Piperazine phosphate-ammonium phosphate copolymerized flame retardant as well as preparation method and application thereof
The polymerization reaction of piperazine diphosphate, ammonium dihydrogen phosphate and urea is formed to form piperazine phosphate-ammonium phosphate copolymer flame retardant, solving the problem of easy hydrolysis of ammonium polyphosphate and realizing a low-cost, hydrolysis-resistant expansion flame retardant , used to maintain V-0 flame retardant properties in polyolefin materials and avoid the generation of precipitates.
Patent Information
- Application Number
- CN202411113286.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
AI Technical Summary
Traditional ammonium polyphosphate is easy to hydrolyze and precipitate, affecting its flame retardant performance in plastics and other materials. The existing modification methods increase the process flow and cost, and lack low-cost, hydrolysis-resistant expansion flame retardant solutions.
By polymerizing piperazine diphosphate, ammonium dihydrogen phosphate and urea, piperazine phosphate-ammonium phosphate copolymer flame retardant is formed, and an expanded flame retardant with a carbon source and an acid source is formed, which solves the ease of ammonium polyphosphate Hydrolysis problems and reduce costs.
The prepared piperazine phosphate-ammonium phosphate copolymer flame retardant maintained V-0 flame retardant in the polyolefin material, and boiled in water for 168 hours without precipitates, which was lower than the traditional method.
Smart Images

Figure CN119019693A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of flame retardant preparation, and relates to a piperazine phosphate-ammonium phosphate copolymer flame retardant and a preparation method and application thereof. Background Art
[0002] Intumescent flame retardant (IFR) is an environmentally friendly green flame retardant that does not contain halogens and does not use antimony oxide as a synergist. The system itself has a synergistic effect. When plastics containing intumescent flame retardants are burned, a carbon foam layer will be generated on the surface, which has the functions of heat insulation, oxygen isolation, smoke suppression, and drip prevention. It has excellent flame retardant properties, and produces low smoke, low toxicity, and no corrosive gas. It is in line with the future research and development direction of flame retardants and has become one of the most active flame retardant research fields at home and abroad.
[0003] As an important component of intumescent flame retardants, ammonium polyphosphate (APP) is an important inorganic flame retardant developed in the past decade and is widely used in the fields of plastics, fibers, paper, rubber, wood, etc. APP has the advantages of large phosphorus and nitrogen content, low specific gravity, low toxicity and low price. However, the molecular structure of APP is unstable. In a humid and water environment, APP is easy to precipitate and decompose from the material, resulting in frost on the surface of the product and flame retardant failure, which seriously affects the application of APP in special fields. At present, surface modification, surface treatment, microcapsule coating and other technologies are often adopted to improve the hydrolysis resistance of ammonium polyphosphate. CN116376114A discloses a preparation method of a double-layer coated ammonium polyphosphate flame retardant. The method introduces melamine and silicon-phosphorus synergistic flame retardant DPDM into the system through double-layer coating modification of ammonium polyphosphate. DPDM and MF resin are densely coated on the surface of ammonium polyphosphate, which greatly isolates the contact between ammonium polyphosphate and water, reduces the loss of ammonium polyphosphate in the system, and improves its water resistance. However, these methods increase process flow and cost.
[0004] There are few technical solutions in the existing technology to solve the problem of APP being easy to hydrolyze and precipitate from the flame retardant synthesis stage. Therefore, it is necessary to develop a new type of intumescent flame retardant that is low in price and resistant to hydrolysis, thereby providing a new idea for the synthesis and application of APP environmentally friendly flame retardants. Summary of the invention
[0005] In view of this, one of the objects of the present invention is to provide a method for preparing a piperazine phosphate-ammonium phosphate copolymer flame retardant; a second object of the present invention is to provide a piperazine phosphate-ammonium phosphate copolymer flame retardant; a third object of the present invention is to provide an application of a piperazine phosphate-ammonium phosphate copolymer flame retardant in the preparation of flame-retardant polyolefin materials.
[0006] In order to achieve the above object, the present invention provides the following technical solutions:
[0007] 1. A method for preparing a piperazine phosphate-ammonium phosphate copolymer flame retardant, the preparation method comprising the following steps:
[0008] Piperazine diphosphate, ammonium dihydrogen phosphate and urea are ground into powder and mixed evenly, placed in an oven at 250-270°C for polymerization reaction, cooled after the reaction, and ground to obtain a copolymer flame retardant.
