Polyaromatic ether type aromatic amide polymer as well as preparation method and coating thereof
By using step-by-step polymerization of terephthalide and terephthalide chloride in the lithium battery separator coating, a stable polyaromatic ether type aramid polymer is formed, and the lithium battery separator coating and base are solved. The problem of poor membrane bonding performance achieves high-performance coating preparation and low defect rate.
Patent Information
- Application Number
- CN202310606310.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-26
AI Technical Summary
The poor bonding performance of the existing lithium battery separator coating polymer solution and the base film leads to a high coating defect rate and is difficult to meet the requirements of industrial production.
The polyaromatic ether acoramide polymer is prepared by polymerizing the para-phenylenediamine and aromatic ether phenylenediamine in the tertiary amide composite solvent in two steps to form a stable three-dimensional porous structure and improve the polymer solution. The uniformity and adhesive properties of the coating film are reduced.
The high tensile strength, puncture strength and low defect rate of polyaramid ether aramid nanofiber coating are achieved, and the temperature resistance and industrial production applicability of lithium battery separators are improved.
Smart Images

Figure CN119019678A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a polyaromatic ether type aromatic amide polymer and a preparation method and a coating thereof, and specifically relates to a high-performance aromatic amide lithium battery diaphragm coating based on polyaromatic ether, a polymerization solution for preparing the coating and a preparation method of the polymerization solution, and belongs to the technical field of lithium battery diaphragm coating materials. Technical Background
[0002] Lithium battery is a kind of battery that uses lithium metal or lithium alloy as positive / negative electrode material and non-aqueous electrolyte solution. It is widely used in electronic products such as mobile phones, laptops, and new energy vehicles due to its excellent performance. In the structure of lithium battery, the diaphragm is one of the key inner components. The performance of the diaphragm determines the interface structure and internal resistance of the battery, which directly affects the battery's capacity, cycle and safety performance. Therefore, a diaphragm with excellent performance plays an important role in improving the comprehensive performance of the battery. At present, with the continuous development of new diaphragm material products, coated polyester film (PET), cellulose film, polyimide film (PI), polyamide film (PA), spandex or aramid film, etc. have appeared. These diaphragms have the characteristics of low temperature output, long charging cycle life, high temperature resistance and moderate mechanical strength, and are used to manufacture power lithium batteries.
[0003] In the prior art, an invention patent with publication number CN107452921A discloses a method for preparing a para-aramid nanofiber composite lithium-ion battery separator. The method uses N-methyl-2-pyrrolidone and para-phenylenediamine as raw materials, calcium chloride / aluminum chloride as co-solvents, and after completely dissolving them in an ice water bath, terephthaloyl chloride is added for polymerization to obtain a para-aramid polymer slurry, and then the slurry is coated on the surface of a base film to obtain the para-aramid nanofiber composite ion battery separator. This patent uses the prepared aramid polymer slurry to form a film and form a loose and porous nanofiber network structure. By comparing the number of charging cycles of the prepared para-aramid fiber nanofiber composite lithium-ion battery membrane with the lithium battery without a coated membrane, when the number of charge and discharge cycles increases to more than 30 times, the discharge specific capacity of the lithium battery with the patented membrane increases, proving that the use of the membrane lithium battery is more stable. However, there is no verifiable data to support the temperature resistance and mechanical properties of the patented membrane based on lithium batteries.
[0004] The invention patent with the publication number of JP2013032491A discloses a porous membrane with high porosity, dense pore structure and uniform pore structure in the thickness direction, a battery separator using the porous membrane and a manufacturing method thereof, which is composed of aromatic polyamide as a component. Among them, as a method for preparing polymerized aromatic polyamide, acyl chloride and diamine can be synthesized by solution polymerization in a non-protonic organic polar solvent medium such as N-methyl-2-pyrrolidone, N,N-dimethylacetamide, dimethylformamide, dimethyl sulfoxide, etc., and the molecular weight of the polymer can be easily controlled. By controlling the porosity, the mechanical strength and conductivity of the membrane can be improved, but it requires the use of aqueous polymers to be mixed and then coated and precipitated to obtain a porous structure.
