermentation method to obtain a high-purity double bond dibasic acid monomer, which is a fully bio-based dibasic acid monomer. In the esterification reaction, the double bond dibasic acid removes the hydroxyl group to form -R3-, and the double bond dibasic acid esterified product removes the alkoxy group to form -R3- in the transesterification reaction.

[0064] In some embodiments, in step (1), the double bond-containing dibasic acid and / or double bond-containing dibasic acid ester comprises at least one of fumaric acid, dimethyl fumarate, diethyl fumarate, dipropyl fumarate, dibutyl fumarate, maleic acid, dimethyl maleate, diethyl maleate, dipropyl maleate, dibutyl maleate, etc.

[0065] Furthermore, the double bond-containing dibasic acid and / or double bond-containing dibasic acid ester may preferably include at least one of fumaric acid, dimethyl fumarate, maleic acid, dimethyl maleate, and the like.

[0066] In some embodiments, the cyclic dibasic acid removes the hydroxyl group to form -R1- in the esterification reaction, and the esterified product of the cyclic dibasic acid removes the alkoxy group to form -R1- in the transesterification reaction. Specifically, the cyclic dibasic acid and / or the cyclic dibasic acid esterified product can be selected from at least one of 2,5-furandicarboxylic acid, 2,5-furandicarboxylic acid dimethyl ester, 2,5-furandicarboxylic acid diethyl ester, 2,5-thiophenedicarboxylic acid, 2,5-thiophenedicarboxylic acid dimethyl ester, 2,5-thiophenedicarboxylic acid diethyl ester, 1,4-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid dimethyl ester, 1,4-cyclohexanedicarboxylic acid diethyl ester, terephthalic acid, dimethyl terephthalate, diethyl terephthalate, isophthalic acid, dimethyl isophthalate, diethyl isophthalate, etc., but is not limited thereto.

[0067] Furthermore, the cyclic dibasic acid and / or cyclic dibasic acid ester may preferably include at least one of 2,5-furandicarboxylic acid, dimethyl 2,5-furandicarboxylate, 1,4-cyclohexanedicarboxylic acid, dimethyl 1,4-cyclohexanedicarboxylate, terephthalic acid, dimethyl terephthalate, and the like.

[0068] In some embodiments, the diol is dehydrogenated to form -O-R2-O- in the esterification reaction, and the diol is mostly dehydrogenated to form -O-R2-O- and / or -O-R3-O- in the transesterification reaction.

[0069] Specifically, the diol may include at least one of ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, octanediol, decanediol, etc., but is not limited thereto.

[0070] In some embodiments, in step (1), the molar ratio of the sum of the molar amounts of the cyclic dibasic acid and / or cyclic dibasic acid ester, the double-bond dibasic acid and / or double-bond dibasic acid ester to the diol is 1:1.1 to 1:1.5.

[0071] In some embodiments, in step (1), the mass fraction of the esterification catalyst in the first mixed system is 0.01% to 0.5%.

[0072] In some embodiments, in order to improve the reaction efficiency, an esterification catalyst is required during the esterification reaction, while an ester exchange catalyst is required during the ester exchange reaction.

[0073] It should be noted that the reaction process is not limited to a single esterification reaction or transesterification reaction. Depending on the type of cyclic dibasic acid or its esterification product, carbon-carbon double bond-containing dibasic acid or its esterification product, esterification reaction and transesterification reaction can exist simultaneously in the reaction process.

[0074] In some specific embodiments, the esterification catalyst includes at least one of a titanium-based catalyst, a Lewis acid catalyst, a germanium-based catalyst, and the like.

[0075] Furthermore, the titanium-based catalyst includes at least one of tetrabutyl titanate, isopropyl titanate, an inorganic supported titanium catalyst, etc.; the Lewis acid catalyst includes at least one of aluminum chloride, ferric chloride, boron trifluoride, niobium pentachloride, etc.; the germanium-based catalyst includes at least one of germanium dioxide, germanium acetate, etc.

[0076] In some embodiments, in step (2), the step of subjecting the product of step (1) to a condensation reaction further includes adding a polymerization inhibitor and a condensation aid to the product, wherein the condensation aid is selected from at least one of a condensation catalyst, a stabilizer, and the like.

[0077] In some embodiments, in step (2), the mass fraction of the polymerization inhibitor in the mixture of the product obtained in step (1) and the polycondensation aid is 0.5% to 3%.

[0078] Furthermore, the mass fraction of the polycondensation catalyst in the mixture of the product obtained in step (1) and the polycondensation aid is 0.01% to 0.5%.

[0079] Furthermore, the mass fraction of the stabilizer in the mixture of the product obtained in step (1) and the polycondensation aid is 0.01% to 0.5%.

[0080] Specifically, the polymerization inhibitor includes at least two of p-hydroxyanisole, hydroquinone, p-benzoquinone, oxidized diphosphoric acid, etc., preferably, it is selected from a mixture of p-hydroxyanisole and p-benzoquinone.

[0081] Furthermore, the mass fraction of the mixture of p-hydroxyanisole and p-benzoquinone in the mixture of the product obtained in step (1) and the polycondensation aid is 0.5% to 3%. The mixed inhibitor system can effectively prevent the cis-trans transformation from cis-maleate units to trans-fumarate units under reaction conditions below 175°C, and helps to accurately control the cis-trans isomerization composition of the double-bond copolyester pair.

[0082] Furthermore, the mass fraction of the p-hydroxyanisole in the mixture of the product obtained in step (1) and the polycondensation aid is 0.2% to 2%.

[0083] Furthermore, the mass fraction of the benzodiquinone in the mixture of the product obtained in step (1) and the polycondensation aid is 0.2% to 2%.

[0084] Specifically, the polycondensation catalyst includes at least one of a titanium-based catalyst, a germanium-based catalyst, and the like.

[0085] Furthermore, the stabilizer includes at least one of phosphorous acid, hypophosphorous acid, pyrophosphoric acid, ammonium phosphate, trimethyl phosphate, dimethyl phosphate, triphenyl phosphate, etc.

