Star graft modified liquid styrene-butadiene rubber as well as preparation method and application thereof
Through the preparation of star-type grafted modified liquid styrene butadiene-styrene copolymerization segment and cellulose ether-modified terpene resin, the problem of insufficient performance of liquid styrene butadiene-styrene rubber is solved, and the problem of insufficient performance of liquid styrene rubber is achieved. Efficient adhesion and stability, broaden the scope of application and reduce process complexity and cost.
Patent Information
- Application Number
- CN202310587657.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-23
AI Technical Summary
The existing liquid styrene butadhesion rubber has poor adhesion, stability, viscosity and adhesion properties, complex process and high cost, which are easy to generate gels and cause environmental pollution.
The star-type grafting structure is modified by negative ion solution polymerization method. The star-type grafting structure is formed by coupling reaction between butadiene-styrene copolymerization segment and cellulose ether-modified terpene resin segment. , improve the branching degree and compatibility of polymer chains.
It achieves good compatibility, stability and adhesion of liquid styrene butadiene rubber, broadening its application range, including as high-end adhesives, plasticizers and coatings, reducing process complexity and cost while improving the environment Influence.
Smart Images

Figure CN119019695A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of rubber preparation, and in particular to a star-shaped grafted modified liquid styrene-butadiene rubber and a preparation method and application thereof. Background Art
[0002] Liquid rubber generally refers to a polymer with a number-average molecular weight of 2000-15000 g / mol, and its viscosity changes with the relative molecular mass and molecular configuration of the polymer. Liquid rubber has the characteristics of fluidity and a wide range of bulk viscosity, simple processing, easy to achieve continuous and automated production, improved production efficiency, and reduced power consumption. Liquid rubber can be directly added with fillers and reinforcing agents to prepare rubber products, or it can be added to thermosetting resins and other polymers for modification. Liquid rubber containing functional groups is easier to extend the chain and cross-link into solid vulcanized rubber due to the presence of active functional groups, which not only greatly improves the physical properties, but also can react with many other groups to form new materials with various structures. There are many types of liquid rubber. According to whether there are functional groups and their locations, they can be divided into liquid rubber without functional groups, liquid rubber with random functional groups, and liquid rubber with terminal functional groups. Among the many types of liquid rubbers, diene liquid rubbers, especially butadiene liquid rubbers, were studied as "rubbers of the future" at the end of the 20th century because of their wide source of raw materials and low prices. Liquid nitrile rubber, liquid styrene butadiene rubber and liquid isoprene rubber have outstanding application advantages in their respective fields.
[0003] Liquid styrene butadiene rubber (LSBR) is a copolymer with low relative molecular weight made by free radical emulsion or negative (anionic) ion polymerization with butadiene and styrene as monomers. It has a molecular weight of 2000-15000g / mol and is a light yellow or light brown transparent viscous liquid. Liquid styrene butadiene rubber has excellent electrical insulation and physical properties, and is insoluble in general organic solvents and does not melt when heated. Liquid styrene butadiene rubber has the characteristics of good compatibility with certain general rubbers, so they can be mixed and used, and fillers and oils can also be added at the same time. Since these mixed components are evenly dispersed and have good pouring fluidity, they can be injection molded to produce hard rubber products. They can also be used as plasticizers for styrene butadiene rubber, nitrile rubber and chloroprene rubber, or as adhesives, sealing materials, etc. It can also be used to make high-end coatings, expanding the scope of application.
[0004] Reports at home and abroad are that liquid rubber is used in different fields or various polymers are modified by liquid rubber, and most of them are liquid nitrile rubber, liquid isoprene rubber, etc., or liquid rubber is modified by terminalization. The poor adhesion, stability, viscosity, and branching degree of the prepared liquid rubber, as well as the improvement of the viscosity and adhesion performance of the copolymer system are problems that need to be solved in this field. In addition, there are also problems such as complex process, difficult actual operation, long reaction cycle, high cost, easy generation of gel, and environmental pollution. Summary of the invention
[0005] The purpose of the present invention is to overcome the problems of poor adhesion, stability, viscosity, adhesion performance and branching degree of liquid rubber in the prior art, and to provide a star-shaped grafted modified liquid styrene-butadiene rubber and a preparation method and application thereof.
[0006] The inventor of the present invention found in research that the liquid styrene butadiene rubber can be modified by using a common liquid styrene butadiene rubber anion solution polymerization method, which is simple and reliable. Thus, the present invention is obtained.
[0007] In order to achieve the above-mentioned purpose, the first aspect of the present invention provides a star-shaped grafted modified liquid styrene butadiene rubber, wherein the modified liquid styrene butadiene rubber comprises a polymer segment from a coupling agent and a plurality of butadiene-styrene copolymer segments and cellulose ether modified terpene resin segments grafted on the polymer segment, wherein the coupling agent is selected from polyvinyl aromatic monomers.
[0008] A second aspect of the present invention provides a method for preparing a star-shaped graft-modified liquid styrene-butadiene rubber, wherein the preparation method comprises:
[0009] (1) in the presence of an initiator and a polar activator, copolymerizing butadiene and styrene to obtain an active butadiene-styrene copolymer segment;
[0010] (2) subjecting the active butadiene-styrene copolymer segment to a coupling reaction with a coupling agent to obtain an active chain;
[0011] (3) subjecting the active chain to polymerization reaction with a modified terpene resin to obtain the star-shaped grafted modified liquid styrene-butadiene rubber.
[0012] The third aspect of the present invention provides a star-shaped grafted modified liquid styrene-butadiene rubber obtained by the preparation method.
[0013] The fourth aspect of the present invention provides the star-shaped grafted modified liquid styrene butadiene rubber and the star-shaped grafted modified liquid styrene butadiene rubber obtained by the preparation method and their applications in the field of rubber processing.
[0014] Through the above technical scheme, the invention provides a modified liquid styrene butadiene rubber. From the perspective of the structure of the polymer chain, it is a branched polymer with a star-shaped structure, that is, multiple molecular chains are grafted on the polymer chain segment to form different segments as branches, and similarly connected molecular arms (such as polybutadiene styrene arms, modified terpene resin polymer arms) are called mixed arms. In the modified liquid styrene butadiene rubber, the polymer chain segment formed by the coupling agent is equivalent to the polybutadiene-styrene rubber and the modified terpene resin as the core and chained together, realizing the combination of different polymer molecular chains at the short-range structural level of the polymer chain, and having good compatibility, stability and adhesion. The obtained modified liquid styrene butadiene rubber improves the viscosity, adhesion and other properties of the copolymer system, and can be used as high-end adhesives, plasticizers, coatings, and expands the scope of application. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 It is a schematic diagram of the molecular chain structure of star-shaped grafted modified liquid styrene-butadiene rubber.
[0016] Description of Reference Numerals
[0017] PSB-represents butadiene-styrene copolymer segment, and PT-represents cellulose ether modified terpene resin segment. DETAILED DESCRIPTION
[0018] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0019] The first aspect of the present invention provides a star-shaped grafted modified liquid styrene butadiene rubber, wherein the modified liquid styrene butadiene rubber comprises a polymer segment from a coupling agent and a plurality of butadiene-styrene copolymer segments and cellulose ether modified terpene resin segments grafted on the polymer segment, wherein the coupling agent is selected from polyvinyl aromatic monomers.