[0005] The invention patent with the publication number CN112201903A discloses a high-performance polyaromatic amide lithium battery separator coating polymerization solution and its preparation method and application. The method is to dissolve aromatic diamine in N-methylpyrrolidone, then add diacyl halide or dicarboxylic acid monomer and aromatic diamine to polymerize to obtain a low molecular weight polyaromatic amide polymer solution. After the polymerization solution is applied to the surface of the base film, a polyaromatic amide nanofiber coating can be obtained, and a porous structure is naturally formed. The patent records the tensile strength, puncture strength and air permeability of the separator, among which the tensile strength and puncture strength are used to prove its mechanical properties, and the air permeability is used to characterize the pore density and size of the membrane.
[0006] In summary, although the above-mentioned existing patents provide a variety of polymer solutions for coating and preparing battery separator coatings, and these polymer solutions improve the pore structure, mechanical properties, temperature resistance and number of lithium battery charge and discharge cycles of the coated separators, there is no patent or literature reporting the yield rate of such polymer solutions after coating to prepare separators. Due to the difference in the bonding performance between the polymer solution and the base film, the coating defect rate may increase. Therefore, the premise for applying such polymer solutions to industrial production is to solve the bonding performance between the polymer solution and the base film, while satisfying the advantages of the polymer solution in the preparation of lithium battery separator coatings. Summary of the invention
[0007] In view of the above-mentioned defects, the present invention provides a method for preparing a polyaromatic ether type aromatic amide polymer. In the presence of a tertiary amide type composite solvent, p-phenylenediamine, aromatic ether phenylenediamine and terephthaloyl chloride are polymerized to form a low molecular weight polyaromatic ether type aromatic amide polymer system having specific physical and chemical properties, so that the polymer has better uniformity, deeper penetration into the base membrane and stronger adhesion, no need for pore-forming agents or other auxiliary materials, good solution fluidity, and is suitable for industrial mass production. For this purpose, the present invention also provides a polyaromatic ether type aromatic amide polymer prepared by the method, and a polyaromatic ether type aromatic amide nanofiber coating obtained by coating the same, which has excellent tensile strength, puncture strength, and air permeability, and a low defect rate of the diaphragm coating.
[0008] To solve the above problems, the present invention is implemented by the following technical scheme: a method for preparing a polyaromatic ether type aromatic amide polymer, wherein p-phenylenediamine and aromatic ether phenylenediamine are added to a tertiary amide type composite solvent for dissolution, and the molar concentration of the aromatic ether in the tertiary amide type composite solvent is controlled to be 20-90% of the total phenylenediamine to obtain a dissolving solution; Terephthaloyl chloride is added to the dissolving solution twice, the molar ratio of the first added terephthaloyl chloride to the total amount of p-phenylenediamine and aromatic ether in the dissolving solution is 20-35:100, and the reaction is carried out for 5-20 minutes after the addition, and the molar ratio of the second added terephthaloyl chloride to the total amount of p-phenylenediamine and aromatic ether in the dissolving solution is 65-75:100, and the reaction is carried out for 10-30 minutes after the addition to obtain a polymerization solution, and after degassing the polymerization solution, a polyaromatic ether type aromatic amide polymer is obtained, The polyaromatic ether type aromatic amide polymer meets the following requirements: solid content ≤3%, dynamic viscosity at 30°C of 100-5000 cPs, characteristic viscosity η<3 dl / g, and thermal decomposition temperature>450°C.
[0009] The aromatic ether phenylenediamine is 4,4'-diaminodiphenyl ether or 3,4'-diaminodiphenyl ether.
[0010] The tertiary amide type composite solvent is a composite solution formed by a tertiary amide solvent and a halide alkaline earth metal or alkali metal salt. In terms of mass percentage, the tertiary amide solvent accounts for 90-98% and the halide alkaline earth metal or alkali metal salt accounts for 2-10% in the tertiary amide type composite solvent.
[0011] The tertiary amide solvent includes N-methylpyrrolidone, N,N-dimethylacetamide, and N,N-dimethylformamide.
[0012] The alkaline earth metal halide is CaCl 2, : The alkali metal halide is LiCl.
[0013] The halogenated alkaline earth metal or alkali metal is added into the tertiary amide solvent, and the mixture is heated to 30-50° C. and dissolved under nitrogen protection to obtain a tertiary amide type composite solvent.
[0014] After the solution is cooled to 0-5°C, terephthaloyl chloride is added.