[0009] Preferably, the molar ratio of the piperazine diphosphate, diammonium phosphate and urea is 1:0.5 to 1:1 to 1.2.
[0010] Further preferably, the molar ratio of piperazine diphosphate, ammonium dihydrogen phosphate and urea is 1:1:1.1.
[0011] Preferably, the polymerization reaction temperature is 260°C.
[0012] Preferably, the polymerization reaction time is 1 to 3 hours.
[0013] More preferably, the polymerization reaction time is 2 hours.
[0014] 2. The piperazine phosphate-ammonium phosphate copolymer flame retardant prepared according to the above preparation method.
[0015] 3. Application of the above copolymer flame retardant in the preparation of flame retardant polyolefin materials.
[0016] 4. Flame-retardant polyolefin material, which comprises the following components by weight: 70-77 parts of polyolefin, 14-18 parts of the above-mentioned piperazine phosphate-ammonium phosphate copolymer flame retardant, 8-12 parts of melamine polyphosphate, 0.3-0.8 parts of antioxidant and 0.3-0.5 parts of processing lubricant.
[0017] Preferably, the polyolefin is any one or more of polyethylene, polypropylene, polybutylene, vinyl elastomer, propylene elastomer or EPDM rubber;
[0018] The antioxidant is any one or more of antioxidant 1010, antioxidant 168, antioxidant 1098 or antioxidant 1076;
[0019] The processing lubricant is any one or more of calcium stearate, zinc stearate, montan wax, silicone wax, polyester sodium or pentaerythritol stearate.
[0020] 5. A method for preparing the flame retardant polyolefin material, comprising the following steps:
[0021] The polyolefin, the piperazine phosphate-ammonium phosphate copolymer flame retardant, melamine polyphosphate, antioxidant and processing lubricant are uniformly mixed and placed in an extruder, and then melted, blended, extruded, stretched, pelletized and dried to obtain a flame-retardant polyolefin material.
[0022] Preferably, the temperature of each section of the extruder from the main feeding port to the die head is: 170-200°C, 180-210°C, 190-220°C, 190-220°C, 190-220°C, 190-220°C, 190-220°C, 190-220°C, 180-210°C, 220-230°C;
[0023] The rotation speed of the extruder is 300-350 rpm.
[0024] The beneficial effects of the present invention are as follows: the present invention provides a piperazine phosphate-ammonium phosphate copolymer flame retardant, the structural formula of the copolymer flame retardant contains both a piperazine phosphate structure and an ammonium phosphate structure, the piperazine phosphate-ammonium phosphate copolymer flame retardant of the present invention forms an intumescent flame retardant having both a carbon source and an acid source by copolymerizing easily soluble and easily hydrolyzed ammonium phosphate (ammonium dihydrogen phosphate) with insoluble and intractable piperazine phosphate (piperazine diphosphate), thereby solving the problem of easy precipitation and easy hydrolysis of traditional ammonium polyphosphate, and at the same time, the addition of cheap ammonium phosphate is lower in cost than that of piperazine pyrophosphate and melamine polyphosphate compound flame retardant. The piperazine phosphate-ammonium phosphate copolymer flame retardant of the present invention is used to prepare polyolefin materials, and the flame retardant performance of the prepared polyolefin materials still maintains V-0 level after 168h boiling, and there is no precipitate on the surface.
[0025] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:
[0027] Figure 1 This is the infrared spectrum analysis result of the piperazine phosphate-ammonium phosphate copolymer flame retardant prepared in Example 1;
[0028] Figure 2 This is the nuclear magnetic resonance phosphorus spectrum analysis of the piperazine phosphate-ammonium phosphate copolymer flame retardant prepared in Example 1. DETAILED DESCRIPTION
[0029] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0030] In the following embodiments, since the addition ratios of piperazine diphosphate, ammonium dihydrogen phosphate and urea, as well as the temperature and time of the copolymerization reaction are different, the connection modes between the groups during the polymerization process are different. It is possible that the piperazine phosphate structure and the ammonium phosphate structure are polymerized separately and then connected, or it is possible that the piperazine phosphate structure and the ammonium phosphate structure are directly connected and then polymerized.