[0086] In some embodiments, the polycondensation reaction in step (2) of the present invention can stably maintain the structural stability of the maleic acid chain segment without cis-trans conversion; the post-polycondensation reaction in step (3) is carried out at a relatively high temperature of 185°C to achieve quantitative conversion of maleic acid to fumaric acid, and the cis-trans content can be accurately controlled according to the length of the post-polycondensation reaction time; taking the sum of the main chain double-bond dibasic acid structures as 100%, the main chain double-bond degradable copolyester has a cis-maleic acid content ranging from 0% to 90%; and a trans-fumaric acid content ranging from 10% to 100%.

[0087] In summary, the preparation method of the present invention conducts esterification reaction and / or transesterification reaction of cyclic dibasic acid or its esterification product, double-bond dibasic acid or its esterification product with diol, and through the synergistic effect between the components, it can not only make the double-bond dibasic acid or its esterification product realize efficient polymerization at a polycondensation temperature of 170-175°C, meet the high temperature requirements of polyester polymerization, obtain a high molecular weight preliminary polycondensation product, and curb the cis-trans isomerization transformation of the double-bond dibasic acid, so that its structural composition is similar to the feed ratio, effectively avoid the isomerization transformation of maleic acid to fumaric acid under high temperature melting conditions, and cause the real structural composition of the copolyester to be uncontrollable. And it can realize the precise control of double-bond cis-trans isomerization, and further give the degradable polyester stable and excellent thermal properties and mechanical properties, and can realize the control of shelf life and degradation rate.

[0088] As another aspect of the technical solution of the present invention, it also relates to a main chain double bond-containing degradable copolyester with adjustable shelf life and degradation rate, which is prepared by the above-mentioned preparation method.

[0089] As another aspect of the technical solution of the present invention, it also relates to the application of the aforementioned main chain double-bond degradable copolyester with adjustable shelf life and degradation rate in plastic products.

[0090] Specifically, the present invention provides a degradable copolyester material with controllable shelf life and degradation rate and stable comprehensive thermodynamic properties. The material has good crystallization ability, mechanical properties and gas properties, and can be widely used in plastic products such as mulch films, fishing nets, plastic containers, packaging materials, drug sustained-release carriers, and human implant components. In addition, by utilizing the excellent controllable degradation properties of degradable polyester, the problem of plastic pollution can be effectively addressed, and the requirements for shelf life and degradation rate in different application scenarios can be met.

[0091] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the biodegradable polyester and its preparation method, degradation method and application will be further described through the following specific examples. It should be understood that the specific examples described herein are only used to explain the present invention and are not used to limit the present invention; all variations associated with or derived from the contents disclosed in the present invention are considered to be within the scope of protection of the present invention.

[0092] In the following examples, a differential scanning calorimeter (Mettler Toledo DSC) was used to test thermal properties, wherein the heating rate was 10°C / min, the temperature range was -20°C-250°C, and the measurement was performed in a N2 atmosphere.

[0093] In the following examples, a Zwicki 1kN universal material testing machine was used to test the mechanical properties, wherein the sample strip dimensions were 15.0 mm in length, 2.0 mm in width, and 1.0 mm in thickness, and the tensile speed was 20 mm / min.

[0094] In the following examples, Labthink VAC-V2 was used to test the barrier properties of O2 and CO2, where O2 and CO2 were used as gas sources, respectively, and the measurements were performed at a temperature of 23°C and a humidity of 50% RH. The sample size was Φ = 97 mm, and the permeation area was 38.5 cm 2 .

[0095] In the following examples, phosphate buffer solution was used as the degradation solvent, and the hydrolysis degradation test was carried out at a constant temperature of 37° C., wherein the sample was 10 mm in length, 10 mm in width, and 0.5 mm in thickness.

[0096] In the following examples, a phosphate buffer solution containing 0.1 mg / ml lipase was used as a degradation solvent, and the enzyme degradation test was carried out at a constant temperature of 37° C., wherein the sample was 10 mm in length, 10 mm in width, and 0.5 mm in thickness.

[0097] Example 1

[0098] 0.5 mol of dimethyl furandicarboxylate, 0.4 mol of dimethyl maleate, 0.1 mol of dimethyl fumarate, 1.4 mol of 1,4-butanediol and 0.15 g of tetrabutyl titanate were put into a reactor. Under nitrogen protection, the temperature was raised to 150°C and reacted for 2 hours. The temperature was gradually raised to 170°C and the reaction was continued for 3 hours to obtain an intermediate product.

[0099] Continue to add 0.12g of germanium acetate and 0.15g of triphenyl phosphate, as well as 1.2g of p-hydroxyanisole and 1.3g of p-benzoquinone as inhibitors to the intermediate product, maintain the temperature at 170°C, continue to evacuate to maintain the vacuum degree of the reaction system below 5Pa, heat to 175°C for reaction for 5h, quickly heat to 185°C, maintain high vacuum for reaction for 1.5h, and obtain a light yellow main chain double bond-containing degradable copolyester, whose structure is shown in formula (1-1):

[0100]

[0101] Among them, m, n, and y are all integers, m=1-5, n=1-5, y=1-5, and z=15-50.

[0102] The prepared biodegradable copolyester containing double bonds in the main chain was tested by H NMR spectrum, DSC, mechanical properties, O2 and CO2 barrier properties, storage stability and degradation performance.

[0103] Figure 1 , Figure 2 , Figure 3 The following are the NMR hydrogen spectrum curve, DSC curve and stress-strain curve of the prepared main chain double-bond degradable polyester. Figure 1 It can be seen that the molecular structure of the main chain degradable polyester containing double bonds is clear, and the molar ratio of furandicarboxylic acid: fumaric acid: maleic acid in the dibasic acid composition is 50:32.5:17.5. Figure 2 It can be seen that the glass transition temperature of the degradable polyester containing double bonds in the main chain is 7.8°C and the melting point is 117°C. Figure 3 It can be seen that the elongation at break of the degradable polyester containing double bonds in the main chain is 325%.