[0015] The reaction temperature after the first addition of terephthaloyl chloride is controlled to be 0-5°C, and the reaction temperature after the second addition of terephthaloyl chloride is controlled to be 15-20°C.
[0016] A polyaromatic ether type aromatic amide polymer prepared by any of the preparation methods described above.
[0017] A lithium battery separator coating, wherein the prepared polymer solution is applied to the surface of a base film, and then solidified, cleaned and dried to obtain a polyaromatic ether type aramid nanofiber coating. The polyaromatic ether aramid nanofiber coating satisfies the following requirements: the coating thickness is 1 to 4 μm, and the coating defect rate is ≤1 / 10 m.
[0018] The present invention has the following beneficial effects: (1) The present invention introduces aromatic ether phenylenediamine into the polyaromatic ether type aromatic amide polymer system for the first time. Specifically, in a tertiary amide type composite solvent, p-phenylenediamine and aromatic ether phenylenediamine are used to react with terephthaloyl chloride in two steps. This can not only further improve the pore-forming performance of the polymer solution and obtain a more stable three-dimensional porous structure, but also make the polymer solution more uniform, so that it can penetrate deeper into the base film and adhere more firmly. At the same time, it can reduce coating defects and achieve the standard of coating defect rate of ≤1 / 10m.
[0019] (2) The present invention can obtain a polymer solution with specific physical and chemical properties by reasonably controlling the content of aromatic ether phenylenediamine in the polyaromatic ether type aromatic amide polymer system, and meet the specific index system of the polymer solution, namely: solid content ≤3%, dynamic viscosity at 30°C is 100-5000cPs, characteristic viscosity η<3dl / g, thermal decomposition temperature>450°C, which can improve the pore formation and air permeability of the coating film, as well as the wettability of the membrane liquid, and ensure the temperature resistance of the coating.
[0020] In summary, the present invention provides a polyaromatic ether amide polymer suitable for lithium battery separator coating. During the polymerization process, a specific proportion of aromatic ether is introduced to prepare a polymer solution with a specific index system. Not only a three-dimensional porous structure can be obtained, but also its bonding performance with the base membrane can be improved. In the field of lithium battery separators, the defect rate of the separator coating can be reduced to avoid the risk of spontaneous combustion and explosion of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The structure of the polyaromatic ether type aramid nanofiber coating obtained after the polymer solution of the present invention is coated on the surface of the base film, solidified, cleaned and dried is magnified 5000 times under a microscope; DETAILED DESCRIPTION
[0022] The invention objectives, technical solutions and beneficial effects of the present invention are further described in detail below.
[0023] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the claimed invention, and unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the invention belongs.
[0024] The present invention aims to solve the problem that the existing battery separator has poor bonding performance between the polymer solution coating and the base film, and the coating defect rate is high. For example, the existing patents CN107452921A, JP2013032491A and CN112201903A have improved the pore structure, mechanical properties, temperature resistance and number of lithium battery charge and discharge cycles of the separator coating to a certain extent, but still lack the defects caused by the difference in the bonding performance between the polymer solution and the base film during its industrial production process. Therefore, the present invention needs to provide a polyaromatic ether type aromatic amide polymer suitable for industrial separator production and a preparation method thereof, as well as a coating obtained by coating the polymer.
[0025] The technical solution of the present invention can be further summarized as follows: According to the mass percentage, 2-10% of alkaline earth metal halide or alkali metal is added to 90-98% of tertiary amide solvent, and heated to 30-50° C. and dissolved under nitrogen protection to obtain a tertiary amide type composite solvent, and p-phenylenediamine and aromatic ether phenylenediamine are added, and the molar concentration of aromatic ether in the tertiary amide type composite solvent is controlled to be 20-90% of the total phenylenediamine to obtain a dissolving solution; after cooling the dissolving solution to 0-5° C., terephthaloyl chloride is added twice, and when terephthaloyl chloride is added for the first time, The molar ratio of terephthaloyl chloride to the total amount of p-phenylenediamine and aromatic ether in the dissolving solution is controlled to be 20-35:100, and then the reaction is carried out at 0-5°C for 5-20 minutes. The terephthaloyl chloride is added for the second time, and the molar ratio of the terephthaloyl chloride added for the second time to the total amount of p-phenylenediamine and aromatic ether in the dissolving solution is 65-75:100. Then the reaction is carried out at 15-20°C for 10-30 minutes to obtain a polymerization solution. After degassing the polymerization solution, a polyaromatic ether type aromatic amide polymer is obtained.