[0020] In the present invention, the modified liquid styrene-butadiene rubber provided is a branched polymer from the perspective of the structure of the polymer chain, and has a star-shaped structure, wherein the polymer segment formed by the coupling agent serves as the polymer core, and the multiple vinyl functional groups possessed by the coupling agent provide the polymer segment with multiple vinyl groups that can further graft other branches; the butadiene-styrene copolymer chain and the cellulose ether modified terpene resin chain can be bonded to the vinyl groups on the polymer segment through the carbon-carbon double bonds contained in each of them, to form a butadiene-styrene copolymer segment and a cellulose ether modified terpene resin segment grafted on the polymer segment, that is, a plurality of molecular chains are grafted on the polymer segment to form different segments as branches, and similarly connected molecular arms (such as polybutadiene styrene arms, modified terpene resin polymer arms) can be called mixed arms. In the modified liquid styrene-butadiene rubber, the polybutadiene-styrene rubber and the modified terpene resin are chained together with the polymer chain segments formed by the coupling agent as the core, thereby realizing the combination of different polymer molecular chains at the short-range structural level of the polymer chain, and having good compatibility, stability and adhesion.
[0021] In the present invention, the coupling agent is selected from polyvinyl aromatic monomers, which form polymer segments with multi-terminal molecular arms through self-polymerization, thereby forming polymers with a high degree of branching.
[0022] In some specific embodiments of the present invention, in the modified liquid styrene-butadiene rubber, based on the sum of the weights of the butadiene-styrene copolymer segment and the cellulose ether modified terpene resin segment, the content of the cellulose ether modified terpene resin segment is 20-80wt%, and the content of the butadiene-styrene copolymer segment is 20-80wt%. By limiting the modified liquid styrene-butadiene rubber to the above content, the combination of different polymer molecular chains at the short-range structural level of the polymer chain is achieved, and good compatibility, stability and adhesion can be achieved.
[0023] In some embodiments of the present invention, in the modified liquid styrene-butadiene rubber, based on the sum of the weights of the butadiene-styrene copolymer segment and the cellulose ether-modified terpene resin segment, the content of the cellulose ether-modified terpene resin segment can be selected from 20wt%, 30wt%, 40wt%, 50wt%, 60wt%, 70wt%, 80wt% and any value in the range consisting of any two of the above values. The content of the butadiene-styrene copolymer segment can be selected from 20wt%, 30wt%, 40wt%, 50wt%, 60wt%, 70wt%, 80wt% and any value in the range consisting of any two of the above values.
[0024] In some specific embodiments of the present invention, in the butadiene-styrene copolymer segment, the content of the butadiene structural unit is 50-90wt%, and the content of the styrene structural unit is 10-50wt%. By limiting the modified liquid styrene-butadiene rubber with the above content, the combination of different polymer molecular chains at the short-range structural level of the polymer chain is achieved, and good compatibility, stability and adhesion can be achieved.
[0025] In some embodiments of the present invention, in the butadiene-styrene copolymer segment, the content of the butadiene structural unit can be selected from 50wt%, 60wt%, 70wt%, 80wt%, 90wt%, and any value in the range of any two of the above values. The content of the styrene structural unit can be selected from 10wt%, 20wt%, 30wt%, 40wt%, 50wt%, and any value in the range of any two of the above values.
[0026] In some specific embodiments of the present invention, in the cellulose ether modified terpene resin segment, the content of the cellulose ether is 10-40wt%, and the content of the terpene resin is 60-90wt%. By limiting the modified liquid styrene-butadiene rubber with the above content, the combination of different polymer molecular chains at the short-range structural level of the polymer chain is achieved, and good compatibility, stability and adhesion can be achieved. Among them, the higher the content of terpene resin in the cellulose ether modified terpene resin segment, the higher the average binding force of the star-shaped grafted modified liquid styrene-butadiene rubber, and the better the anti-slip property, high temperature anti-flow performance and adhesion binding force of the liquid styrene-butadiene rubber.
[0027] In some embodiments of the present invention, the content of the cellulose ether in the cellulose ether modified terpene resin segment can be selected from 10wt%, 20wt%, 30wt%, 40wt%, and any value in the range of any two of the above values. The content of the terpene resin can be selected from 60wt%, 70wt%, 80wt%, 90wt%, and any value in the range of any two of the above values.
[0028] In some specific embodiments of the present invention, preferably, the coupling agent is selected from divinylbenzene.
[0029] In some specific embodiments of the present invention, in the modified liquid styrene-butadiene rubber, the amount of the coupling agent is relatively small, the polymer segment formed by the coupling agent is used as a core, the core formed by the coupling agent is a macromolecular active species, and the macromolecular active species provides the polymer with multiple reactive active points that can further initiate polymerization of the reaction monomers, thereby initiating polymerization of the monomers to form polymer segments. The proportion of the polymer segment formed by the coupling agent itself is very small relative to the amount of the macromolecular polymer, and the content can be excluded from the polymer proportion. The amount of the coupling agent has been described in the text.
[0030] In the present invention, the functionality is the active point on the polymer chain that can react chemically to generate new bonds. The more active points are formed, the more polymer segments are formed by initiating monomer polymerization, the better the branching of the modified liquid styrene-butadiene rubber, the greater the functionality. By characterizing and analyzing the polymer segments, the amount of polymer segments formed by the coupling agent can be determined by the polymer functionality.
[0031] In some specific embodiments of the present invention, the number average molecular weight of the modified liquid styrene butadiene rubber is 3000-25000 g / mol, the viscosity at 25° C. is 20-60 Pa·S, and the functionality is 4-7. The higher the viscosity, the better the adhesive property of the liquid styrene butadiene rubber; the higher the functionality, the better the branching property of the modified liquid styrene butadiene rubber.
[0032] A second aspect of the present invention provides a method for preparing a star-shaped graft-modified liquid styrene-butadiene rubber, wherein the preparation method comprises:
[0033] (1) in the presence of an initiator and a polar activator, copolymerizing butadiene and styrene to obtain an active butadiene-styrene copolymer segment;
[0034] (2) subjecting the active butadiene-styrene copolymer segment to a coupling reaction with a coupling agent to obtain an active chain;
[0035] (3) subjecting the active chain to polymerization reaction with a modified terpene resin to obtain the star-shaped grafted modified liquid styrene-butadiene rubber.
[0036] In some specific embodiments of the present invention, the preparation method of the modified terpene resin comprises: mixing the terpene resin and a solvent, and then adding cellulose ether to obtain the modified terpene resin.
[0037] In some specific embodiments of the present invention, the cellulose ether is selected from one or more of sodium methyl cellulose, sodium hydroxypropyl methyl cellulose, and sodium carboxymethyl cellulose.
[0038] The invention utilizes a negative ion solution polymerization method to prepare the star-shaped grafted modified liquid styrene butadiene rubber, and modifies the liquid styrene butadiene rubber. The method is simple and reliable.
[0039] In the present invention, in step (1), butadiene, styrene monomer and initiator are sequentially added to the polymerization system, and after the first monomer polymerization is completed, a coupling agent is added to carry out a coupling reaction to obtain the star-shaped grafted modified liquid styrene butadiene rubber. In step (3), a modified terpene resin is added and polymerized to obtain the star-shaped grafted modified liquid styrene butadiene rubber.
[0040] In some specific embodiments of the present invention, the coupling reaction is that the polymer segment formed by the coupling agent and the butadiene-styrene copolymer chain are bonded to the vinyl group on the polymer segment through the carbon-carbon double bond contained therein to obtain the active chain.
