Barrier film and preparation method and application thereof

By using inductively coupled plasma enhanced chemical vapor deposition technology in flexible thin films to deposit silicon oxide films and coat them with organic layers, the problem of insufficient water vapor barrier rate and light transmittance in the prior art is solved. A combination of efficient and low-cost barrier performance and good optical performance is achieved.

CN119019727APending Publication Date: 2024-11-26CHINA ENERGY INVESTMENT CORP LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310592528.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to achieve a barrier film with high barrier performance and good optical performance in flexible thin-film solar cells. The existing barrier film has insufficient water vapor barrier rate and light transmittance, and the complex multi-layer structure leads to high cost and low efficiency.

Method used

Using inductively coupled plasma enhanced chemical vapor deposition technology to deposit silicon oxide film as a barrier layer on the surface of polymer substrate, and coating polydimethylsiloxane or organosilazane film as an organic layer on its outer surface, forming a simple form single-layer or double-layer structural barrier film.

Benefits of technology

A barrier film with a water vapor transmission rate of less than 5×10-4 g/(m2·day) and a light transmission rate of more than 90% is achieved, which simplifies the structure, reduces costs and improves efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004246007350000081
    Figure BDA0004246007350000081
  • Figure BDA0004246007350000091
    Figure BDA0004246007350000091
  • Figure BDA0004246007350000092
    Figure BDA0004246007350000092
Patent Text Reader

Abstract

The invention provides a barrier film and a preparation method and application thereof, and belongs to the technical field of materials. The barrier film comprises a base layer, a barrier layer arranged on the surface of one side or two sides of the base layer, and an organic layer arranged on the outer surface of the barrier layer on at least one side, wherein the base layer is one or more of a polyethylene naphthalate film, a polyethylene terephthalate film and a polycarbonate film, the barrier layer is a silicon oxide film, and the organic layer is one or two of a polydimethylsiloxane film and an organic silazane film. The inductively coupled plasma enhanced chemical vapor deposition technology is adopted, the silicon oxide thin film is deposited on the surface of one side or two sides of the base layer to serve as the barrier layer, and the obtained silicon oxide thin film is smooth in surface, good in uniformity and good in compactness; the barrier film provided by the invention has excellent barrier property and high light transmittance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of materials, and in particular relates to a barrier film and a preparation method and application thereof. Background Art

[0002] Flexible electronic devices usually use polymer materials to replace glass and metal, but due to the inherent porosity of polymers, the water vapor transmission rate is usually greater than 1g / (m 2 .day), which is not suitable for providing adequate protection for devices. Therefore, thin film encapsulation technology has developed rapidly in recent years. For flexible thin film solar cells, barrier films are usually used to encapsulate the devices to reduce the erosion of external water and oxygen and increase the service life of the devices.

[0003] Breakthroughs in thin film encapsulation technology are the key to the current development of the flexible industry. The permeability of a polymer substrate can be effectively reduced by coating it with a substantially impermeable inorganic layer through an appropriate vacuum deposition process. This inorganic layer is usually a transparent oxide, nitride or carbide, which is impermeable to moisture and oxygen when it is defect-free. However, defects are difficult to avoid, including defects during the deposition process (inherent defects) and impurities in the vacuum chamber and on the surface of the substrate (external defects). Therefore, it is crucial to reduce defects, improve film density, and obtain high-quality deposited films. In addition, while improving barrier properties, it is also necessary to maintain a high transmittance to sunlight as a barrier film for encapsulation.

[0004] In the prior art, barrier films mostly adopt a multi-layer structure, including "inorganic / organic" and "inorganic / inorganic" multi-layer stacking routes. For example, Chinese patent application CN111574715A discloses a composition, a packaging film containing it, a preparation method and an electronic device, and specifically proposes a composition with an organic silane resin as the main material, and uses it as an organic layer to form a multi-layer barrier stack packaging film with an inorganic layer. Among them, the inorganic layer is a 100nm thick silicon oxide film deposited on a PET substrate using traditional PECVD, and the water permeability is 0.04g / (m 2 .day), only negative two levels, indicating that the density of the silicon oxide layer is poor. For another example, Chinese patent application CN105405986A proposes a water vapor barrier film, a preparation method thereof and a display comprising the same, specifically a water vapor barrier film with a barrier layer formed by silicon oxide and aluminum oxide. The barrier film has good optical properties, but the barrier performance is not high, and the water vapor barrier rate is only 10 -3 g / (m 2 .day) level.