[0026] In the above preparation process, it can be listed that the alkaline earth metal halide can be selected from CaCl2; the alkali metal halide can be selected from LiCl; the tertiary amide solvent can be selected from any one of N-methylpyrrolidone (NMP), N,N-dimethylacetamide (DMAc), N,N-dimethylformamide (DMF); the aromatic ether phenylenediamine can be selected from 4,4'-diaminodiphenyl ether or 3,4'-diaminodiphenyl ether.
[0027] Due to the introduction of aromatic ether phenylenediamine and its specific proportion in the polyaromatic ether type aromatic amide polymer system, the polyaromatic ether type aromatic amide polymer can meet the following index system: solid content ≤3%, dynamic viscosity at 30°C is 100-5000cPs, characteristic viscosity η<3dl / g, and thermal decomposition temperature>450°C.
[0028] Among them, the control of solid content can achieve the control of coating and the optimization of air permeability, and at the same time, it is also beneficial to the wettability of the polymer solution to the base film; the dynamic viscosity is the apparent characteristic of the polymer solution, which can achieve the adjustment and optimization of the membrane liquid wettability; the characteristic viscosity is the characteristic of the polymer, which is positively correlated with the dynamic viscosity, and can also achieve the adjustment and optimization of the membrane liquid wettability; the thermal decomposition temperature is used to characterize the temperature resistance of the polymer solution coating of the present invention.
[0029] The polyaromatic ether aramid polymer solution based on the above index system can be coated on the surface of the base film, and then solidified, cleaned and dried to obtain a polyaromatic ether aramid nanofiber coating, so that the coating has a more stable three-dimensional porous structure and better bonding performance to the base film. Therefore, the polyaromatic ether aramid nanofiber coating meets the following requirements: the coating thickness is 1 to 4 μm, and the coating defect rate is ≤1 / 10m.
[0030] Several typical embodiments are listed below to illustrate the specific implementation of the present invention. Of course, the protection scope of the present invention is not limited to the following embodiments.
[0031] Embodiment 1: 3.6 g of anhydrous LiCl was added to 100 g of DMAc, and the mixture was heated to 50°C under N2 protection to dissolve. Then, 0.4259 g of p-phenylenediamine and 0.786 g of 4,4'-diaminodiphenyl ether were added to dissolve. The mixture was then cooled to 5°C, 0.5597 g of terephthaloyl chloride was added for the first time, and the mixture was reacted at 0°C for 10 min. Then, 1.0021 g of terephthaloyl chloride was added for the second time, and the mixture was reacted at 20°C for 25 min. The polymer solution after the reaction was then degassed to obtain a polyaromatic ether type aromatic amide polymer. The polymer solution had a solid content of 2.18%, a dynamic viscosity of 2369 cPs at 30°C, a characteristic viscosity η of 1.34 dl / g, and a thermal decomposition temperature of 455°C.
[0032] Embodiment 2: 4.3 g of anhydrous CaCl2 was added to 100 g of NMP, and the mixture was heated to 50°C under N2 protection to dissolve. Then, 0.4619 g of p-phenylenediamine and 0.8552 g of 3,4'-diaminodiphenyl ether were added to dissolve, and then the temperature was lowered to 5°C. 0.6070 g of terephthaloyl chloride was added for the first time, and the mixture was reacted at 5°C for 10 min. Then, 1.112 g of terephthaloyl chloride was added for the second time, and the mixture was reacted at 18°C for 25 min. The polymer solution after the reaction was then degassed to obtain a polyaromatic ether type aromatic amide polymer. The solid content of the polymer solution was 2.36%, the dynamic viscosity at 30°C was 4322 cPs, the characteristic viscosity η was 1.40 dl / g, and the thermal decomposition temperature was 453°C.