[0041] In some specific embodiments of the present invention, the solvent is selected from one or more of pentane, hexane, octane, heptane, cyclohexane, benzene, toluene and ethylbenzene, preferably cyclohexane.
[0042] In some specific embodiments of the present invention, the polar activator is selected from one or more of diethylene glycol dimethyl ether, tetrahydrofuran, ethyl ether, ethyl methyl ether, anisole, diphenyl ether, ethylene glycol dimethyl ether, triethylamine, tetramethylethylenediamine and hexamethylphosphonic triamide, preferably selected from one or more of diethylene glycol dimethyl ether, tetrahydrofuran and tetramethylethylenediamine. Polar organic compounds need to be added as activators in the polymerization system of the present invention to make the initiator produce polarization or solvation effects, reduce its degree of association, and increase the initiation reaction speed of initiators such as n-butyl lithium. The activator can also adjust the reactivity ratio of butadiene and styrene to make the two copolymerize randomly. At the same time, the polar activator can increase the 1,2-structure content in the butadiene unit.
[0043] In some specific embodiments of the present invention, the initiator is selected from one or more of n-butyllithium, sec-butyllithium, methylbutyllithium, phenylbutyllithium, naphthalenelithium, cyclohexyllithium and dodecyllithium, preferably selected from n-butyllithium and / or sec-butyllithium.
[0044] In some specific embodiments of the present invention, the coupling agent is selected from polyvinyl aromatic hydrocarbons, preferably divinyl benzene.
[0045] In some specific embodiments of the present invention, the copolymerization reaction temperature is 50-90° C., the copolymerization reaction pressure is 0.1-0.25 MPa, and the copolymerization reaction time is 20-80 min.
[0046] In some specific embodiments of the present invention, the coupling reaction temperature is 50-90° C., the coupling reaction pressure is 0.1-0.25 MPa, and the coupling reaction time is 60-90 min.
[0047] In some specific embodiments of the present invention, the polymerization reaction temperature is 50-90° C., the polymerization reaction pressure is 0.1-0.25 MPa, and the polymerization reaction time is 60-100 min.
[0048] In some specific embodiments of the present invention, after the reaction is complete, the obtained polymer solution is treated with water, and the amount of water used is generally 100-300 times the amount of the initiator used, preferably 150-250 times.
[0049] In some specific embodiments of the present invention, 0.5%-1% of the polymer weight of an antioxidant can be added to the obtained star-shaped grafted modified liquid styrene butadiene rubber, and then high-performance star-shaped grafted modified liquid styrene butadiene rubber is obtained through washing, dehydration and drying.
[0050] In some specific embodiments of the present invention, the mixed monomer of butadiene and styrene is 20-80 parts by weight, wherein butadiene accounts for 60-90wt% of the mixed monomer amount, and styrene accounts for 10-40wt% of the mixed monomer amount; preferably, the mixed monomer of butadiene and styrene is 30-70 parts by weight, wherein butadiene accounts for 70-90wt% of the mixed monomer amount, and styrene accounts for 10-30wt% of the mixed monomer amount.
[0051] In some specific embodiments of the present invention, the modified terpene resin is 20-80 parts by weight, wherein the cellulose ether accounts for 10-40wt% of the modified terpene resin, and the terpene resin accounts for 60-90wt% of the modified terpene resin; preferably, the modified terpene resin is 30-70 parts by weight, wherein the cellulose ether accounts for 10-30wt% of the modified terpene resin, and the terpene resin accounts for 70-90wt% of the modified terpene resin;
[0052] In some specific embodiments of the present invention, the initiator is 0.02-0.2 parts by weight, preferably 0.025-0.1 parts by weight.
[0053] In some specific embodiments of the present invention, the molar ratio of the polar activator to the initiator is 0.1-30:1, preferably 0.1-20:1.
[0054] In some specific embodiments of the present invention, the molar ratio of the coupling agent to the initiator is 0.1-1.5:1, preferably 0.1-1:1.
[0055] In the present invention, the functionality is determined by gel permeation chromatography, and the composition and structure of the star-shaped grafted modified liquid styrene-butadiene rubber can be determined by nuclear magnetic resonance, infrared, GPC, elemental analysis, etc., or by preparing and feeding.
[0056] The third aspect of the present invention provides a star-shaped grafted modified liquid styrene-butadiene rubber obtained by the preparation method, which may have the aforementioned composition and structural characteristics, which will not be described in detail.
[0057] The fourth aspect of the present invention provides the star-shaped grafted modified liquid styrene butadiene rubber and the star-shaped grafted modified liquid styrene butadiene rubber obtained by the preparation method and their applications in the field of rubber processing.
[0058] The present invention will be described in detail below through examples.
[0059]
[0060] Determination of molecular weight: The molecular weight and distribution of the sample were analyzed using a Viscoteck TDA 302 gel permeation chromatograph (GPC) from Agilent Technologies, USA.
[0061] Determination of viscosity: Determine according to GJB 2050-1994 using a rotational viscometer and cone-plate viscometer method.
[0062] Fourier transform infrared spectroscopy (FTIR) analysis: The analysis was performed using the American Nicolet 560 FTIR instrument, without purification, and with potassium bromide tablets and films. It is used to determine the styrene content and butadiene content in the modified liquid styrene-butadiene rubber structure.
[0063] Determination of peeling force: The average bonding strength was tested according to GB / T7124-2008 using the 5567 universal material testing machine produced by Instron, USA.
[0064] In the following examples and comparative examples, if no specific conditions are specified, the conditions are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are conventional products that can be obtained through commercial channels. The composition and structure of the modified liquid styrene-butadiene rubber described in the following examples and comparative examples can be determined by nuclear magnetic resonance, infrared, GPC, elemental analysis, etc., or by preparing and feeding.
[0065] Example 1
[0066] 1) Preparation of modified terpene resin: In a reaction kettle, 4212 g of cyclohexane and 374 g of terpene resin were added, heated to 80° C. and stirred until they were completely dissolved, then 94 g of dissolved sodium methyl cellulose was added, and stirred and mixed uniformly to obtain a modified terpene resin (wherein, in the obtained cellulose ether modified terpene resin segment, the content of terpene resin was 80 wt %, and the content of cellulose ether was 20 wt %).
[0067] 2) In a 15L stainless steel reactor with a jacket, argon was passed through the system to replace 3 times. 4212g of cyclohexane, 234g of butadiene, 234g of styrene, 44.93g of tetrahydrofuran were added to the polymerization reactor, and then 0.624mol of n-butyl lithium was added, and the temperature was raised to 50°C, and the polymerization was carried out for 80min. After the monomers were completely converted, the temperature was raised to 80°C (wherein, in the obtained butadiene-styrene copolymer segment, the content of butadiene structural units was 50wt%, and the content of styrene structural units was 50wt%), 0.249mol of divinylbenzene was added to continue coupling, and after the reaction for 60min, the mixture of 468g of the prepared modified terpene resin and 4212g of cyclohexane was pressed into the polymerization reactor, and the reaction was continued for 60min. After the reaction was completed, the reaction mixture after coupling was treated with water, and 100g of water and 12g of antioxidant 1010 were added and stirred. The rubber solution is coagulated by wet method and dried to obtain high-performance star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 50wt%, and the content of the butadiene-styrene copolymer segment is 50wt%).