[0005] In view of this, preparing a barrier film with both high barrier properties and good optical properties remains a difficult problem to be solved urgently in the current industry. Summary of the invention

[0006] In order to solve the above problems existing in the prior art, the present invention provides a barrier film and a preparation method and application thereof. The barrier film has good water and oxygen barrier properties and light transmittance, and when applied to the packaging of flexible thin-film solar cells, it can effectively improve the service life of the device.

[0007] An object of the present invention is to provide a barrier film.

[0008] The barrier film comprises a base layer, a barrier layer disposed on one or both sides of the base layer, and an organic layer disposed on at least one outer surface of the barrier layer;

[0009] The base layer is one or more of polyethylene naphthalate film, polyethylene terephthalate film and polycarbonate film, the barrier layer is silicon oxide film, and the organic layer is one or both of polydimethylsiloxane film and organosilazane film.

[0010] In some embodiments, the density of the silicon oxide film is 2.7-3.0 g / cm 3 The surface roughness is between 2.5 nm and 2.5%, the unevenness is between 2.5%, the refractive index is between 1.47 and 1.52, and the thickness is between 100 and 500 nm. In some preferred embodiments, the thickness of the silicon oxide film is between 150 and 400 nm.

[0011] The inventors have found that if the thickness of the silicon oxide film is less than 100 μm, the barrier properties will be affected; if the thickness of the silicon oxide film is greater than 500 μm, cracks are likely to occur due to the through-growth of defects in the inorganic film, which will also cause a decrease in the barrier properties.

[0012] In some embodiments, the thickness of the base layer is 50-150 μm, and the light transmittance is greater than 80%; in some preferred embodiments, the thickness of the base layer is 80-130 μm, and the light transmittance is greater than 85%.

[0013] The inventors have found that if the thickness of the base polymer film is less than 50 μm, the mechanical strength will be low, which is not conducive to the subsequent coating on the base; if the thickness of the base polymer film is greater than 150 μm, the transmittance will decrease and the flexibility will also deteriorate.

[0014] In some embodiments, the thickness of the organic layer is 2-15 μm, and in some preferred embodiments, the thickness of the organic layer is 5-10 μm.

[0015] The inventors have found that if the thickness of the organic layer is less than 2 μm, the protective effect on the inorganic layer is weakened, and the degree of improvement in the final light transmittance of the barrier film is limited; if the thickness of the organic layer is greater than 15 μm, it is not conducive to interface adhesion.

[0016] In some embodiments, the water vapor transmission rate of the barrier film is less than 5×10 -4 g / (m 2 ·day).

[0017] In some embodiments, the light transmittance of the barrier film is >90%.

[0018] Another object of the present invention is to provide a method for preparing any of the above barrier films.

[0019] The preparation method comprises the following steps:

[0020] S1. Using inductively coupled plasma enhanced chemical vapor deposition technology, a silicon oxide film is deposited on one or both sides of the substrate as a barrier layer;

[0021] S2. Coating an organic layer on the outer surface of at least one side of the barrier layer by a coating process, and then performing a curing treatment to obtain the barrier film.

[0022] In some embodiments, in step S1, the deposition temperature of the inductively coupled plasma enhanced chemical vapor deposition technology is 70-140°C, and the radio frequency power is 250-650w; in some preferred embodiments, the deposition temperature of the inductively coupled plasma enhanced chemical vapor deposition technology is 80-120°C, and the radio frequency power is 300-500w.

[0023] The inventors have found that when using inductively coupled plasma enhanced chemical vapor deposition (ICPECVD) technology to deposit silicon oxide thin films at low temperature on one or both sides of the base layer, the selection of two key process parameters, radio frequency power and deposition temperature, directly affects the film quality of the silicon oxide thin film. In view of the particularity of the base polymer substrate, it is necessary to balance the relationship between the densification of the silicon oxide thin film and the non-deformation of the substrate to achieve better performance of the barrier film. If the radio frequency power and deposition temperature are continuously increased in order to improve the densification of the silicon oxide thin film, after exceeding the tolerance conditions of the polymer substrate, the substrate will cause curling, and the performance of the barrier film will eventually decrease.