[0104] According to tests, the tensile modulus of the biodegradable polyester containing double bonds in the main chain is 153 MPa, the tensile strength is 37.0 MPa, the CO2 permeability coefficient is 1.10 barrer, and the O2 permeability coefficient is 0.12 barrer.

[0105] According to tests, the intrinsic viscosity of the biodegradable polyester containing double bonds in the main chain is 1.5 dL / g; the number average molecular weight is 45 KDa; according to the L*a*b* color model, the L* value is 75, the a* value is 3.5, and the b* value is 3.7.

[0106] The test showed that the main chain double bond degradable polyester had a mass loss of 27.5% by enzyme degradation within 28 days and a mass loss of 2.7% by hydrolysis within 28 days. After 7 months of storage, the number average molecular weight of the compression molded sample dropped to 88% of the original number average molecular weight, and the tensile strength remained 90% of the original tensile strength.

[0107] Example 2

[0108] 0.5 mol of terephthalic acid, 0.5 mol of maleic acid, 1.25 mol of ethylene glycol and 0.18 g of isopropyl titanate were put into a reactor. Under nitrogen protection, the temperature was raised to 150°C and reacted for 3 hours. The temperature was gradually raised to 170°C and the reaction was continued for 2 hours to obtain an intermediate product.

[0109] 0.06 g of germanium dioxide, 0.08 g of tetrabutyl titanate and 0.15 g of trimethyl phosphate, as well as 1.1 g of hydroquinone and 1.5 g of benzoquinone as inhibitors were added to the intermediate product, the temperature was raised to 175 ° C, and the vacuum was continuously drawn to maintain the vacuum degree of the reaction system below 5 Pa. After reacting for 6 hours, the temperature was quickly raised to 185 ° C, and the high vacuum degree was maintained for 0.5 hours to obtain a white main chain double bond-containing degradable copolyester, whose structure is shown in formula (1-2):

[0110]

[0111] Among them, m, n, and y are all integers, m=1-5, n=1-5, y=1-5, and z=15-50.

[0112] According to the test, the molar ratio of terephthalic acid: fumaric acid: maleic acid in the dibasic acid composition of the degradable polyester is 50:5:45. The glass transition temperature of the degradable polyester is -10.5°C and the melting point is 135°C. According to the test, the tensile modulus of the degradable polyester is 159.5MPa, the tensile strength is 35.2MPa, and the elongation at break of the degradable polyester is 285%. The CO2 permeability coefficient is 1.8barrer, and the O2 permeability coefficient is 0.35barrer.

[0113] According to the test, the intrinsic viscosity of the biodegradable polyester containing double bonds in the main chain is 1.45 dL / g; the number average molecular weight is 43 KDa; according to the L*a*b* color model, the L* value is 78, the a* value is 4.2, and the b* value is 4.7.

[0114] The test showed that the main chain double bond degradable polyester had a mass loss of 32% by enzyme degradation within 28 days and a mass loss of 5.8% by hydrolysis within 28 days. After 5 months of storage, the number average molecular weight of the compression molded sample dropped to 87% of the original number average molecular weight, and the tensile strength remained 85% of the original tensile strength.

[0115] Example 3

[0116] 0.55 mol of 2,5-thiophenedicarboxylic acid, 0.25 mol of fumaric acid, 0.2 mol of maleic acid, 1.1 mol of 1,6-hexanediol and 0.2 g of aluminum chloride were put into the reactor. Under nitrogen protection, the temperature was raised to 160°C and reacted for 3 hours. The temperature was gradually raised to 170°C and the reaction was continued for 2 hours to obtain an intermediate product.

[0117] Continue to add 0.05g of germanium dioxide, 0.10g of isopropyl titanate and 0.18g of pyrophosphoric acid, as well as 0.5g of p-hydroxyanisole and 3.5g of oxidized diphosphoric acid as inhibitors to the intermediate product, raise the temperature to 175°C, and continue to evacuate to maintain the vacuum degree of the reaction system below 7Pa. After reacting for 6h, quickly raise the temperature to 180°C and maintain high vacuum for 3h to obtain a white main chain degradable copolyester containing double bonds.

[0118] According to the test, the molar ratio of thiophenedicarboxylic acid: fumaric acid: maleic acid in the dibasic acid composition of the degradable polyester is 55:35:10. The glass transition temperature of the degradable polyester is 2.5°C and the melting point is 135°C. According to the test, the tensile modulus of the degradable polyester is 237.6MPa, the tensile strength is 37.2MPa, and the elongation at break of the degradable polyester is 435%. The CO2 permeability coefficient is 0.8barrer, and the O2 permeability coefficient is 0.115barrer.

[0119] According to tests, the intrinsic viscosity of the biodegradable polyester containing double bonds in the main chain is 1.7 dL / g; the number average molecular weight is 58 KDa; according to the L*a*b* color model, the L* value is 80, the a* value is 4.2, and the b* value is 5.5.

[0120] The test showed that the degradation mass loss of the main chain double-bond degradable polyester was 19.5% in 28 days by enzyme degradation and 1.8% in 28 days by hydrolysis. After 10 months of storage, the number average molecular weight of the compression molded sample dropped to 95% of the original number average molecular weight, and the tensile strength remained 89% of the original tensile strength.

[0121] Example 4

[0122] 0.4 mol of diethyl isophthalate, 0.4 mol of diethyl fumarate, 0.2 mol of diethyl maleate, 1.5 mol of 1,4-butanediol, 0.1 of aluminum chloride and 0.08 g of tetrabutyl titanate were put into a reactor. Under nitrogen protection, the temperature was raised to 160°C and reacted for 3 hours. The temperature was gradually raised to 170°C and the reaction was continued for 4 hours to obtain an intermediate product.

[0123] 0.15 g of isopropyl titanate and 0.18 g of hypophosphorous acid, as well as 1.5 g of p-hydroxyanisole and 0.3 g of p-benzoquinone were added to the intermediate product as polymerization inhibitors, and vacuum was continuously drawn at 170 ° C to maintain the vacuum degree of the reaction system below 6 Pa. After reacting for 6.5 hours, the temperature was quickly raised to 183 ° C. After reacting for 3 hours, a white main chain double-bond degradable copolyester was obtained, and its structure is shown in formula (1-3):

[0124]

[0125] Among them, m, n, and y are all integers, m=1-5, n=1-5, y=1-5, and z=15-50.