[0031] Embodiment 1 to Embodiment 8
[0032] A piperazine phosphate-ammonium phosphate copolymer flame retardant, the specific preparation method is as follows:
[0033] Piperazine diphosphate, ammonium dihydrogen phosphate and urea (the corresponding ratios of piperazine diphosphate, ammonium dihydrogen phosphate and urea in each embodiment are shown in Table 1) are ground into powder and mixed evenly, and placed in an oven for polymerization reaction (the specific copolymerization temperature and copolymerization reaction time corresponding to each embodiment are shown in Table 1). After the reaction is completed, the mixture is cooled and ground to obtain a copolymer flame retardant.
[0034] Table 1 Raw materials, polymerization temperature and polymerization time used in different embodiments and comparative examples
[0035]
[0036]
[0037] Comparative Example 1 to Comparative Example 8
[0038] A piperazine phosphate-ammonium phosphate copolymer flame retardant, the specific preparation method is as follows:
[0039] Piperazine diphosphate, ammonium dihydrogen phosphate and urea (the corresponding ratios of piperazine diphosphate, ammonium dihydrogen phosphate and urea in each embodiment are shown in Table 1) are ground into powder and mixed evenly, and placed in an oven for polymerization reaction (the specific polymerization temperature and polymerization reaction time corresponding to each embodiment are shown in Table 1). After the reaction is completed, the mixture is cooled and ground to obtain a copolymer flame retardant.
[0040] Embodiment 9 to Embodiment 17
[0041] The piperazine phosphate-ammonium phosphate copolymer flame retardant prepared in the above Examples 1 to 8 and Comparative Examples 1 to 8 is used to prepare a flame-retardant polyolefin material, and the specific preparation method is as follows:
[0042] Polyolefin, piperazine phosphate-ammonium phosphate copolymer flame retardant, melamine polyphosphate, antioxidant and processing lubricant (specific components and parts are shown in Table 2) are mixed evenly and placed in an extruder (the temperatures of each section from the main feed port to the die head of the extruder are shown in Table 3), and then melted, blended, extruded, drawn, pelletized and dried to obtain a flame retardant polyolefin material.
[0043] Table 2 Corresponding reaction raw materials and parts in the process of preparing flame-retardant polyolefin materials in Examples 9 to 17 and Comparative Examples 8 to 11
[0044]
[0045]
[0046] Table 3 Extruder parameters in the process of preparing flame-retardant polyolefin materials in Examples 9 to 17 and Comparative Examples 8 to 11
[0047] Examples or Comparative Examples Extruder parameters Example 9 170℃、180℃、190℃、190℃、190℃、190℃、190℃、190℃、180℃、220℃ Example 10 200℃、210℃、220℃、220℃、220℃、220℃、220℃、220℃、210℃、230℃ Embodiment 11 170℃、210℃、190℃、220℃、190℃、220℃、190℃、220℃、180℃、230℃ Example 12 200℃、180℃、220℃、190℃、220℃、190℃、220℃、190℃、210℃、220℃ Embodiment 13 170℃、180℃、190℃、190℃、190℃、190℃、190℃、190℃、180℃、220℃ Embodiment 14 200℃、210℃、220℃、220℃、220℃、220℃、220℃、220℃、210℃、230℃ Embodiment 15 170℃、210℃、190℃、220℃、190℃、220℃、190℃、220℃、180℃、230℃ Example 16 200℃、180℃、220℃、190℃、220℃、190℃、220℃、190℃、210℃、220℃ Embodiment 17 170℃、210℃、190℃、220℃、190℃、220℃、190℃、220℃、180℃、230℃ Embodiment 18 200℃、180℃、220℃、190℃、220℃、190℃、220℃、190℃、210℃、220℃ Comparative Example 8 170℃、180℃、190℃、190℃、190℃、190℃、190℃、190℃、180℃、220℃ Comparative Example 9 200℃、210℃、220℃、220℃、220℃、220℃、220℃、220℃、210℃、230℃ Comparative Example 10 170℃、210℃、190℃、220℃、190℃、220℃、190℃、220℃、180℃、230℃ Comparative Example 11 200℃、180℃、220℃、190℃、220℃、190℃、220℃、190℃、210℃、220℃
[0048] Comparative Example 8 to Comparative Example 11
[0049] Flame retardant polyolefin material, the specific preparation method is as follows:
[0050] Polyolefin, piperazine phosphate-ammonium phosphate copolymer flame retardant, melamine polyphosphate, antioxidant and processing lubricant (specific components and parts are shown in Table 2) are mixed evenly and placed in an extruder (the temperatures of each section from the main feed port to the die head of the extruder are shown in Table 3), and then melted, blended, extruded, drawn, pelletized and dried to obtain a flame retardant polyolefin material.