[0024] In some embodiments, in step S2, the coating process is selected from one or both of blade coating and spin coating; the curing temperature is 50-80°C and the time is 2-6h; in some preferred embodiments, the curing temperature is 60-70°C and the time is 3-5h.

[0025] Another object of the present invention is to provide application of any of the above barrier films and barrier films prepared by any of the above barrier film preparation methods in the field of flexible thin-film solar cell packaging.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1) Compared with conventional chemically deposited silicon oxide films, the present invention uses inductively coupled plasma enhanced chemical vapor deposition technology to deposit a silicon oxide film as a barrier layer on one or both sides of the base layer, and the obtained silicon oxide film has a smooth surface, good uniformity and good density;

[0028] 2) The barrier film of the present invention only needs one inorganic barrier layer and one organic layer to achieve a good barrier effect, and has a relatively simple structure, low cost and high efficiency;

[0029] 3) The barrier film of the present invention has excellent barrier properties (water vapor transmission rate <5×10 -4 g / (m 2 ·day) and high light transmittance (>90%). DETAILED DESCRIPTION

[0030] The technical solution of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] The experimental methods without specific conditions in the examples are usually carried out according to conventional conditions and conditions described in the manual, or according to conditions recommended by the manufacturer. The general equipment, materials, reagents, etc. used are all available from commercial channels unless otherwise specified.

[0032] The water vapor transmission rate was measured according to the GB / T 21529-2008 method (testing instrument: AQUATRAN model 3 moisture permeability tester produced by MOCON Company, USA); the light transmittance was measured according to the ASTM D1003-13 method.

[0033] Substrate A: Polyethylene naphthalate (PEN) film (trade name: DuPont Teijin teonex Q65HA), thickness 125 μm, commercially available; water vapor transmission rate 1.7 g / (m 2 ·day), light transmittance 87.3%.

[0034] Substrate B: polyethylene naphthalate (PEN) film (trade name: DuPont Teijin teonex Q65HA), thickness 100 μm, commercially available; water vapor transmission rate 1.63 g / (m 2 ·day), light transmittance 87.5%.

[0035] Substrate C: Polyethylene terephthalate film (PET) film (trade name: Toray U483, Japan), thickness 125 μm, commercially available; water vapor transmission rate 5.06 g / (m 2 ·day), light transmittance 89.5%.

[0036] Substrate D: polycarbonate (PC) film (trade name: SABIC LEXANTM 8010MC), thickness 100 μm, commercially available; water vapor transmission rate 65.9 g / (m 2 ·day), light transmittance 90.1%.

[0037] Polydimethylsiloxane (PDMS184) and organopolysilazane (1500 rc) were both commercially available.

[0038] The inductively coupled plasma enhanced chemical vapor deposition equipment was purchased from SENTECH, Germany, model SI500D.

[0039] Example 1

[0040] The method for preparing a barrier film comprises the following steps:

[0041] S1. Using inductively coupled plasma enhanced chemical vapor deposition (ICPECVD) technology, SiH4 and O2 are used as reaction gases to deposit a 200nm thick silicon oxide film as a barrier layer on the single side surface of substrate A, with a deposition temperature of 120°C and a radio frequency power of 500w;

[0042] S2. A 6 μm thick polydimethylsiloxane film is coated on the outer surface of the barrier layer as an organic layer by a doctor blade coating process, and then a curing treatment is performed at a temperature of 70° C. for 3 hours to obtain a barrier film.

[0043] The process parameters of deposition and curing treatment as well as the film thickness and materials are shown in Table 1.

[0044] Example 2

[0045] The method for preparing a barrier film comprises the following steps:

[0046] S1. Using inductively coupled plasma enhanced chemical vapor deposition (ICPECVD) technology, SiH4 and O2 are used as reaction gases to deposit a 200nm thick silicon oxide film as a barrier layer on the single side surface of substrate A, with a deposition temperature of 80°C and a radio frequency power of 500w;

[0047] S2. A 6 μm thick polydimethylsiloxane film is coated on the outer surface of the barrier layer as an organic layer by a doctor blade coating process, and then a curing treatment is performed at a temperature of 70° C. for 3 hours to obtain a barrier film.