[0068] Example 2
[0069] 1) Preparation of modified terpene resin: In a reaction kettle, 4212 g of cyclohexane and 374 g of terpene resin were added, heated to 80° C. and stirred until they were completely dissolved, then 94 g of dissolved sodium methyl cellulose was added, and stirred and mixed uniformly to obtain a modified terpene resin (wherein, in the obtained cellulose ether modified terpene resin segment, the content of terpene resin was 80 wt %, and the content of cellulose ether was 20 wt %).
[0070] 2) In a 15L stainless steel reactor with a jacket, the system was replaced 3 times by passing argon. 4212g of cyclohexane, 234g of butadiene, 234g of styrene, 29.95g of tetrahydrofuran, and 0.416mol of n-butyl lithium were added to the polymerization reactor, the temperature was raised to 50°C, and the polymerization was carried out for 80min. After the monomers were completely converted, the temperature was raised to 80°C (wherein, in the obtained butadiene-styrene copolymer segment, the content of butadiene structural units was 50wt%, and the content of styrene structural units was 50wt%), 0.167mol of divinylbenzene was added to continue coupling, and after the reaction for 60min, the mixture of 468g of the prepared modified terpene resin and 4212g of cyclohexane was pressed into the polymerization reactor, and the reaction was continued for 60min. After the reaction was completed, the reaction mixture after coupling was treated with water, 100g of water and 12g of antioxidant 1010 were added, and stirred. The rubber solution is coagulated by wet method and dried to obtain high-performance star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 50wt%, and the content of the butadiene-styrene copolymer segment is 50wt%).
[0071] Example 3
[0072] 1) Preparation of modified terpene resin: In a reaction kettle, 4212 g of cyclohexane and 327 g of terpene resin were added, heated to 80° C. and stirred until they were completely dissolved, then 141 g of dissolved sodium methyl cellulose was added, and stirred and mixed uniformly to obtain a modified terpene resin (wherein, in the obtained cellulose ether modified terpene resin segment, the content of terpene resin was 70 wt % and the content of cellulose ether was 30 wt %).
[0073] 2) In a 15L stainless steel reactor with a jacket, the system was replaced 3 times by passing argon. 4212g of cyclohexane, 234g of butadiene, 234g of styrene, 44.93g of tetrahydrofuran, and 0.936mol of n-butyl lithium were added to the polymerization reactor, the temperature was raised to 50°C, and the polymerization was carried out for 80min. After the monomers were completely converted, the temperature was raised to 80°C (wherein, in the obtained butadiene-styrene copolymer segment, the content of butadiene structural units was 50wt%, and the content of styrene structural units was 50wt%), 0.374mol of divinylbenzene was added to continue coupling, and after the reaction for 60min, the mixture of 468g of the prepared modified terpene resin and 4212g of cyclohexane was pressed into the polymerization reactor, and the reaction was continued for 60min. After the reaction was completed, the reaction mixture after coupling was treated with water, 100g of water and 12g of antioxidant 1010 were added, and stirred. The glue solution is coagulated by wet method and dried to obtain star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 50wt%, and the content of the butadiene-styrene copolymer segment is 50wt%).
[0074] Example 4
[0075] 1) Preparation of modified terpene resin: In a reaction kettle, 4212 g of cyclohexane and 327 g of terpene resin were added, heated to 80° C. and stirred until they were completely dissolved, then 141 g of dissolved sodium methyl cellulose was added, and stirred and mixed uniformly to obtain a modified terpene resin (wherein, in the obtained cellulose ether modified terpene resin segment, the content of terpene resin was 70 wt % and the content of cellulose ether was 30 wt %).
[0076] 2) In a 15L stainless steel reactor with a jacket, the system was replaced 3 times by passing argon. 4212g of cyclohexane, 234g of butadiene, 234g of styrene, 44.93g of tetrahydrofuran, and 0.624mol of n-butyl lithium were added to the polymerization reactor, the temperature was raised to 50°C, and the polymerization was carried out for 80min. After the monomers were completely converted, the temperature was raised to 80°C (wherein, in the obtained butadiene-styrene copolymer segment, the content of butadiene structural units was 50wt%, and the content of styrene structural units was 50wt%), 0.249mol of divinylbenzene was added to continue coupling, and after the reaction for 60min, the mixture of 468g of the prepared modified terpene resin and 4212g of cyclohexane was pressed into the polymerization reactor, and the reaction was continued for 60min. After the reaction was completed, the reaction mixture after coupling was treated with water, 100g of water and 12g of antioxidant 1010 were added, and stirred. The glue solution is coagulated by wet method and dried to obtain star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 50wt%, and the content of the butadiene-styrene copolymer segment is 50wt%).
[0077] Example 5
[0078] 1) Preparation of modified terpene resin: In a reaction kettle, 2527 g of cyclohexane and 197 g of terpene resin were added, heated to 80° C. and stirred until they were completely dissolved, then 84 g of dissolved sodium methyl cellulose was added, and stirred and mixed uniformly to obtain a modified terpene resin (wherein, in the obtained cellulose ether modified terpene resin segment, the content of terpene resin was 70 wt % and the content of cellulose ether was 30 wt %).
[0079] 2) In a 15L stainless steel reactor with a jacket, the system was replaced 3 times by passing argon. 5897g of cyclohexane, 468g of butadiene, 187g of styrene, 37.73g of tetrahydrofuran, and 0.524mol of n-butyl lithium were added to the polymerization reactor, the temperature was raised to 50°C, and the polymerization was carried out for 80min. After the monomers were completely converted, the temperature was raised to 80°C (wherein, in the obtained butadiene-styrene copolymer segment, the content of butadiene structural units was 70wt%, and the content of styrene structural units was 30wt%), 0.212mol of divinylbenzene was added to continue coupling, and after the reaction for 60min, a mixture of 281g of the prepared modified terpene resin and 2527g of cyclohexane was pressed into the polymerization reactor, and the reaction was continued for 60min. After the reaction was completed, the reaction mixture after coupling was treated with water, 100g of water and 12g of antioxidant 1010 were added, and stirred. The glue solution is coagulated by wet method and dried to obtain star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 30wt%, and the content of the butadiene-styrene copolymer segment is 70wt%).
[0080] Example 6
[0081] 1) Preparation of modified terpene resin: In a reaction kettle, add 2527g of cyclohexane and 225g of terpene resin, heat to 80°C and stir until they are completely dissolved, then add 56g of dissolved sodium methyl cellulose, stir and mix evenly to obtain a modified terpene resin (wherein, in the obtained cellulose ether modified terpene resin segment, the content of terpene resin is 80wt%, and the content of cellulose ether is 20wt%).
[0082] 2) In a 15L stainless steel reactor with a jacket, the system was replaced 3 times by passing argon. 5897g of cyclohexane, 468g of butadiene, 187g of styrene, 23.58g of tetrahydrofuran, and 0.327mol of n-butyl lithium were added to the polymerization reactor, the temperature was raised to 50°C, and the polymerization was carried out for 80min. After the monomers were completely converted, the temperature was raised to 80°C (wherein, in the obtained butadiene-styrene copolymer segment, the content of butadiene structural units was 70wt%, and the content of styrene structural units was 30wt%), 0.131mol of divinylbenzene was added to continue coupling, and after the reaction for 60min, a mixture of 281g of the prepared modified terpene resin and 2527g of cyclohexane was pressed into the polymerization reactor, and the reaction was continued for 60min. After the reaction was completed, the reaction mixture after coupling was treated with water, 100g of water and 12g of antioxidant 1010 were added, and stirred. The glue solution is coagulated by wet method and dried to obtain star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 30wt%, and the content of the butadiene-styrene copolymer segment is 70wt%).