[0051] Performance Testing
[0052] The piperazine phosphate-ammonium phosphate copolymer flame retardant, diammonium phosphate and piperazine diphosphate prepared in Example 1 were subjected to infrared spectroscopy analysis, and the results are as follows: Figure 1 As shown. Figure 1 It can be seen from the infrared spectrum analysis results that the infrared spectrum peaks of the piperazine phosphate-ammonium phosphate copolymer flame retardant prepared in Example 1 are obviously different from those of diammonium phosphate and piperazine diphosphate. -1 The peak is the characteristic peak of the stretching vibration absorption of POP, indicating that a polycondensation reaction occurred during the preparation process of Example 1, proving that a product with a piperazine phosphate-ammonium phosphate copolymer flame retardant structure was prepared in Example 1.
[0053] The piperazine phosphate-ammonium phosphate copolymer flame retardant prepared in Example 1 was subjected to nuclear magnetic resonance phosphorus spectrum analysis, and the results are as follows: Figure 2 As shown. Figure 2 It can be seen that the NMR phosphorus spectrum of the piperazine phosphate-ammonium phosphate copolymer flame retardant prepared in Example 1 simultaneously shows a free phosphorus peak with a chemical shift of -0.42, terminal phosphorus peaks with chemical shifts of -10.14 and -11.16, and an intermediate phosphorus peak with a chemical shift of -23.13. The presence of the terminal and intermediate phosphorus peaks indicates that the piperazine phosphate-ammonium phosphate copolymer flame retardant structure is indeed present in the product prepared by the preparation method of Example 1.
[0054] Similarly, the piperazine phosphate-ammonium phosphate copolymer flame retardant prepared in the other embodiments above was subjected to infrared spectrum and nuclear magnetic resonance phosphorus spectrum analysis, and the results were basically the same as those in the above embodiment 1, which shows that the preparation method of the present invention can indeed prepare piperazine phosphate-ammonium phosphate copolymer flame retardant. The piperazine phosphate-ammonium phosphate copolymer flame retardant of the present invention contains both piperazine phosphate structure and ammonium phosphate structure, and the following situations may exist during the polymerization process: (1) the piperazine phosphate structure and the ammonium phosphate structure are randomly copolymerized; (2) the piperazine phosphate structure and the ammonium phosphate structure are alternately copolymerized; (3) the piperazine phosphate structure and the ammonium phosphate structure are block copolymerized.
[0055] In order to verify the performance and polymerization process of the piperazine phosphate-ammonium phosphate copolymer flame retardant prepared by the present invention, the piperazine phosphate-ammonium phosphate copolymer flame retardant prepared in Examples 1 to 8 and Comparative Examples 1 to 7 was tested for yield, TG (1% thermal weight loss), and flame retardant color. The test results are shown in Table 4. The specific test method is as follows:
[0056] (1) Yield test: the total weight of the mixture of piperazine diphosphate, ammonium dihydrogen phosphate and urea before high-temperature polymerization is m1, the weight of the piperazine phosphate-ammonium phosphate copolymer flame retardant obtained after high-temperature polymerization is m2, and the flame retardant yield = m1÷m2*100%;
[0057] (2) TG (1% thermal weight loss): carried out in accordance with the latest standard of ASTM E2550;
[0058] (3) Flame retardant color: judged by the eyes as white, gray, or black.