[0033] Embodiment 3: 7.6 g of anhydrous CaCl2 was added to 100 g of NMP, and the mixture was heated to 50°C under N2 protection to dissolve. Then, 0.5340 g of p-phenylenediamine and 0.9888 g of 3,4'-diaminodiphenyl ether were added to dissolve, and then the temperature was lowered to 10°C. 0.7017 g of terephthaloyl chloride was added for the first time, and the mixture was reacted at 5°C for 20 min. Then, 1.2231 g of terephthaloyl chloride was added for the second time, and the mixture was reacted at 20°C for 30 min. The polymer solution after the reaction was then degassed to obtain a polyaromatic ether type aromatic amide polymer. The solid content of the polymer solution was 2.71%, the dynamic viscosity at 30°C was 4311 cPs, the characteristic viscosity η was 1.35 dl / g, and the thermal decomposition temperature was 451°C.
[0034] Embodiment 4: 5.6 g of anhydrous CaCl2 was added to 100 g of NMP, and the mixture was heated to 50°C under N2 protection to dissolve. Then, 0.3677 g of p-phenylenediamine and 1.3617 g of 4,4'-diaminodiphenyl ether were added to dissolve, and then the temperature was lowered to 10°C. 0.7248 g of terephthaloyl chloride was added for the first time, and the mixture was reacted at 2°C for 20 min. Then, 1.2567 g of terephthaloyl chloride was added for the second time, and the mixture was reacted at 20°C for 30 min. The polymer solution after the reaction was then degassed to obtain a polyaromatic ether type aromatic amide polymer. The polymer solution had a solid content of 2.94%, a dynamic viscosity of 3241 cPs at 30°C, a characteristic viscosity η of 1.47 dl / g, and a thermal decomposition temperature of 455°C.
[0035] Embodiment 5: 3.1 g of anhydrous LiCl was added to 100 g of DMAC, and heated to 50° C. under N2 protection to dissolve, and then 0.5630 g of p-phenylenediamine and 1.0424 g of 3,4'-diaminodiphenyl ether were added to dissolve, and then the temperature was lowered to 5° C., 0.7398 g of terephthaloyl chloride was added for the first time, and the mixture was reacted at 0° C. for 15 min, and 1.3037 g of terephthaloyl chloride was added for the second time, and the mixture was reacted at 15° C. for 30 min. The polymer solution after the reaction was then degassed to obtain a polyaromatic ether type aromatic amide polymer, the solid content of the polymer solution was 2.85%, the dynamic viscosity at 30° C. was 4175 cPs, the characteristic viscosity η was 1.45 dl / g, and the thermal decomposition temperature was 456° C.
[0036] Embodiment 6: 3.1 g of anhydrous LiCl was added to 100 g of DMAC, and heated to 50° C. under N2 protection to dissolve, and then 0.2445 g of phenylenediamine and 1.3605 g of 3,4'-diaminodiphenyl ether were added to dissolve, and then the temperature was lowered to 5° C., 0.6437 g of terephthaloyl chloride was added for the first time, and the mixture was reacted at 5° C. for 15 min, and 1.1834 g of terephthaloyl chloride was added for the second time, and the mixture was reacted at 15° C. for 30 min. The polymer solution after the reaction was then degassed to obtain a polyaromatic ether type aromatic amide polymer, the solid content of the polymer solution was 2.69%, the dynamic viscosity at 30° C. was 4572 cPs, the characteristic viscosity η was 1.29 dl / g, and the thermal decomposition temperature was 453° C.
[0037] Comparative Example 1: The difference between this comparative example 1 and example 6 is that the amounts of p-phenylenediamine, 3,4'-diaminodiphenyl ether and terephthaloyl chloride in the polymer system are different, and the temperature and time of the polymerization reaction are slightly adjusted.
[0038] 3.1 g of anhydrous LiCl was added to 100 g of DMAC, and heated to 50°C under N2 protection to dissolve, then 0.6427 g of p-phenylenediamine and 1.1902 g of 3,4'-diaminodiphenyl ether were added to dissolve, and then the temperature was lowered to 5°C, 0.8447 g of terephthaloyl chloride was added for the first time, and the mixture was reacted at 5°C for 10 min, and 1.5400 g of terephthaloyl chloride was added for the second time, and the mixture was reacted at 20°C for 25 min. The polymer solution after the reaction was then degassed, and the obtained polymer solution had a solid content of 3.24%, a dynamic viscosity of 5122 cPs at 30°C, a characteristic viscosity η of 1.86 dl / g, and a thermal decomposition temperature of 455°C.