[0083] Example 7
[0084] 1) Preparation of modified terpene resin: In a reaction kettle, 2527 g of cyclohexane and 225 g of terpene resin (accounting for 80 wt% of the modified terpene resin segment) were added, heated to 80° C. and stirred until completely dissolved, then 56 g of dissolved sodium methyl cellulose (accounting for 20 wt% of the modified terpene resin segment) was added, and the mixture was stirred and mixed uniformly to obtain a modified terpene resin (wherein, in the obtained cellulose ether modified terpene resin segment, the content of terpene resin was 80 wt% and the content of cellulose ether was 20 wt%).
[0085] 2) In a 15L stainless steel reactor with a jacket, argon was passed through the system to replace 3 times. 5897g of cyclohexane, 557g of butadiene, 98g of styrene, 37.73g of tetrahydrofuran, and 0.524mol of n-butyl lithium were added to the polymerization reactor, the temperature was raised to 50°C, and the polymerization was carried out for 80min. After the monomers were completely converted, the temperature was raised to 80°C (wherein, in the obtained butadiene-styrene copolymer segment, the content of butadiene structural units was 85wt%, and the content of styrene structural units was 15wt%), 0.212mol of divinylbenzene was added to continue coupling, and after the reaction for 60min, a mixture of 281g (30wt% of the total amount) of the prepared modified terpene resin and 2527g of cyclohexane was pressed into the polymerization reactor, and the reaction was continued for 60min. After the reaction was completed, the reaction mixture after coupling was treated with water, 100g of water and 12g of antioxidant 1010 were added, and stirred. The glue solution is coagulated by wet method and dried to obtain star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 30wt%, and the content of the butadiene-styrene copolymer segment is 70wt%).
[0086] Example 8
[0087] 1) Preparation of modified terpene resin: In a reaction kettle, 2527 g of cyclohexane and 197 g of terpene resin were added, heated to 80° C. and stirred until they were completely dissolved, then 84 g of dissolved sodium methyl cellulose was added, and stirred and mixed uniformly to obtain a modified terpene resin (wherein, in the obtained cellulose ether modified terpene resin segment, the content of terpene resin was 70 wt % and the content of cellulose ether was 30 wt %).
[0088] 2) In a 15L stainless steel reactor with a jacket, the system was replaced 3 times by passing argon. 5897g of cyclohexane, 557g of butadiene, 98g of styrene, 53.90g of tetrahydrofuran, and 0.504mol of n-butyl lithium were added to the polymerization reactor, the temperature was raised to 50°C, and the polymerization was carried out for 80min. After the monomers were completely converted, the temperature was raised to 80°C (wherein, in the obtained butadiene-styrene copolymer segment, the content of butadiene structural units was 85wt%, and the content of styrene structural units was 15wt%), 0.301mol of divinylbenzene was added to continue coupling, and after the reaction for 60min, a mixture of 281g of the prepared modified terpene resin and 2527g of cyclohexane was pressed into the polymerization reactor, and the reaction was continued for 60min. After the reaction was completed, the reaction mixture after coupling was treated with water, 100g of water and 12g of antioxidant 1010 were added, and stirred. The glue solution is coagulated by wet method and dried to obtain star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 30wt%, and the content of the butadiene-styrene copolymer segment is 70wt%).
[0089] Example 9
[0090] 1) Preparation of modified terpene resin: In a reaction kettle, add 2611 g of cyclohexane and 211 g of terpene resin, heat to 80° C. and stir until they are completely dissolved, then add 70 g of dissolved sodium methyl cellulose, stir and mix evenly to obtain a modified terpene resin (wherein, in the obtained cellulose ether modified terpene resin segment, the content of terpene resin is 75 wt %, and the content of cellulose ether is 25 wt %).
[0091] 2) In a 15L stainless steel reactor with a jacket, the system was replaced 3 times by passing argon. 5813g of cyclohexane, 478g of butadiene, 84g of styrene, 37.73g of tetrahydrofuran, and 0.281mol of n-butyl lithium were added to the polymerization reactor, the temperature was raised to 50°C, and the polymerization was carried out for 80min. After the monomers were completely converted, the temperature was raised to 80°C (wherein, the content of butadiene structural units in the obtained butadiene-styrene copolymer segment was 85wt%, and the content of styrene structural units was 15wt%), 0.212mol of divinylbenzene was added to continue coupling, and after the reaction for 60min, a mixture of 281g of the prepared modified terpene resin and 2527g of cyclohexane was pressed into the polymerization reactor, and the reaction was continued for 60min. After the reaction was completed, the reaction mixture after coupling was treated with water, 100g of water and 12g of antioxidant 1010 were added, and stirred. The glue solution is coagulated by wet method and dried to obtain star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 30wt%, and the content of the butadiene-styrene copolymer segment is 70wt%).
[0092] Example 10
[0093] 1) Preparation of modified terpene resin: In a reaction kettle, add 2527g of cyclohexane and 225g of terpene resin, heat to 80°C and stir until they are completely dissolved, then add 56g of dissolved sodium methyl cellulose, stir and mix evenly to obtain a modified terpene resin (wherein, in the obtained cellulose ether modified terpene resin segment, the content of terpene resin is 80wt%, and the content of cellulose ether is 20wt%).
[0094] 2) In a 15L stainless steel reactor with a jacket, the system was replaced 3 times by passing argon. 5897g of cyclohexane, 468g of butadiene, 187g of styrene, 23.58g of tetrahydrofuran, and 0.197mol of n-butyl lithium were added to the polymerization reactor, the temperature was raised to 50°C, and the polymerization was carried out for 80min. After the monomers were completely converted, the temperature was raised to 80°C (wherein, in the obtained butadiene-styrene copolymer segment, the content of butadiene structural units was 70wt%, and the content of styrene structural units was 30wt%), 0.197mol of divinylbenzene was added to continue coupling, and after the reaction for 60min, a mixture of 281g of the prepared modified terpene resin and 2527g of cyclohexane was pressed into the polymerization reactor, and the reaction was continued for 60min. After the reaction was completed, the reaction mixture after coupling was treated with water, 100g of water and 12g of antioxidant 1010 were added, and stirred. The glue solution is coagulated by wet method and dried to obtain star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 30wt%, and the content of the butadiene-styrene copolymer segment is 70wt%).
[0095] Embodiment 11
[0096] 1) Preparation of modified terpene resin: In a reaction kettle, add 2527g of cyclohexane and 225g of terpene resin, heat to 80°C and stir until they are completely dissolved, then add 56g of dissolved sodium methyl cellulose, stir and mix evenly to obtain a modified terpene resin (wherein, in the obtained cellulose ether modified terpene resin segment, the content of terpene resin is 80wt%, and the content of cellulose ether is 20wt%).