[0048] The process parameters of deposition and curing treatment as well as the film thickness and materials are shown in Table 1.

[0049] Example 3

[0050] The method for preparing a barrier film comprises the following steps:

[0051] S1. Using inductively coupled plasma enhanced chemical vapor deposition (ICPECVD) technology, SiH4 and O2 are used as reaction gases to deposit a 200nm thick silicon oxide film as a barrier layer on the single side surface of substrate A, with a deposition temperature of 120°C and a radio frequency power of 250w;

[0052] S2. A 6 μm thick polydimethylsiloxane film is coated on the outer surface of the barrier layer as an organic layer by a doctor blade coating process, and then a curing treatment is performed at a temperature of 70° C. for 3 hours to obtain a barrier film.

[0053] The process parameters of deposition and curing treatment as well as the film thickness and materials are shown in Table 1.

[0054] Example 4

[0055] The method for preparing a barrier film comprises the following steps:

[0056] S1. Using inductively coupled plasma enhanced chemical vapor deposition (ICPECVD) technology, SiH4 and O2 are used as reaction gases to deposit a 400nm thick silicon oxide film as a barrier layer on the single side surface of substrate A, with a deposition temperature of 120°C and a radio frequency power of 500w;

[0057] S2. A 6 μm thick polydimethylsiloxane film is coated on the outer surface of the barrier layer as an organic layer by a doctor blade coating process, and then a curing treatment is performed at a temperature of 70° C. for 3 hours to obtain a barrier film.

[0058] The process parameters of deposition and curing treatment as well as the film thickness and materials are shown in Table 1.

[0059] Example 5

[0060] The method for preparing a barrier film comprises the following steps:

[0061] S1. Using inductively coupled plasma enhanced chemical vapor deposition (ICPECVD) technology, SiH4 and O2 are used as reaction gases to deposit a 200nm thick silicon oxide film as a barrier layer on the single side surface of substrate A, with a deposition temperature of 120°C and a radio frequency power of 500w;

[0062] S2. A 10 μm thick polydimethylsiloxane film is coated on the outer surface of the barrier layer as an organic layer by a doctor blade coating process, and then cured at 70° C. for 3 h to obtain a barrier film.

[0063] The process parameters of deposition and curing treatment as well as the film thickness and materials are shown in Table 1.

[0064] Example 6

[0065] The method for preparing a barrier film comprises the following steps:

[0066] S1. Using inductively coupled plasma enhanced chemical vapor deposition (ICPECVD) technology, SiH4 and O2 were used as reaction gases to deposit a 200nm thick silicon oxide film as a barrier layer on both sides of substrate A, with a deposition temperature of 120°C and a radio frequency power of 500w;

[0067] S2. A 6 μm thick polydimethylsiloxane film is coated on the outer surface of the barrier layer (on both sides) as an organic layer by a doctor blade coating process, and then cured at 70° C. for 3 h to obtain a barrier film.

[0068] The process parameters of deposition and curing treatment as well as the film thickness and materials are shown in Table 1.

[0069] Example 7

[0070] The method for preparing a barrier film comprises the following steps:

[0071] S1. Using inductively coupled plasma enhanced chemical vapor deposition (ICPECVD) technology, SiH4 and O2 are used as reaction gases to deposit a 200nm thick silicon oxide film as a barrier layer on the single side surface of substrate B, with a deposition temperature of 120°C and a radio frequency power of 500w;

[0072] S2. A 6 μm thick polydimethylsiloxane film is coated on the outer surface of the barrier layer as an organic layer by a doctor blade coating process, and then a curing treatment is performed at a temperature of 70° C. for 3 hours to obtain a barrier film.

[0073] The process parameters of deposition and curing treatment as well as the film thickness and materials are shown in Table 1.