[0039] Comparative Example 2: The difference between this comparative example and Example 2 is that p-phenylenediamine and terephthaloyl chloride are used in the polymer system, and the amounts of p-phenylenediamine and terephthaloyl chloride, as well as the polymerization reaction time and temperature are slightly adjusted.
[0040] 7.2 g of anhydrous CaCl2 was added to 100 g of NMP, and the mixture was heated to 50°C under N2 protection to dissolve. Then, 1.1122 g of p-phenylenediamine was added to dissolve, and the mixture was then cooled to 5°C. 0.7308 g of terephthaloyl chloride was added for the first time, and the mixture was reacted at 5°C for 20 min. Then, 1.3272 g of terephthaloyl chloride was added for the second time, and the mixture was reacted at 18°C for 25 min. The polymer solution after the reaction was then degassed, and the obtained polymer solution had a solid content of 2.36%, a dynamic viscosity of 4278 cPs at 30°C, a characteristic viscosity η of 1.78 dl / g, and a thermal decomposition temperature of 452°C.
[0041] Comparative Example 3: The difference between this comparative example and Example 4 is that p-phenylenediamine, o-p-phenylenediamine and terephthaloyl chloride are used in the polymer system, and the amounts of p-phenylenediamine and terephthaloyl chloride, as well as the polymerization reaction time and temperature are slightly adjusted.
[0042] 7.6 g of anhydrous CaCl2 was added to 100 g of NMP, and heated to 50°C under N2 protection to dissolve, then 0.079 g of p-phenylenediamine and 1.7540 g of o-p-phenylenediamine were added to dissolve, and then the temperature was lowered to 0°C, 0.6743 g of terephthaloyl chloride was added for the first time, and the reaction was carried out at 5°C for 20 min, and 1.2523 g of terephthaloyl chloride was added for the second time, and the reaction was carried out at 20°C for 25 min. The polymer solution after the reaction was then degassed, and the obtained polymer solution had a solid content of 2.96%, a dynamic viscosity of 2435 cPs at 30°C, a characteristic viscosity η of 1.56 dl / g, and a thermal decomposition temperature of 452°C.
[0043] Comparative Example 4: The difference between this comparative example and Example 1 is that an excessive amount of aromatic ether diamine is used in the polymer system (i.e., the molar concentration of the aromatic ether diamine after dissolution exceeds 90%), and the amounts of the remaining p-phenylenediamine and terephthaloyl chloride, as well as the polymerization reaction time and temperature are slightly adjusted.
[0044] 3.6 g of anhydrous LiCl was added to 100 g of DMAc, and the mixture was heated to 50°C under N2 protection to dissolve. Then, 0.036 g of p-phenylenediamine and 1.254 g of 4,4'-diaminodiphenyl ether were added to dissolve. The mixture was then cooled to 5°C, 0.4686 g of terephthaloyl chloride was added for the first time, and the mixture was reacted at 5°C for 10 min. Then, 0.8032 g of terephthaloyl chloride was added for the second time, and the mixture was reacted at 25°C for 25 min. The polymer solution after the reaction was then degassed to obtain a polyaromatic ether type aromatic amide polymer. The polymer solution had a solid content of 2.0%, a dynamic viscosity of 6894 cPs at 30°C, a characteristic viscosity η of 1.74 dl / g, and a thermal decomposition temperature of 453°C.
[0045] Comparative Example 5: The difference between this comparative example and Example 1 is that a small amount of aromatic ether diamine is used in the polymer system (i.e., the molar concentration of the aromatic ether diamine after dissolution is less than 20%), and the amounts of the remaining p-phenylenediamine and terephthaloyl chloride, as well as the polymerization reaction time and temperature are slightly adjusted.
[0046] 3.6 g of anhydrous LiCl was added to 100 g of DMAc, and the mixture was heated to 50°C under N2 protection to dissolve. Then, 1.0700 g of p-phenylenediamine and 0.2201 g of 4,4'-diaminodiphenyl ether were added to dissolve, and then the temperature was lowered to 5°C. 0.7812 g of terephthaloyl chloride was added for the first time, and the mixture was reacted at 5°C for 10 min. Then, 14124 g of terephthaloyl chloride was added for the second time, and the mixture was reacted at 30°C for 25 min. The polymer solution after the reaction was then degassed to obtain a polyaromatic ether type aromatic amide polymer. The solid content of the polymer solution was 2.53%, the dynamic viscosity at 30°C was 6462 cPs, the characteristic viscosity η was 1.43 dl / g, and the thermal decomposition temperature was 452°C.