[0126] According to the test, the molar ratio of isophthalic acid: fumaric acid: maleic acid in the dibasic acid composition of the degradable polyester is 40:52:8. The glass transition temperature of the degradable polyester is -17.6°C and the melting point is 55°C. According to the test, the tensile modulus of the degradable polyester is 57.2MPa, the tensile strength is 7.2MPa, the elongation at break of the degradable polyester is 835%, the CO2 permeability coefficient is 2.5barrer, and the O2 permeability coefficient is 0.85barrer.

[0127] According to tests, the intrinsic viscosity of the biodegradable polyester containing double bonds in the main chain is 1.75 dL / g; the number average molecular weight is 80 KDa; according to the L*a*b* color model, the L* value is 78, the a* value is 2.5, and the b* value is 2.7.

[0128] The test showed that the degradation mass loss of the main chain double-bond degradable polyester was 10% in 28 days due to enzymatic degradation and 1.5% in 28 days due to hydrolysis. After 15 months of storage, the number average molecular weight of the compression molded sample dropped to 92.5% of the original number average molecular weight, and the tensile strength remained at 93.3% of the original tensile strength.

[0129] Example 5

[0130] 0.48 mol of dimethyl terephthalate, 0.22 mol of dimethyl maleate, 0.3 mol of dimethyl fumarate, 1.25 mol of butanediol, 0.2 g of tetrabutyl titanate and 0.1 g of boron trifluoride were put into a reactor. Under nitrogen protection, the temperature was raised to 155°C and the reaction was carried out for 3.5 hours. The temperature was gradually raised to 170°C and the reaction was continued for 2.5 hours until the methanol content reached 98% of the theoretical value to obtain an intermediate product.

[0131] Continue to add 0.10g of tetrabutyl titanate and 0.15g of phosphorous acid, as well as 1.3g of p-hydroxyanisole and 1.6g of p-benzoquinone as inhibitors to the intermediate product, heat to 175°C, continue to evacuate to maintain the vacuum degree of the reaction system below 7Pa, react for 5.5h, quickly heat to 180°C, maintain high vacuum for 2.3h, and obtain a light yellow main chain double bond-containing degradable copolyester, whose structure is shown in formula (1-4):

[0132]

[0133] Among them, m, n, and y are all integers, m=1-5, n=1-5, y=1-5, and z=15-50.

[0134] According to the test, the molar ratio of terephthalic acid: fumaric acid: maleic acid in the dibasic acid composition of the degradable polyester is 48:10:42. The glass transition temperature of the degradable polyester is -14.3°C and the melting point is 114.5°C. According to the test, the tensile modulus of the degradable polyester is 99.8MPa, the tensile strength is 20.8MPa, and the elongation at break of the degradable polyester is 457%. The CO2 permeability coefficient is 1.2barrer, and the O2 permeability coefficient is 0.77barrer.

[0135] After testing, the intrinsic viscosity of the biodegradable polyester containing double bonds in the main chain is 1.55 dL / g; the number average molecular weight is 48.5 KDa; according to the L*a*b* color model, the L* value is 76, the a* value is 2.5, and the b* value is 2.77.

[0136] The test showed that the main chain double bond degradable polyester had a mass loss of 21% by enzyme degradation within 28 days and a mass loss of 1.8% by hydrolysis within 28 days. After 9 months of storage, the number average molecular weight of the compression molded sample dropped to 92% of the original number average molecular weight, and the tensile strength remained 88% of the original tensile strength.

[0137] Example 6

[0138] 0.52 mol of dimethyl terephthalate, 0.42 mol of dimethyl maleate, 0.06 mol of dimethyl fumarate, 1.35 mol of butanediol, 0.15 g of tetrabutyl titanate and 0.1 g of ferric chloride were put into a reactor. Under nitrogen protection, the temperature was raised to 158°C and the reaction was carried out for 3.5 hours. The temperature was gradually raised to 160°C and the reaction was continued for 3 hours until the methanol content reached 97% of the theoretical value to obtain an intermediate product.

[0139] Continue to add 0.15g of tetrabutyl titanate and 0.12g of phosphorous acid, as well as 1.5g of p-hydroxyanisole and 1.3g of p-benzoquinone as inhibitors to the intermediate product, heat to 175°C, continue to evacuate to maintain the vacuum degree of the reaction system below 6Pa, after reacting for 10h, quickly heat to 180°C, maintain high vacuum degree for 0.6h, and obtain a light yellow main chain containing double bonds and degradable copolyester, whose structure is shown in formula (1-5):

[0140]

[0141] Among them, m, n, and y are all integers, m=1-5, n=1-5, y=1-5, and z=15-50.

[0142] According to the test, the molar ratio of terephthalic acid: fumaric acid: maleic acid in the dibasic acid composition of the degradable polyester is 52:40:8. The glass transition temperature of the degradable polyester is -17.3°C and the melting point is 125.7°C. According to the test, the tensile modulus of the degradable polyester is 113.8MPa, the tensile strength is 25.8MPa, the elongation at break of the degradable polyester is 453%, the CO2 permeability coefficient is 0.96barrer, and the O2 permeability coefficient is 0.55barrer.

[0143] After testing, the intrinsic viscosity of the biodegradable polyester containing double bonds in the main chain is 1.98 dL / g; the number average molecular weight is 108.5 KDa; according to the L*a*b* color model, the L* value is 85.2, the a* value is 2.7, and the b* value is 3.9.

[0144] The test showed that the main chain double bond degradable polyester had a mass loss of 32% by enzyme degradation within 28 days and a mass loss of 4.6% by hydrolysis within 28 days. After 6 months of storage, the number average molecular weight of the compression molded sample dropped to 86% of the original number average molecular weight, and the tensile strength remained 85% of the original tensile strength.