[0097] 2) In a 15L stainless steel reactor with a jacket, the system was replaced 3 times by passing argon. 5897g of cyclohexane, 468g of butadiene, 187g of styrene, 23.58g of tetrahydrofuran, and 0.143mol of n-butyl lithium were added to the polymerization reactor, the temperature was raised to 50°C, and the polymerization was carried out for 80min. After the monomers were completely converted, the temperature was raised to 80°C (wherein, in the obtained butadiene-styrene copolymer segment, the content of butadiene structural units was 70wt%, and the content of styrene structural units was 30wt%), 0.172mol of divinylbenzene was added to continue coupling, and after the reaction for 60min, a mixture of 281g of the prepared modified terpene resin and 2527g of cyclohexane was pressed into the polymerization reactor, and the reaction was continued for 60min. After the reaction was completed, the reaction mixture after coupling was treated with water, 100g of water and 12g of antioxidant 1010 were added, and stirred. The glue solution is coagulated by wet method and dried to obtain star-shaped grafted modified liquid styrene butadiene rubber (wherein, in the modified liquid styrene butadiene rubber, the content of the cellulose ether modified terpene resin segment is 30wt%, and the content of the butadiene-styrene copolymer segment is 70wt%).
[0098] Comparative Example 1
[0099] The method of Example 1 is followed, except that the terpene resin is not modified, that is, the styrene-butadiene rubber segment and the terpene resin are directly coupled and then coagulated.
[0100] The specific preparation steps are as follows: In a 15L stainless steel reactor with a jacket, argon is passed through the system to replace 3 times. 4212g of cyclohexane, 234g of butadiene (accounting for 50wt% of the mixed monomer amount), 234g of styrene (accounting for 50wt% of the mixed monomer amount), 44.93g of tetrahydrofuran, and 0.624mol of n-butyl lithium are added to the polymerization reactor, the temperature is raised to 50°C, and the polymerization is carried out for 80min. After the monomer is completely converted, the temperature is raised to 80°C, and 0.249mol of divinylbenzene is added to continue coupling. After the reaction is carried out for 60min, a mixture of 468g of terpene resin (accounting for 50wt% of the total amount) and 4212g of cyclohexane is pressed into the polymerization reactor, and the reaction is continued for 60min. After the reaction is completed, the reaction mixture after coupling is treated with water, 100g of water and 12g of antioxidant 1010 are added, and stirred. The glue solution is wet-coagulated and dried to obtain liquid styrene-butadiene rubber.
[0101] Comparative Example 2
[0102] The method of Example 2 is followed, except that the terpene resin is not modified, that is, the styrene-butadiene rubber segment and the terpene resin are directly coupled and then coagulated.
[0103] The specific preparation steps are as follows: In a 15L stainless steel reactor with a jacket, argon is passed through the system to replace 3 times. 4212g of cyclohexane, 234g of butadiene (accounting for 50wt% of the mixed monomer amount), 234g of styrene (accounting for 50wt% of the mixed monomer amount), 29.95g of tetrahydrofuran, and then 0.416mol of n-butyl lithium are added to the polymerization reactor, the temperature is raised to 50°C, and the polymerization is carried out for 80min. After the monomer is completely converted, the temperature is raised to 80°C, and 0.167mol of divinylbenzene is added to continue coupling. After the reaction is completed for 60min, a mixture of 468g of terpene resin (accounting for 50wt% of the total amount) and 4212g of cyclohexane is pressed into the polymerization reactor, and the reaction is continued for 60min. After the reaction is completed, the reaction mixture after coupling is treated with water, 100g of water and 12g of antioxidant 1010 are added, and stirred. The glue solution is wet-coagulated and dried to obtain liquid styrene-butadiene rubber.
[0104] Comparative Example 3
[0105] The method of Example 3 is followed, except that the terpene resin is not modified, that is, the styrene-butadiene rubber segment and the terpene resin are directly coupled and then coagulated.
[0106] The specific preparation steps are as follows: In a 15L stainless steel reactor with a jacket, argon is passed through the system to replace 3 times. 4212g of cyclohexane, 234g of butadiene (accounting for 50wt% of the mixed monomer amount), 234g of styrene (accounting for 50wt% of the mixed monomer amount), 44.93g of tetrahydrofuran, and 0.936mol of n-butyl lithium are added to the polymerization reactor, the temperature is raised to 50°C, and the polymerization is carried out for 80min. After the monomer is completely converted, the temperature is raised to 80°C, and 0.374mol of divinylbenzene is added to continue coupling. After the reaction is carried out for 60min, a mixture of 468g of terpene resin (accounting for 50wt% of the total amount) and 4212g of cyclohexane is pressed into the polymerization reactor, and the reaction is continued for 60min. After the reaction is completed, the reaction mixture after coupling is treated with water, 100g of water and 12g of antioxidant 1010 are added, and stirred. The glue solution is wet-coagulated and dried to obtain liquid styrene-butadiene rubber.
[0107] Comparative Example 4
[0108] The method of Example 4 is followed, except that the terpene resin is not modified, that is, the styrene-butadiene rubber segment and the terpene resin are directly coupled and then coagulated.
[0109] The specific preparation steps are as follows: In a 15L stainless steel reactor with a jacket, argon is passed through the system to replace 3 times. 4212g of cyclohexane, 234g of butadiene (accounting for 50wt% of the mixed monomer amount), 234g of styrene (accounting for 50wt% of the mixed monomer amount), 44.93g of tetrahydrofuran, and 0.624mol of n-butyl lithium are added to the polymerization reactor, the temperature is raised to 50°C, and the polymerization is carried out for 80min. After the monomer is completely converted, the temperature is raised to 80°C, and 0.249mol of divinylbenzene is added to continue coupling. After the reaction is 60min, a mixture of 468g of terpene resin (accounting for 50wt% of the total amount) and 4212g of cyclohexane is pressed into the polymerization reactor, and the reaction is continued for 60min. After the reaction is completed, the reaction mixture after coupling is treated with water, 100g of water and 12g of antioxidant 1010 are added, and stirred. The glue solution is wet-coagulated and dried to obtain liquid styrene-butadiene rubber.
[0110] Comparative Example 5
[0111] The method of Example 5 is followed, except that no coupling agent is added for coupling reaction, that is, after the polymerization reaction of butadiene and styrene is completed, the modified terpene resin is added and mixed.
[0112] The specific preparation steps are as follows: 1) Preparation of modified terpene resin: In a reaction kettle, add 2527g of cyclohexane and 187g of terpene resin (accounting for 70wt% of the modified terpene resin segment), heat to 80°C and stir until they are completely dissolved, then add 94g of dissolved sodium methylcellulose (accounting for 30wt% of the modified terpene resin segment), stir and mix evenly to obtain modified terpene resin. 2) In a 15L stainless steel reaction kettle with a jacket, replace the system 3 times with argon. Add 5897g of cyclohexane, 468g of butadiene (accounting for 70wt% of the mixed monomers), 187g of styrene (accounting for 30wt% of the mixed monomers), 37.73g of tetrahydrofuran, and then add 0.281mol of n-butyl lithium, heat to 50°C, polymerize for 80min, heat to 80°C after the monomers are completely converted, react for 60min, and then press the mixture of 281g of the prepared modified terpene resin (accounting for 30wt% of the total amount) and 2527g of cyclohexane into the polymerization kettle, add 100g of water and 12g of antioxidant 1010 after mixing for 20min, and stir. The rubber solution is wet coagulated and dried to obtain liquid styrene-butadiene rubber.
[0113] Comparative Example 6
[0114] The method of Example 6 is followed, except that no coupling agent is added for coupling reaction, that is, after the polymerization reaction of butadiene and styrene is completed, the modified terpene resin is added and mixed.