[0074] Example 8

[0075] The method for preparing a barrier film comprises the following steps:

[0076] S1. Using inductively coupled plasma enhanced chemical vapor deposition (ICPECVD) technology, SiH4 and O2 are used as reaction gases to deposit a 200nm thick silicon oxide film as a barrier layer on the single side surface of substrate D, with a deposition temperature of 120°C and a radio frequency power of 500w;

[0077] S2. A 6 μm thick polydimethylsiloxane film is coated on the outer surface of the barrier layer as an organic layer by a doctor blade coating process, and then a curing treatment is performed at a temperature of 70° C. for 3 hours to obtain a barrier film.

[0078] The process parameters of deposition and curing treatment as well as the film thickness and materials are shown in Table 1.

[0079] Example 9

[0080] The method for preparing a barrier film comprises the following steps:

[0081] S1. Using inductively coupled plasma enhanced chemical vapor deposition (ICPECVD) technology, SiH4 and O2 are used as reaction gases to deposit a 200nm thick silicon oxide film as a barrier layer on the single side surface of substrate C, with a deposition temperature of 80°C and a radio frequency power of 300w;

[0082] S2. A 6 μm thick polydimethylsiloxane film is coated on the outer surface of the barrier layer as an organic layer by a doctor blade coating process, and then a curing treatment is performed at a temperature of 70° C. for 3 hours to obtain a barrier film.

[0083] The process parameters of deposition and curing treatment as well as the film thickness and materials are shown in Table 1.

[0084] Example 10

[0085] The method for preparing a barrier film comprises the following steps:

[0086] S1. Using inductively coupled plasma enhanced chemical vapor deposition (ICPECVD) technology, SiH4 and O2 are used as reaction gases to deposit a 200nm thick silicon oxide film as a barrier layer on the single side surface of substrate A, with a deposition temperature of 120°C and a radio frequency power of 500w;

[0087] S2. A 6 μm thick organic polysilazane film is coated on the outer surface of the barrier layer as an organic layer by a doctor blade coating process, and then a curing treatment is performed at a temperature of 70° C. for 3 hours to obtain a barrier film.

[0088] The process parameters of deposition and curing treatment as well as the film thickness and materials are shown in Table 1.

[0089] Comparative Example 1

[0090] The preparation method of the barrier film is basically the same as that of Example 1, except that the deposition temperature is 60°C.

[0091] Comparative Example 2

[0092] The preparation method of the barrier film is basically the same as that of Example 1, except that the deposition temperature is 150°C.

[0093] Comparative Example 3

[0094] The preparation method of the barrier film is basically the same as that of Example 1, except that the thickness of the silicon oxide film is 50 nm.

[0095] Comparative Example 4

[0096] The preparation method of the barrier film is basically the same as that of Example 1, except that the thickness of the organic layer is 0 μm.

[0097] Comparative Example 5

[0098] The preparation method of the barrier film is basically the same as that of Example 1, except that a 200 nm thick silicon oxide film is deposited on a single side surface of the substrate A by plasma enhanced chemical vapor deposition (PECVD) technology as a barrier layer.

[0099] Table 1 Deposition and curing process parameters and film thickness and materials

[0100]

[0101]

[0102] Performance test

[0103] The film thickness non-uniformity, refractive index, density and surface roughness of the silicon oxide thin films in the barrier films prepared in Examples 1-10 and Comparative Examples 1-5 were tested. The water vapor permeability and light transmittance of the barrier films were also tested. The results are shown in Table 2.

[0104] After the silicon oxide film is deposited on the base layer, the performance test of the silicon oxide film is carried out. The prepared sample is divided into 9 regions by using an ellipsometer, and then the thickness of the silicon oxide film in each region is measured and the values ​​are recorded.

[0105] Unevenness = (maximum thickness - minimum thickness) / average thickness.

[0106] The refractive index is tested using an ellipsometer; the density is tested using X-ray reflectometry (XRR); the surface roughness is tested using an atomic force microscope (AFM); the above test methods are conventional methods in the art and will not be described in detail.