[0145] Example 7

[0146] 0.50 mol of dimethyl terephthalate, 0.32 mol of dimethyl maleate, 0.18 mol of dimethyl fumarate, 1.40 mol of butanediol, 0.13 g of tetrabutyl titanate and 0.15 g of ferric chloride were put into a reactor. Under nitrogen protection, the temperature was raised to 160°C and the reaction was carried out for 3.5 hours. The temperature was gradually raised to 170°C and the reaction was continued for 16.5 hours until the methanol content reached 98% of the theoretical value to obtain an intermediate product.

[0147] Continue to add 0.17g of tetrabutyl titanate, 0.11g of germanium dioxide and 0.15g of phosphorous acid, as well as 1.5g of p-hydroxyanisole and 1.3g of p-benzoquinone as inhibitors to the intermediate product, heat to 175°C, continue to evacuate to maintain the vacuum degree of the reaction system below 6Pa, react for 5h, quickly heat to 180°C, maintain high vacuum for 0.5h, and obtain a light yellow main chain double bond-containing degradable copolyester, whose structure is shown in formula (1-6):

[0148]

[0149] Among them, m, n, and y are all integers, m=1-5, n=1-5, y=1-5, and z=15-50.

[0150] According to the test, the molar ratio of terephthalic acid: fumaric acid: maleic acid in the dibasic acid composition of the degradable polyester is 52: 29.8: 18.2. The glass transition temperature of the degradable polyester is -17.3°C and the melting point is 125.7°C. According to the test, the tensile modulus of the degradable polyester is 108.5MPa, the tensile strength is 29.8MPa, and the elongation at break of the degradable polyester is 447%. The CO2 permeability coefficient is 0.85barrer, and the O2 permeability coefficient is 0.32barrer.

[0151] After testing, the intrinsic viscosity of the biodegradable polyester containing double bonds in the main chain is 2.2 dL / g; the number average molecular weight is 115.5 KDa; according to the L*a*b* color model, the L* value is 84.5, the a* value is 1.7, and the b* value is 2.9.

[0152] The test showed that the degradation mass loss of the main chain double-bond degradable polyester was 29.8% in 28 days due to enzymatic degradation and 5.8% in 28 days due to hydrolysis. After eight months of storage, the number average molecular weight of the compression molded sample dropped to 87.5% of the original number average molecular weight, and the tensile strength remained at 83.5% of the original tensile strength.

[0153] Example 8

[0154] 0.50 mol of diethyl 1,4-cyclohexanedicarboxylate, 0.4 mol of diethyl maleate, 0.1 mol of diethyl fumarate, 1.40 mol of butanediol, 0.15 g of tetrabutyl titanate and 0.13 g of niobium pentachloride were put into a reactor. Under nitrogen protection, the temperature was raised to 160° C. and reacted for 3.5 hours. The temperature was gradually raised to 170° C. and the reaction was continued for 0.5 hours until the ethanol content reached 98% of the theoretical value to obtain an intermediate product.

[0155] Continue to add 0.17g of tetrabutyl titanate, 0.18g of germanium acetate and 0.15g of ammonium phosphate, as well as 1.15g of p-hydroxyanisole and 1.65g of p-benzoquinone as inhibitors to the intermediate product, heat to 175°C, continue to evacuate to maintain the vacuum degree of the reaction system below 5Pa, after reacting for 5h, quickly heat to 182°C, maintain high vacuum degree for reaction for 3h, and obtain a white main chain containing double bonds and degradable copolyester, whose structure is shown in formula (1-7):

[0156]

[0157] Among them, m, n, and y are all integers, m=1-5, n=1-5, y=1-5, and z=15-50.

[0158] According to the test, the molar ratio of 1.4-cyclohexanedicarboxylic acid: fumaric acid: maleic acid in the dibasic acid composition of the degradable polyester is 50:35:15. The glass transition temperature of the degradable polyester is -27.3°C and the melting point is 120.7°C. According to the test, the tensile modulus of the degradable polyester is 128.5MPa, the tensile strength is 35.8MPa, the elongation at break of the degradable polyester is 688.5%, the CO2 permeability coefficient is 1.50barrer, and the O2 permeability coefficient is 0.62barrer.

[0159] According to the test, the intrinsic viscosity of the biodegradable polyester containing double bonds in the main chain is 1.8 dL / g; the number average molecular weight is 98.5 KDa; according to the L*a*b* color model, the L* value is 82.5, the a* value is 3.9, and the b* value is 3.9.

[0160] The test showed that the degradation mass loss of the main chain double-bond degradable polyester was 27.8% in 28 days due to enzymatic degradation and 6.8% in 28 days due to hydrolysis. After 6 months of storage, the number average molecular weight of the compression molded sample dropped to 82.5% of the original number average molecular weight, and the tensile strength remained 78.5% of the original tensile strength.

[0161] Example 9

[0162] 0.50 mol of dimethyl terephthalate, 0.32 mol of dimethyl maleate, 0.18 mol of dimethyl fumarate, 1.350 mol of propylene glycol and 0.3 g of tetrabutyl titanate were put into a reactor. Under nitrogen protection, the temperature was raised to 160°C and reacted for 3 hours. The temperature was gradually raised to 170°C and the reaction was continued for 5 hours until the methanol content reached 96% of the theoretical value to obtain an intermediate product.

[0163] Continue to add 0.15g of tetrabutyl titanate, 0.15g of germanium dioxide and 0.2g of phosphorous acid, as well as 1.5g of p-hydroxyanisole and 1.3g of p-benzoquinone as inhibitors to the intermediate product, raise the temperature to 175°C, and continue to evacuate to maintain the vacuum degree of the reaction system below 6Pa. After reacting for 5 hours, quickly heat up to 180°C, maintain high vacuum for reaction for 1.5 hours, and obtain a light yellow main chain degradable copolyester containing double bonds.

[0164] According to the test, the molar ratio of terephthalic acid: fumaric acid: maleic acid in the dibasic acid composition of the degradable polyester is 51.5:33.5:15.0. The glass transition temperature of the degradable polyester is -15.3°C and the melting point is 128.7°C. According to the test, the tensile modulus of the degradable polyester is 115.5MPa, the tensile strength is 23.8MPa, and the elongation at break of the degradable polyester is 350%. The CO2 permeability coefficient is 0.75barrer, and the O2 permeability coefficient is 0.28barrer.