[0115] The specific preparation steps are as follows: 1) Preparation of modified terpene resin: In a reaction kettle, add 2527g of cyclohexane and 234g of terpene resin (accounting for 80wt% of the modified terpene resin segment), heat to 80°C and stir until they are completely dissolved, then add 47g of dissolved sodium methylcellulose (accounting for 20wt% of the modified terpene resin segment), stir and mix evenly to obtain modified terpene resin. 2) In a 15L stainless steel reactor with a jacket, replace the system 3 times with argon. Add 5897g of cyclohexane, 468g of butadiene (accounting for 70wt% of the mixed monomers), 187g of styrene (accounting for 30wt% of the mixed monomers), 23.58g of tetrahydrofuran, and then add 0.327mol of n-butyl lithium, heat to 50°C, polymerize for 80min, heat to 80°C after the monomers are completely converted, react for 60min, and then press the mixture of 281g of the prepared modified terpene resin (accounting for 30wt% of the total amount) and 2527g of cyclohexane into the polymerization kettle, add 100g of water and 12g of antioxidant 1010 after mixing for 20min, and stir. The rubber solution is wet coagulated and dried to obtain liquid styrene-butadiene rubber.
[0116] Comparative Example 7
[0117] The method of Example 7 is followed, except that the terpene resin is not modified, that is, the styrene-butadiene rubber segment and the terpene resin are directly coupled, and then dissolved sodium carboxymethyl cellulose is added and then coagulation is performed.
[0118] The specific preparation steps are as follows: In a 15L stainless steel reactor with a jacket, argon gas was passed through the system to replace it three times. In a polymerization kettle, 5897g of cyclohexane, 557g of butadiene ((accounting for 85wt% of the mixed monomer amount), 98g of styrene (accounting for 15wt% of the mixed monomer amount), 37.73g of tetrahydrofuran, 0.524mol of n-butyl lithium were added, the temperature was raised to 50°C, polymerization was carried out for 80min, the temperature was raised to 80°C after the monomers were fully converted, 0.212mol of divinylbenzene was added to continue coupling, and after the reaction for 60min, a mixture of 225g of terpene resin (accounting for 21wt% of the total amount) and 1685g of cyclohexane was added and pressed into a polymerization kettle, and the reaction was continued for 60min, and a mixture of 56g of dissolved sodium carboxymethyl cellulose (accounting for 9wt% of the total amount) and 842g of cyclohexane was added, and the reaction mixture after the coupling was treated with water after mixing for 20min, 100g of water and 12g of antioxidant 1010 were added, and stirred. The glue solution was coagulated and dried by a wet method to obtain liquid styrene-butadiene rubber.
[0119] Comparative Example 8
[0120] The method of Example 8 was followed, except that the terpene resin was not modified, that is, the styrene-butadiene rubber segment and the terpene resin were directly coupled, and then dissolved sodium carboxymethyl cellulose was added and then coagulated.
[0121] The specific preparation steps are as follows: In a 15L stainless steel reactor with a jacket, argon gas was passed through the system to replace it three times. Add 5897g of cyclohexane, 557g of butadiene (accounting for 85wt% of the mixed monomer amount), 98g of styrene (accounting for 15wt% of the mixed monomer amount), 53.90g of tetrahydrofuran, and then add 0.504mol of n-butyl lithium, heat to 50℃, polymerize for 80min, heat to 80℃ after the monomer is completely converted, add 0.301mol of divinylbenzene to continue coupling, react for 60min, then add 197g of terpene resin (accounting for 21wt% of the total amount) and 1685g of cyclohexane mixture to the polymerizer, continue to react for 60min, then add 84g of dissolved sodium carboxymethyl cellulose (accounting for 9wt% of the total amount) and 842g of cyclohexane mixture, mix for 20min, treat the reaction mixture after coupling with water, add 100g of water and 12g of antioxidant 1010, and stir. The glue is wet coagulated and dried to obtain liquid styrene-butadiene rubber.
[0122] Comparative Example 9
[0123] The method of Example 10 is followed, except that the terpene resin is not modified, that is, the styrene-butadiene rubber segment and the terpene resin are directly coupled, and then dissolved sodium carboxymethyl cellulose is added and then coagulation is performed.
[0124] The specific preparation steps are as follows: In a 15L stainless steel reactor with a jacket, argon gas was passed through the system to replace it three times. Add 5897g of cyclohexane, 468g of butadiene (accounting for 70wt% of the mixed monomer amount), 187g of styrene (accounting for 30wt% of the mixed monomer amount), 23.58g of tetrahydrofuran, and then add 0.262mol of n-butyl lithium, heat to 50℃, polymerize for 80min, heat to 80℃ after the monomer is completely converted, add 0.131mol of divinylbenzene to continue coupling, react for 60min, then add 225g of terpene resin (accounting for 24wt% of the total amount) and 2527g of cyclohexane mixture to the polymerization kettle, continue to react for 60min, then add 56g of dissolved sodium carboxymethyl cellulose (accounting for 6wt% of the total amount) and 842g of cyclohexane mixture, mix for 20min, treat the reaction mixture after coupling with water, add 100g of water and 12g of antioxidant 1010, and stir. The glue is wet coagulated and dried to obtain liquid styrene-butadiene rubber.
[0125] Relevant performance measurements were performed on the results of Examples 1-11 and Comparative Examples 1-9. The results are shown in Table 1, wherein the styrene content is based on the total modified liquid styrene-butadiene rubber.
[0126] Table 1
[0127]
[0128]
[0129] It can be seen from the results in Table 1 that in the synthesis process of the star-shaped grafted modified liquid styrene butadiene rubber of the present invention, a secondary feeding method (divided into butadiene-styrene copolymer segment monomer feeding and cellulose ether modified terpene resin segment feeding) is adopted to synthesize the star-shaped grafted modified liquid styrene butadiene rubber with mixed arms (such as polybutadiene styrene arms, modified terpene resin polymer arms). Due to the presence of the mixed arms, it is equivalent to chaining the polybutadiene-styrene rubber and the modified terpene resin together through the polymer segment core formed by the coupling agent, realizing the combination of different polymer molecular chains at the short-range structural level of the polymer chain, which can promote the coordinated optimization of various performances of the product and enable the modified rubber to have good compatibility, stability and adhesion.
[0130] The average bonding force refers to the average value of the peel strength between the adhesive and the substrate in the peeling test, which is usually expressed by the stress per unit area. It can be used to compare the adhesive adhesion properties of the liquid styrene-butadiene rubber of the embodiments and the comparative examples under different conditions. From the comparison between the embodiments 1-10 and the comparative examples 1-9, it can be seen that as the molecular weight and viscosity of the grafted modified rubber increase, the average bonding force of the grafted modified rubber increases, and the greater the functionality of the grafted modified rubber and the higher the degree of branching, the greater the average bonding force of the grafted modified rubber.
[0131] It can be seen from Examples 1-11 that as the molecular weight of the polymer increases, the viscosity of the polymer also gradually increases, and the average binding force of the modified rubber also gradually increases. As the functionality of the polymer increases, the average binding force of the modified rubber also gradually increases, and the adhesion performance of the grafted modified rubber is better. From the comparison between the examples and the corresponding comparative examples, it can be seen that the average binding force values of the examples are higher than those of the comparative examples, indicating that the adhesion performance of the comparative examples is not as good as the liquid styrene butadiene rubber samples in the examples. The functionality of the liquid styrene butadiene rubber in the examples is also higher. The greater the functionality, the greater the branching degree of the liquid styrene butadiene rubber and the greater the viscosity. The greater the viscosity, the better the adhesion performance of the liquid styrene butadiene rubber.