[0107] Table 2 Performance test results

[0108]

[0109]

[0110] From the results in Table 2, it can be seen that the surface of the low-temperature deposited silicon oxide film suitable for polymer substrates provided by the present invention in Examples 1-10 is flat, uniform and compact, and the barrier film obtained thereby has excellent water-blocking performance and light transmittance. Comparing the results of Example 1 and Comparative Examples 1 and 2, it can be seen that the barrier film obtained by preparing the silicon oxide film at a deposition temperature within a specific range (70-140°C) has better performance. If the temperature is too low, the compactness of the silicon oxide film is poor, and the barrier film obtained has poor performance; if the temperature is too high, although the compactness of the silicon oxide film is improved to a certain extent, the substrate curls, resulting in poor performance of the barrier film. In Comparative Example 3, the thickness of the silicon oxide film is small, and the barrier performance of the barrier film obtained is poor; in Comparative Example 4, no organic layer is provided, and the light transmittance of the barrier film obtained is poor; in Comparative Example 5, the silicon oxide film is deposited by conventional plasma enhanced chemical vapor deposition (PECVD) technology, and the barrier performance of the barrier film obtained is poor.

[0111] In summary, the present invention adopts inductively coupled plasma enhanced chemical vapor deposition technology to deposit a silicon oxide film on one or both sides of the substrate as a barrier layer. The obtained silicon oxide film has a smooth surface, good uniformity and good density, and the obtained barrier film has excellent barrier properties (water vapor transmission rate <5×10 -4 g / (m 2 ·day) and high light transmittance (>90%).

[0112] The above embodiments are only specific implementation methods of the present invention, which are used to illustrate the technical solutions of the present invention rather than to limit them. The protection scope of the present invention is not limited thereto. Although the present invention has been described in detail with reference to the aforementioned embodiments, ordinary technicians in the field should understand that any technician familiar with the technical field can still modify the technical solutions recorded in the aforementioned embodiments within the technical scope disclosed by the present invention, or can easily think of changes, or make equivalent replacements for some of the technical features therein; and these modifications, changes or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention, and should all be covered within the protection scope of the present invention.

Claims

1. A barrier film, characterized in that: It comprises a base layer, a barrier layer arranged on one or both sides of the base layer, and an organic layer arranged on the outer surface of at least one side of the barrier layer; The base layer is one or more of polyethylene naphthalate film, polyethylene terephthalate film and polycarbonate film, the barrier layer is silicon oxide film, and the organic layer is one or both of polydimethylsiloxane film and organosilazane film.

2. The barrier film according to claim 1, characterized in that The density of the silicon oxide film is 2.7-3.0 g / cm 3 The surface roughness is between 2.5 nm and 2.5%, the unevenness is between 2.5%, the refractive index is between 1.47 and 1.52, and the thickness is between 100 and 500 nm, preferably 150 and 400 nm.

3. The barrier film according to claim 1, characterized in that The thickness of the base layer is 50-150 μm, and the light transmittance is greater than 80%; preferably, the thickness of the base layer is 80-130 μm, and the light transmittance is greater than 85%.

4. The barrier film according to claim 1, characterized in that The thickness of the organic layer is 2-15 μm, preferably 5-10 μm.

5. The barrier film according to any one of claims 1 to 4, characterized in that: The water vapor transmission rate of the barrier film is less than 5×10 -4 g / (m 2 ·day).

6. The barrier film according to any one of claims 1 to 4, characterized in that: The light transmittance of the barrier film is greater than 90%.

7. The method for preparing a barrier film according to any one of claims 1 to 6, characterized in that: The steps include: S1. Using inductively coupled plasma enhanced chemical vapor deposition technology, a silicon oxide film is deposited on one or both sides of the substrate as a barrier layer; S2. Coating an organic layer on the outer surface of at least one side of the barrier layer by a coating process, and then performing a curing treatment to obtain the barrier film.

8. The method for preparing a barrier film according to claim 7, characterized in that: In step S1, the deposition temperature of the inductively coupled plasma enhanced chemical vapor deposition technology is 70-140°C, and the radio frequency power is 250-650W; preferably, the deposition temperature of the inductively coupled plasma enhanced chemical vapor deposition technology is 80-120°C, and the radio frequency power is 300-500W.

9. The method for preparing a barrier film according to claim 7, characterized in that: In step S2, the coating process is selected from one or both of blade coating and spin coating; the curing temperature is 50-80°C and the time is 2-6h; preferably, the curing temperature is 60-70°C and the time is 3-5h.