[0165] After testing, the intrinsic viscosity of the biodegradable polyester containing double bonds in the main chain is 1.8 dL / g; the number average molecular weight is 105.5 KDa; according to the L*a*b* color model, the L* value is 83.5, the a* value is 1.8, and the b* value is 2.7.

[0166] The test showed that the degradation mass loss of the main chain double-bond degradable polyester was 23.3% in 28 days due to enzymatic degradation and 4.5% in 28 days due to hydrolysis. After eight months of storage, the number average molecular weight of the compression molded sample dropped to 82.5% of the original number average molecular weight, and the tensile strength remained at 85.5% of the original tensile strength.

[0167] Example 10

[0168] 0.50 mol of dimethyl terephthalate, 0.5 mol of dimethyl maleate, 1.35 mol of octanediol and 0.3 g of tetrabutyl titanate were put into a reactor. Under nitrogen protection, the temperature was raised to 160°C and the reaction was carried out for 3 hours. The temperature was gradually raised to 170°C and the reaction was continued for 5.5 hours until the methanol content reached 97% of the theoretical value to obtain an intermediate product.

[0169] Continue to add 0.15g of tetrabutyl titanate, 0.15g of germanium dioxide and 0.2g of phosphorous acid, as well as 1.5g of p-hydroxyanisole and 1.3g of p-benzoquinone as inhibitors to the intermediate product, raise the temperature to 175°C, and continue to evacuate to maintain the vacuum degree of the reaction system below 6Pa. After reacting for 5h, quickly raise the temperature to 180°C, maintain high vacuum for 0.5h, and obtain a white main chain degradable copolyester containing double bonds.

[0170] According to the test, the molar ratio of terephthalic acid: fumaric acid: maleic acid in the dibasic acid composition of the degradable polyester is 50.0:5.0:45.0. The glass transition temperature of the degradable polyester is -35.3°C and the melting point is 105.7°C. According to the test, the tensile modulus of the degradable polyester is 105.5MPa, the tensile strength is 19.8MPa, and the elongation at break of the degradable polyester is 850%. The CO2 permeability coefficient is 1.25barrer, and the O2 permeability coefficient is 0.50barrer.

[0171] After testing, the intrinsic viscosity of the biodegradable polyester containing double bonds in the main chain is 1.95 dL / g; the number average molecular weight is 108.8 KDa; according to the L*a*b* color model, the L* value is 87.5, the a* value is 2.5, and the b* value is 1.7.

[0172] The test showed that the main chain double bond degradable polyester had a mass loss of 15.3% by enzyme degradation within 28 days and a mass loss of 2.5% by hydrolysis within 28 days. After eight months of storage, the number average molecular weight of the compression molded sample dropped to 87.5% of the original number average molecular weight, and the tensile strength remained at 88.5% of the original tensile strength.

[0173] Embodiment 11

[0174] 0.50 mol of dimethyl terephthalate, 0.32 mol of dimethyl maleate, 0.18 mol of dimethyl fumarate, 1.350 mol of decanediol and 0.3 g of tetrabutyl titanate were put into a reactor. Under nitrogen protection, the temperature was raised to 160°C and reacted for 3 hours. The temperature was gradually raised to 170°C and the reaction was continued for 5.5 hours until the methanol content reached 97% of the theoretical value to obtain an intermediate product.

[0175] Continue to add 0.15g of tetrabutyl titanate, 0.15g of germanium dioxide and 0.2g of phosphorous acid, as well as 1.55g of p-hydroxyanisole and 1.55g of p-benzoquinone as inhibitors to the intermediate product, raise the temperature to 175°C, continue to evacuate to maintain the vacuum degree of the reaction system below 5Pa, after reacting for 4h, quickly raise the temperature to 180°C, maintain high vacuum for reaction for 1.8h, and obtain a white main chain degradable copolyester containing double bonds.

[0176] According to the test, the molar ratio of terephthalic acid: fumaric acid: maleic acid in the dibasic acid composition of the degradable polyester is 51.5:37.5:12.0. The glass transition temperature of the degradable polyester is -45.3°C and the melting point is 98.5°C. According to the test, the tensile modulus of the degradable polyester is 135.7MPa, the tensile strength is 23.0MPa, and the elongation at break of the degradable polyester is 950%. The CO2 permeability coefficient is 1.45barrer, and the O2 permeability coefficient is 0.60barrer.

[0177] After testing, the intrinsic viscosity of the biodegradable polyester containing double bonds in the main chain is 1.87 dL / g; the number average molecular weight is 122.8 KDa; according to the L*a*b* color model, the L* value is 85.5, the a* value is 1.5, and the b* value is 0.5.

[0178] The test showed that the main chain double bond degradable polyester had a mass loss of 12.8% by enzyme degradation within 28 days and a mass loss of 1.8% by hydrolysis within 28 days. After eight months of storage, the number average molecular weight of the compression molded sample dropped to 87.5% of the original number average molecular weight, and the tensile strength remained at 90.5% of the original tensile strength.

[0179] Comparative Example 1

[0180] The difference between this comparative example and Example 1 is that 0.4 mol of dimethyl fumarate is used instead of 0.4 mol of dimethyl maleate.

[0181] The test showed that the polyester had a mass loss of 12.5% ​​by enzyme degradation within 28 days, and had no mass loss by hydrolysis within 28 days.

[0182] The double-bond dibasic acids in Comparative Example 1 are all trans-fumaric acid structures, and their high rigidity and high steric hindrance are not conducive to the enzymatic degradation and hydrolysis of the copolyester. Therefore, under the same degradation conditions and the same degradation time, compared with Example 1, the enzymatic degradation mass loss of Comparative Example 1 is reduced from 27.5% to 12.5%, and the hydrolysis mass loss is reduced from 2.7% to 0.

[0183] Comparative Example 2

[0184] The difference between this comparative example and Example 1 is that 0.4 mol of dimethyl succinate is used instead of 0.4 mol of dimethyl maleate.