[0047] It can be seen from the above-mentioned Examples 1 to 6 and Comparative Examples 1 to 5 that after changing the coordination relationship between p-phenylenediamine and aromatic ether phenylenediamine in the polymer system and the amount of aromatic ether phenylenediamine therein, the specific index system of the polymer solution obtained by the polymerization will be further changed.
[0048] Furthermore, the scraping method can be used to apply the polymer solutions of Examples 1 to 6 and Comparative Examples 1 to 5 to the surface of the PE diaphragm, respectively, with a coating thickness of 3 μm, and then obtain the corresponding coating after coagulation, cleaning and drying.
[0049] The coating prepared in Example 1 of the above Examples 1 to 6 was randomly selected for electron microscope scanning (×5000 times). Figure 1 It can be seen that the coating prepared by the present invention has a three-dimensional porous structure.
[0050] In order to better illustrate the present invention, the following experiments were performed: The uncoated blank PE diaphragm was used as the blank group, the coated diaphragms of Examples 1 to 6 of the present invention were used as experimental groups 1 to 6, respectively, and the coated diaphragms of Comparative Examples 1 to 5 were used as comparative groups 1 to 5, respectively. The relevant indicators were tested and the data were statistically summarized in Table 1 below.
[0051] Table 1 Based on the above content, it can be known that the polyaromatic ether type aromatic amide polymer of the present invention has a specific molar amount of aromatic ether added thereto and has a specific index system. Therefore, when used as a coating, it can give a base film (such as a PE diaphragm) a specific effect, which is as follows: (1) As shown in Table 1, by comparing the coated membranes of experimental groups 1 to 6 with the blank PE membrane, it can be seen that the tensile strength, puncture strength and air permeability of the coated membranes prepared by the method of the present invention are improved.
[0052] (2) Although the solid content of the polymer solution in Comparative Example 1 can be adjusted to 3.24% by controlling the amount of monomer added, the dynamic viscosity of the polymer solution at 30°C reaches 5122 cPs, which is not within the index system range of the present invention. As shown in Table 1, from the performance of the coated diaphragm in Comparative Group 1, its tensile strength is not improved compared with the blank PC diaphragm, and the defect rate of the diaphragm coating is 2 / 10m.
[0053] (3) In Comparative Example 2, only p-phenylenediamine monomer was used for the reaction. Although the index system of its polymer solution was within the index system range of the present invention, the performance of its coating changed. As shown in Table 1 above, from the performance of the coated diaphragm of Comparative Group 2, its tensile strength was equivalent to that of the blank PC diaphragm, which was much lower than that of Experimental Groups 1 to 6 of the present invention, and the defect rate of the diaphragm coating was 4 / 10m.
[0054] (4) In Comparative Example 3, p-phenylenediamine and o-phenylenediamine monomers were reacted. Although the index system of the polymer solution was within the index system of the present invention, the performance of the coating changed. As shown in Table 1 above, from the performance of the coated diaphragm in Comparative Group 3, its tensile strength was lower than that of the blank PC diaphragm, and the defect rate of the diaphragm coating was 2 / 10m.
[0055] (5) In comparative example 4, an excessive amount of aromatic ether groups was introduced into the polymer solution, and the dynamic viscosity of the polymer solution at 30°C reached 6894 cPs, which is far beyond the index system range of the present invention. As shown in Table 1, from the performance of the coated diaphragm of comparative group 4, its tensile strength was not improved compared with the blank PC diaphragm, and the puncture strength was also much lower than that of experimental groups 1 to 6 of the present invention, and the defect rate of the diaphragm coating was 2 / 10m.
[0056] (6) In comparative example 5, a small amount of aromatic ether groups were introduced into the polymer solution, and the dynamic viscosity of the polymer solution at 30°C reached 6462 cPs, which is far beyond the index system range of the present invention. As shown in Table 1, from the performance of the coated diaphragm of comparative group 5, its tensile strength is improved compared with the blank PC diaphragm, but it is still lower than that of experimental groups 1 to 6 of the present invention, and the defect rate of the diaphragm coating is 2 / 10m.