[0059] Table 4 Comparison of the yield, TG (1% thermal weight loss) and color performance of the corresponding flame retardants in Examples 1 to 8 and Comparative Examples 1 to 7
[0060]
[0061]
[0062] In order to verify the performance of the flame-retardant polyolefin material prepared by the piperazine phosphate-ammonium phosphate copolymer flame retardant obtained in the present invention, the flame retardant properties, flame retardant properties after boiling and precipitates on the surface of the sample strips of the corresponding polyolefin materials in Examples 9 to 18 and Comparative Examples 8 to 11 were tested. The test results are shown in Table 5. The specific test methods are as follows:
[0063] (1) Flame retardant properties: According to the latest UL94 standard, the corresponding polyolefin materials in Examples 9 to 18 and Comparative Examples 9 to 14 were placed in an oven and dried at 100° C. for 3 h, and then each material was injection molded into UL94 standard specimens using an injection molding machine;
[0064] (2) Boiling test: carried out in accordance with the latest UL746C standard, with a boiling temperature of 85°C and a boiling time of 168 hours;
[0065] (3) Spline surface precipitate test: The spline surface is judged visually.
[0066] Table 5 Comparison of flame retardancy, flame retardancy after boiling and surface precipitates of the corresponding polyolefin materials in Examples 9 to 18 and Comparative Examples 8 to 11
[0067]
[0068]
[0069] As can be seen from Table 4, the polymerization temperature and polymerization time have a crucial influence on the performance of piperazine phosphate-ammonium phosphate copolymer flame retardant, which is specifically manifested as follows: By comparing Example 1, Examples 5 to 8 and Comparative Examples 1 to 4, it can be found that when the polymerization temperature exceeds 270°C or the polymerization time exceeds 3h, the color of the copolymer flame retardant turns black, indicating that the polymerization temperature is too high and the polymerization time is too long, resulting in carbonization of the copolymer flame retardant; when the polymerization temperature is lower than 250°C or the polymerization time is less than 1h, the yield of the copolymer flame retardant is too large, and the TG (1% thermal weight loss) temperature is low, indicating that the polymerization temperature is too low and the polymerization time is too short, resulting in incomplete polymerization of the copolymer flame retardant. When the polymerization temperature is 250 to 270°C and the polymerization time is 1 to 3h, the yield, TG (1% thermal weight loss) and color performance of piperazine phosphate-ammonium phosphate copolymer flame retardant are optimal.
[0070] It can also be seen from Table 4 and Table 5 that the molar ratio of piperazine diphosphate, ammonium dihydrogen phosphate and urea has a crucial influence on the performance of piperazine phosphate-ammonium phosphate copolymer flame retardant. By comparing Examples 1 to 4, Examples 9 to 12 and Comparative Examples 5 to 8, it can be found that urea provides ammonia in high-temperature polymerization and promotes the formation of ammonium phosphate of piperazine phosphate-ammonium phosphate copolymer flame retardant. When the molar ratio of ammonium dihydrogen phosphate to urea is too little urea (Comparative Example 5), the ammonia provided is insufficient, resulting in a decrease in the yield of the copolymer flame retardant, while the urea is too much (Comparative Example 6), the ammonia exceeds the limit, and the performance of the copolymer flame retardant is not improved, and the cost of the flame retardant is increased. When the molar ratio of piperazine diphosphate to ammonium dihydrogen phosphate is too much (Comparative Example 7), excessive ammonium phosphate that is easily precipitated and easily hydrolyzed is caused in the piperazine phosphate-ammonium phosphate copolymer flame retardant. When it is applied to polyolefin materials (Comparative Example 8), the material can achieve V-0 flame retardancy, but the flame retardancy of the material fails after the water boiling test, and precipitates are produced on the surface of the sample strip; while the molar ratio of piperazine phosphate to ammonium dihydrogen phosphate is too little, which has no effect on the synthesis of the flame retardant and its application in polyolefins, but the more ammonium dihydrogen phosphate, the lower the cost.