[0185] According to the test, the polyester had a mass loss of 26% due to enzymatic degradation within 28 days, and a mass loss of 5% due to hydrolysis within 28 days.

[0186] The aliphatic dibasic acid in Comparative Example 2 does not contain a double bond and has a faster degradation rate than that in Example 1, but its degradation rate cannot be controlled.

[0187] Comparative Example 3

[0188] The difference between this comparative example and Example 1 is that the raw materials are changed to 0.8 mol of dimethyl furandicarboxylate, 0.2 mol of dimethyl maleate and 1.4 mol of 1,4-butanediol.

[0189] According to tests, the polyester had a mass loss of 0% due to enzymatic degradation within 28 days and a mass loss of 0% due to hydrolysis within 28 days.

[0190] In Comparative Example 3, the molar ratio of R1 to R3 is 4:1, and the cyclic dibasic acid content is too high, resulting in the copolyester being non-degradable.

[0191] Comparative Example 4

[0192] The difference between this comparative example and Example 1 is that no polymerization inhibitor is added.

[0193] The polycondensation product was tested to be a cross-linked solid mass, indicating that a side reaction occurred during the polycondensation process and the thermoplastic polyester could not be prepared.

[0194] Comparative Example 5

[0195] The difference between this comparative example and Example 1 is that the polycondensation temperature is 185° C. and the polycondensation time is 6 h.

[0196] The test showed that the molar ratio of furandicarboxylic acid: fumaric acid: maleic acid was 50:48.5:1.5, indicating that most of the maleic acid structure had been converted into fumaric acid structure, and the cis-trans composition of the dibasic acid segment in the copolyester could not be effectively controlled.

[0197] Comparative Example 6

[0198] The difference between this comparative example and Example 1 is that after rapidly heating to 185° C., a high vacuum degree (greater than 7 Pa) is maintained for reaction for 2.5 h.

[0199] The test showed that the molar ratio of furandicarboxylic acid: fumaric acid: maleic acid was 50:39.5:10.5, indicating that the cis-trans composition of the dibasic acid in the copolyester can be effectively regulated by changing the reaction time at 185°C.

[0200] The copolyester was tested to have a mass loss of 21.5% by enzyme degradation within 28 days and a mass loss of 1.8% by hydrolysis within 28 days. After 8.5 months of storage, the number average molecular weight of the compression molded sample dropped to 89% of the original number average molecular weight, and the tensile strength remained at 92% of the original tensile strength.

[0201] It can be seen from Examples 1-8 and Comparative Examples 1-6 that by coordinating the structural units of the cyclic dibasic acid or its ester, the structural units of the dibasic acid or its ester containing carbon-carbon double bonds, and the structural units of the diol in the polyester structure, the cis-trans isomer composition of the double-bond dibasic acid in the final product can be effectively controlled by regulating the reaction time of the 185°C polycondensation stage during the polycondensation process, thereby ensuring that the copolyester has good and stable thermal properties, mechanical properties and barrier properties, while regulating the shelf life and degradation rate of the copolyester.

[0202] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

Claims

1. A main chain double bond-containing degradable copolyester with adjustable shelf life and degradation rate, characterized in that: The structural formula of the main chain double-bond degradable copolyester with adjustable shelf life and degradation rate is shown in formula (1): Among them, -R1- includes structural units of cyclic dibasic acids and / or cyclic dibasic acid esters, -O-R2-O- includes structural units of diols, and -R3- includes structural units of dibasic acids containing double bonds and / or dibasic acid esters containing double bonds; m is any integer from 1 to 5, n is any integer from 1 to 5, and x is any integer from 15 to 200.

2. The main chain double-bond degradable copolyester with adjustable shelf life and degradation rate according to claim 1, characterized in that: The molar ratio of -R1- to -R3- is 3:2 to 2:3; And / or, the structural unit of the double-bond-containing dibasic acid and / or double-bond-containing dibasic acid ester is selected from at least one of the following structures: And / or, the main chain degradable copolyester containing double bonds has a cis structure and / or a trans structure; preferably, the content of the cis structure in the main chain degradable copolyester containing double bonds is 10% to 90%, preferably, the content of the trans structure in the main chain degradable copolyester containing double bonds is 10% to 90%.

3. The main chain double-bond degradable copolyester with adjustable shelf life and degradation rate according to claim 1, characterized in that: The structural unit of the cyclic dibasic acid and / or cyclic dibasic acid ester is selected from at least one of the following structures: And / or, the structural unit of the diol includes a structural unit of a diol with 2 to 10 carbon atoms; preferably, the diol includes at least one of ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, octanediol, and decanediol, and is particularly preferably at least one of ethylene glycol, butylene glycol, hexylene glycol, and octanediol.

4. The main chain double-bond degradable copolyester with adjustable shelf life and degradation rate according to claim 1, characterized in that: The structural formula of the degradable copolyester containing double bonds in the main chain is shown in formula (1-1): Wherein, m is any integer from 1 to 5, n is any integer from 1 to 5, y is any integer from 1 to 5, and z is any integer from 15 to 50; And / or, the main chain of the degradable copolyester containing double bonds has an intrinsic viscosity of 1.2 to 2.5 dL / g and a number average molecular weight of 40 to 120 KDa; And / or, the shelf life of the degradable copolyester containing double bonds in the main chain can be adjusted from 5 months to 20 months.

5. A method for preparing a main chain double-bond degradable copolyester with adjustable shelf life and degradation rate, characterized in that: include: (1) mixing a cyclic dibasic acid and / or a cyclic dibasic acid ester, a double-bond dibasic acid and / or a double-bond dibasic acid ester, a diol, and an esterification catalyst to form a first mixed system, and subjecting the first mixed system to an esterification reaction or an ester exchange reaction; (2) mixing the product obtained in step (1) with a polymerization inhibitor and a polycondensation aid, and performing a polycondensation reaction to obtain a high molecular weight double bond-containing biodegradable copolyester preliminary product; (3) heating the reaction system of step (2) and continuing the post-polycondensation reaction to obtain a main chain double-bond degradable copolyester with adjustable shelf life and degradation rate.