[0057] In summary, the coated diaphragm prepared from the polyaromatic ether type aromatic amide polymer of the present invention can significantly improve the tensile strength of the base film and effectively reduce the defect rate of the diaphragm coating, which can prove that the polyaromatic ether type aromatic amide polymer has better bonding performance with the base film and good coating performance.
[0058] It should be noted that, in the present invention, the solid content of the polymer solution can be calculated by the addition amount; the dynamic viscosity at 30°C is detected by using a Brookfield DV1 digital viscometer; the characteristic viscosity η is obtained by dissolving the polymer solution in concentrated sulfuric acid at 0.5 g / 100 ml and measuring it using an Ubbelohde viscometer at 30°C; the thermal decomposition temperature is detected according to GB / T33047.3-2021; the tensile strength of the film is detected by GB / T 1040.1-2018 instron 3400; the puncture strength is detected by GB / T37841-2019; the defect rate of the diaphragm coating is detected by the Thermo Fisher Online Thin Film Defect Detection System.
[0059] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification or equivalent change made to the above embodiment based on the technical essence of the present invention shall fall within the protection scope of the present invention.
Claims
1. A method for preparing a polyaromatic ether type aromatic amide polymer, characterized in that: Adding p-phenylenediamine and aromatic ether phenylenediamine into a tertiary amide type composite solvent to dissolve, controlling the molar concentration of the aromatic ether in the tertiary amide type composite solvent to be 20-90% of the total phenylenediamine to obtain a solution; Terephthaloyl chloride is added to the dissolving solution twice, the molar ratio of the first added terephthaloyl chloride to the total amount of p-phenylenediamine and aromatic ether in the dissolving solution is 20-35:100, and the reaction is carried out for 5-20 minutes after the addition, and the molar ratio of the second added terephthaloyl chloride to the total amount of p-phenylenediamine and aromatic ether in the dissolving solution is 65-75:100, and the reaction is carried out for 10-30 minutes after the addition to obtain a polymerization solution, and after degassing the polymerization solution, a polyaromatic ether type aromatic amide polymer is obtained, The polyaromatic ether type aromatic amide polymer meets the following requirements: solid content ≤3%, dynamic viscosity at 30°C of 100-5000 cPs, characteristic viscosity η<3 dl / g, and thermal decomposition temperature>450°C.
2. The preparation method according to claim 1, characterized in that: The aromatic ether phenylenediamine is 4,4'-diaminodiphenyl ether or 3,4'-diaminodiphenyl ether.
3. The preparation method according to claim 1, characterized in that: The tertiary amide type composite solvent is a composite solution formed by a tertiary amide solvent and a halide alkaline earth metal or alkali metal salt. In terms of mass percentage, the tertiary amide solvent accounts for 90-98% and the halide alkaline earth metal or alkali metal salt accounts for 2-10% in the tertiary amide type composite solvent.
4. The preparation method according to claim 3, characterized in that: The tertiary amide solvent includes N-methylpyrrolidone, N,N-dimethylacetamide, and N,N-dimethylformamide.
5. The preparation method according to claim 3, characterized in that: The alkaline earth metal halide is CaCl 2, : The alkali metal halide is LiCl.
6. The preparation method according to claim 3, characterized in that: The halogenated alkaline earth metal or alkali metal is added into the tertiary amide solvent, and the mixture is heated to 30-50° C. and dissolved under nitrogen protection to obtain a tertiary amide type composite solvent.
7. The preparation method according to claim 1, characterized in that: After the solution is cooled to 0-5°C, terephthaloyl chloride is added.
8. The preparation method according to claim 1, characterized in that: The reaction temperature after the first addition of terephthaloyl chloride is controlled to be 0-5°C, and the reaction temperature after the second addition of terephthaloyl chloride is controlled to be 15-20°C.
9. A polyaromatic ether type aromatic amide polymer prepared by the preparation method according to any one of claims 1 to 8.
10. A lithium battery separator coating, characterized in that: The polymer solution prepared in claim 9 is applied to the surface of the base film, and then solidified, cleaned and dried to obtain a polyaromatic ether type aramid nanofiber coating. The polyaromatic ether aramid nanofiber coating satisfies the following requirements: the coating thickness is 1 to 4 μm, and the coating defect rate is ≤1 / 10 m.