[0071] At the same time, it can be seen from Table 5 that by comparing Examples 9 to 18 and Comparative Examples 9 to 11, it can be found that the piperazine phosphate-ammonium phosphate copolymer flame retardant is applied to polyolefin materials (polypropylene, polyethylene, vinyl elastomer), and the flame retardant performance of the polyolefin material reaches V-0 level, and the material remains flame retardant at V-0 level after boiling, and there is no precipitate on the surface of the strip; while using the ammonium polyphosphate (APP) system flame retardant, the flame retardant performance of the polyolefin material reaches V-0 level, but the material fails to flame retardant after boiling, is not flame retardant, and there are precipitates on the surface of the strip. This shows that the piperazine phosphate-ammonium phosphate copolymer flame retardant prepared by the present invention has a good application effect in the preparation and application of polyolefin materials.
[0072] In summary, the present invention provides a piperazine phosphate-ammonium phosphate copolymer flame retardant, the structural formula of the copolymer flame retardant contains both piperazine phosphate structure and ammonium phosphate structure, the piperazine phosphate-ammonium phosphate copolymer flame retardant of the present invention is formed by copolymerizing easily soluble and easily hydrolyzed ammonium phosphate (dihydrogen ammonium acid) with insoluble and intractable hydrolyzed piperazine phosphate (piperazine diphosphate), and an intumescent flame retardant having both a carbon source and an acid source is formed, the problem of easy precipitation and easy hydrolysis of traditional ammonium polyphosphate is solved, and at the same time, the low cost of ammonium phosphate is added, which is lower than the compound flame retardant of piperazine pyrophosphate and melamine polyphosphate. The piperazine phosphate-ammonium phosphate copolymer flame retardant of the present invention is used to prepare polyolefin materials, and the flame retardant performance of the prepared polyolefin materials still remains V-0 after 168h boiling, and there is no precipitate on the surface.
[0073] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing a piperazine phosphate-ammonium phosphate copolymer flame retardant, characterized in that: The preparation method comprises the following steps: Piperazine diphosphate, ammonium dihydrogen phosphate and urea are ground into powder and mixed evenly, placed in an oven at 250-270°C for polymerization reaction, cooled after the reaction, and ground to obtain a copolymer flame retardant.
2. The preparation method according to claim 1, characterized in that: The molar ratio of piperazine diphosphate, ammonium dihydrogen phosphate and urea is 1:0.5 to 1:1 to 1.2; The polymerization temperature was 260°C.
3. The preparation method according to claim 1, characterized in that: The polymerization reaction time is 1 to 3 hours.
4. The piperazine phosphate-ammonium phosphate copolymer flame retardant prepared according to the preparation method according to any one of claims 1 to 3.
5. Use of the copolymer flame retardant according to claim 4 in the preparation of flame retardant polyolefin materials.
6. Flame retardant polyolefin material, characterized in that: The flame retardant polyolefin material comprises the following components by weight: 70-77 parts of polyolefin, 14-18 parts of the piperazine phosphate-ammonium phosphate copolymer flame retardant according to claim 4, 8-12 parts of melamine polyphosphate, 0.3-0.8 parts of antioxidant and 0.3-0.5 parts of processing lubricant.
7. The flame retardant polyolefin material according to claim 6, characterized in that: The polyolefin is any one or more of polyethylene, polypropylene, polybutylene, vinyl elastomer, propylene elastomer or EPDM rubber; The antioxidant is any one or more of antioxidant 1010, antioxidant 168, antioxidant 1098 or antioxidant 1076; The processing lubricant is any one or more of calcium stearate, zinc stearate, montan wax, silicone wax, polyester sodium or pentaerythritol stearate.
8. The method for preparing the flame retardant polyolefin material according to any one of claims 6 to 7, characterized in that: The preparation method comprises the following steps: The polyolefin, the piperazine phosphate-ammonium phosphate copolymer flame retardant according to claim 4 or 5, melamine polyphosphate, antioxidant and processing lubricant are uniformly mixed and placed in an extruder, and then melted, blended, extruded, stretched, pelletized and dried to obtain a flame-retardant polyolefin material.
9. The preparation method according to claim 8, characterized in that: The temperatures of the extruder from the main feed port to the die are: 170-200°C, 180-210°C, 190-220°C, 190-220°C, 190-220°C, 190-220°C, 190-220°C, 190-220°C, 180-210°C, 220-230°C; The rotation speed of the extruder is 300-350 rpm.
Citation Information
Patent Citations
Preparation method of double-layer coated ammonium polyphosphate flame retardant
CN116376114A