6. The preparation method according to claim 5, characterized in that: The molar ratio of the sum of the molar amounts of the cyclic dibasic acid and / or cyclic dibasic acid ester, the double-bond dibasic acid and / or double-bond dibasic acid ester to the diol is 1:1.1 to 1:1.5; And / or, the double-bond-containing dibasic acid and / or double-bond-containing dibasic acid ester comprises at least one of fumaric acid, dimethyl fumarate, diethyl fumarate, dipropyl fumarate, dibutyl fumarate, maleic acid, dimethyl maleate, diethyl maleate, dipropyl maleate, and dibutyl maleate, preferably comprises at least one of fumaric acid, dimethyl fumarate, maleic acid, and dimethyl maleate; and / or, the cyclic dibasic acid and / or cyclic dibasic acid ester include 2,5-furandicarboxylic acid, dimethyl 2,5-furandicarboxylate, diethyl 2,5-furandicarboxylate, 2,5-thiophenedicarboxylic acid, dimethyl 2,5-thiophenedicarboxylate, diethyl 2,5-thiophenedicarboxylate, 1,4-cyclohexanedicarboxylic acid, dimethyl 1,4-cyclohexanedicarboxylate, 1,4-cyclohexanedicarboxylic acid At least one of diethyl ester, terephthalic acid, dimethyl terephthalate, diethyl terephthalate, isophthalic acid, dimethyl isophthalate, and diethyl isophthalate, preferably at least one of 2,5-furandicarboxylic acid, dimethyl 2,5-furandicarboxylate, 1,4-cyclohexanedicarboxylic acid, dimethyl 1,4-cyclohexanedicarboxylate, terephthalic acid, and dimethyl terephthalate; And / or, the diol includes a diol having 2 to 10 carbon atoms, preferably, the diol includes at least one of ethylene glycol, propylene glycol, butylene glycol, hexylene glycol, octanediol, and decanediol, and particularly preferably at least one of ethylene glycol, butylene glycol, hexylene glycol, and octanediol; And / or, the esterification catalyst includes at least one of a titanium catalyst, a Lewis acid catalyst, and a germanium catalyst; preferably, the titanium catalyst includes at least one of tetrabutyl titanate, isopropyl titanate, and an inorganic supported titanium catalyst; preferably, the Lewis acid catalyst includes at least one of aluminum chloride, ferric chloride, boron trifluoride, and niobium pentachloride; preferably, the germanium catalyst includes at least one of germanium dioxide and germanium acetate; And / or, the mass fraction of the esterification catalyst in the first mixed system is 0.01% to 0.5%; And / or, the temperature of the esterification reaction or the transesterification reaction is 150° C. to 170° C., the time is 4 h to 20 h, and the esterification reaction or the transesterification reaction is carried out in a protective atmosphere.

7. The preparation method according to claim 5, characterized in that: include: Adding a polymerization inhibitor and a polycondensation aid to the product obtained in step (1), reducing the pressure of the reaction system to 5Pa to 200Pa, and conducting a polycondensation reaction at 170°C to 175°C, wherein the stable vacuum degree of the polycondensation reaction is less than or equal to 7Pa, and the polycondensation reaction time is 5 to 10 hours, to obtain a preliminary product of a degradable copolyester containing double bonds; Preferably, the number average molecular weight of the preliminary product of the double bond-containing degradable copolyester is 20 to 60 KDa, preferably 20 to 50 KDa; And / or, the polymerization inhibitor comprises at least two of p-hydroxyanisole, hydroquinone, p-benzoquinone, and oxidized diphosphoric acid, preferably a mixture of p-hydroxyanisole and p-benzoquinone; and / or, the mass fraction of the polymerization inhibitor in the mixture of the product obtained in step (1) and the polycondensation aid is 0.5% to 3%; Preferably, the mass fraction of the p-hydroxyanisole in the mixture of the product obtained in step (1) and the polycondensation aid is 0.2% to 2%; Preferably, the mass fraction of the benzodiquinone in the mixture of the product obtained in step (1) and the polycondensation aid is 0.2% to 2%; And / or, the polycondensation aid includes at least one of a polycondensation catalyst and a stabilizer; Preferably, the mass fraction of the polycondensation catalyst in the mixture of the product obtained in step (1) and the polycondensation aid is 0.01% to 0.5%; Preferably, the mass fraction of the stabilizer in the mixture of the product obtained in step (1) and the polycondensation aid is 0.01% to 0.5%; Preferably, the polycondensation catalyst includes at least one of a titanium-based catalyst and a germanium-based catalyst; Preferably, the stabilizer includes at least one of phosphorous acid, hypophosphorous acid, pyrophosphoric acid, ammonium phosphate, trimethyl phosphate, dimethyl phosphate, and triphenyl phosphate.

8. The preparation method according to claim 5, characterized in that: include: The reaction system of step (2) is heated to 180-185° C., and the post-condensation reaction is continued. The stable vacuum degree of the post-condensation reaction is less than or equal to 7 Pa, and the time of the post-condensation reaction is 0.5-3 hours, so as to obtain the main chain double bond-containing degradable copolyester with adjustable shelf life and degradation rate.

9. A main chain double-bond degradable copolyester with adjustable shelf life and degradation rate, obtained by the preparation method according to any one of claims 5 to 8.

10. Use of the main chain double-bond degradable copolyester with adjustable shelf life and degradation rate according to any one of claims 1-4 and 9 in plastic products; preferably, the plastic products include mulch films, fishing nets, plastic containers, packaging materials, drug sustained-release carriers or human implant components.

Citation Information

Patent Citations

  • Polyester containing unsaturated double bond and preparation method thereof

    CN105482084A

  • Modified polybutylene terephthalate PBT patch and preparation and application thereof

    CN109731146A

  • Preparation method of high-cis polybutylene maleate with high molecular weight

    CN110563867A

  • Degradable polyester as well as preparation method, degradation method and application thereof

    CN115572380A

  • Thermosetting resin composition

    JP1999080286A

Cited By

  • Anti-aging biodegradable material as well as preparation method and application thereof