[0132] From the comparison between Examples 1-4 and Comparative Examples 1-4, it can be seen that after the terpene resin is modified, the viscosity and average bonding force of the grafted modified rubber are increased, indicating that the adhesion performance of the modified liquid styrene butadiene rubber in the examples is better than that in the comparative examples, indicating that the modified cellulose ether has a good bonding effect. The cellulose ether-modified terpene resin segment affects the average bonding force of the prepared rubber, and the rubber of the structure of the present invention has good bonding properties.
[0133] From the comparison between Example 5-6 and Comparative Example 5-6, it can be seen that after adding the coupling agent to couple the modified terpene resin, the modified liquid styrene butadiene rubber forms a mixed arm, so the viscosity, functionality and average binding force of the star-shaped modified liquid styrene butadiene rubber in Example 5-6 are greater than those in Comparative Example 5-6, indicating that the adhesion performance of the star-shaped modified liquid styrene butadiene rubber in Example 5-6 is better than that of the corresponding Comparative Example 5-6. Therefore, the coupling effect of the divinylbenzene coupling agent can chain the polybutadiene-styrene rubber and the modified terpene resin together, promote the synergistic optimization of various properties of the product, and enable the modified rubber to have good compatibility, stability and adhesion.
[0134] From the results in Table 1, it can be seen that, by comparing Example 1 with Example 3, and by comparing Example 2 with Example 4, under the same content of styrene and butadiene, the content of terpene resin in the cellulose ether modified terpene resin segment increases, the average binding force of the modified rubber prepared therefrom becomes larger, and the adhesion of the rubber is better.
[0135] The examples 1-11 using the star-shaped grafting modified liquid styrene butadiene rubber of the present invention have the effects of high viscosity, high branching degree, and significantly better adhesive compatibility. The greater the adhesive bonding force, the greater the viscosity, and the better the adhesiveness of the liquid styrene butadiene rubber. It shows that the modified liquid styrene butadiene rubber has the advantages of anti-slip properties, high temperature anti-flow properties, and good adhesive bonding force, and has broadened the scope of application.
[0136] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A star-shaped grafted modified liquid styrene-butadiene rubber, It is characterized in that The modified liquid styrene butadiene rubber comprises a polymer segment from a coupling agent and a plurality of butadiene-styrene copolymer segments and a cellulose ether modified terpene resin segment grafted on the polymer segment, wherein the coupling agent is selected from polyvinyl aromatic monomers.
2. The modified liquid styrene-butadiene rubber according to claim 1, It is characterized in that In the modified liquid styrene-butadiene rubber, based on the sum of the weights of the butadiene-styrene copolymer segment and the cellulose ether-modified terpene resin segment, the content of the cellulose ether-modified terpene resin segment is 20-80wt%, and the content of the butadiene-styrene copolymer segment is 20-80wt%; Preferably, in the butadiene-styrene copolymer segment, the content of the butadiene structural unit is 50-90wt%, and the content of the styrene structural unit is 10-50wt%; Preferably, in the cellulose ether-modified terpene resin segment, the content of the cellulose ether is 10-40wt%, and the content of the terpene resin is 60-90wt%; Preferably, the coupling agent is selected from divinylbenzene.
3. The modified liquid styrene-butadiene rubber according to claim 1 or 2, It is characterized in that The modified liquid styrene-butadiene rubber has a number average molecular weight of 3000-25000 g / mol, a viscosity of 20-60 Pa·S at 25° C., and a functionality of 4-7.
4. A method for preparing a star-shaped grafted modified liquid styrene-butadiene rubber, It is characterized in that The preparation method comprises: (1) in the presence of an initiator and a polar activator, copolymerizing butadiene and styrene to obtain an active butadiene-styrene copolymer segment; (2) subjecting the active butadiene-styrene copolymer segment to a coupling reaction with a coupling agent to obtain an active chain; (3) subjecting the active chain to polymerization reaction with a modified terpene resin to obtain the star-shaped grafted modified liquid styrene-butadiene rubber.
5. The preparation method according to claim 4, It is characterized in that The preparation method of the modified terpene resin comprises: mixing the terpene resin and a solvent, and then adding cellulose ether to obtain the modified terpene resin.
6. The preparation method according to claim 4 or 5, It is characterized in that The solvent is selected from one or more of pentane, hexane, octane, heptane, cyclohexane, benzene, toluene and ethylbenzene, preferably cyclohexane; Preferably, the polar activator is selected from one or more of diethylene glycol dimethyl ether, tetrahydrofuran, ethyl ether, ethyl methyl ether, anisole, diphenyl ether, ethylene glycol dimethyl ether, triethylamine, tetramethylethylenediamine and hexamethylphosphonic triamide, preferably selected from one or more of diethylene glycol dimethyl ether, tetrahydrofuran and tetramethylethylenediamine; Preferably, the initiator is selected from one or more of n-butyllithium, sec-butyllithium, methylbutyllithium, phenylbutyllithium, naphthalenelithium, cyclohexyllithium and dodecyllithium, preferably selected from n-butyllithium and / or sec-butyllithium; Preferably, the coupling agent is selected from polyvinyl aromatic hydrocarbons, preferably from divinyl benzene.
7. The preparation method according to any one of claims 4 to 6, It is characterized in that The copolymerization reaction temperature is 50-90°C, the copolymerization reaction pressure is 0.1-0.25MPa, and the copolymerization reaction time is 20-80min; Preferably, the coupling reaction temperature is 50-90°C, the coupling reaction pressure is 0.1-0.25MPa, and the coupling reaction time is 60-90min; Preferably, the polymerization reaction temperature is 50-90° C., the polymerization reaction pressure is 0.1-0.25 MPa, and the polymerization reaction time is 60-100 min.
8. The preparation method according to any one of claims 4 to 7, It is characterized in that The mixed monomer of butadiene and styrene is 20-80 parts by weight, wherein butadiene accounts for 60-90wt% of the mixed monomer, and styrene accounts for 10-40wt% of the mixed monomer; preferably, the mixed monomer of butadiene and styrene is 30-70 parts by weight, wherein butadiene accounts for 70-90wt% of the mixed monomer, and styrene accounts for 10-30wt% of the mixed monomer; Preferably, the modified terpene resin is 20-80 parts by weight, wherein the cellulose ether accounts for 10-40wt% of the modified terpene resin, and the terpene resin accounts for 60-90wt% of the modified terpene resin; preferably, the modified terpene resin is 30-70 parts by weight, wherein the cellulose ether accounts for 10-30wt% of the modified terpene resin, and the terpene resin accounts for 70-90wt% of the modified terpene resin; Preferably, the initiator is 0.02-0.2 parts by weight, preferably 0.025-0.1 parts by weight; Preferably, the molar ratio of the polar activator to the initiator is 0.1-30:1, preferably 0.1-20:1; Preferably, the molar ratio of the coupling agent to the initiator is 0.1-1.5:1, preferably 0.1-1:
1.
9. The star-shaped grafted modified liquid styrene-butadiene rubber obtained by the preparation method described in any one of claims 4 to 8.
10. Use of the star-shaped grafted modified liquid styrene butadiene rubber described in any one of claims 1 to 3 and the star-shaped grafted modified liquid styrene butadiene rubber obtained by the preparation method described in any one of claims 4 to 8 in the field of rubber processing.
Citation Information
Patent Citations
Method for synthesizing star amphiphilic rubber
CN101062964A
Preparation method of high-performance liquid styrene butadiene rubber
CN103539949A
Hot-melt adhesive agent