Mining PVC (polyvinyl chloride) whole-core flame-retardant conveyor belt covering rubber composition, covering rubber, preparation method of covering rubber and conveyor belt
By using environmentally friendly materials such as polyvinyl chloride SG-3 resin, chlorinated palm oil methyl ester, triisopropyl phosphate and epoxy soybean oil, an efficient flame retardant system is formed, and PVC is solved in the prior art mining in the existing technology The environmental protection and insufficient flame retardant performance of core flame retardant conveyor belt cover glue have achieved improvements in environmental protection, plasticization and thermal stability.
Patent Information
- Application Number
- CN202411354445.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-26
AI Technical Summary
The existing mineral PVC whole-core flame-retardant conveyor belt cover glue is difficult to meet the increasingly stringent environmental protection requirements at home and abroad. At the same time, its flame retardant performance is insufficient and it cannot effectively replace traditional harmful additives.
Adopt environmentally friendly raw materials such as polyvinyl chloride SG-3 resin, chlorinated palm oil methyl ester, triisopropyl phosphate, epoxy soybean oil and rare earth composite stabilizers to achieve plasticization, flame retardant and thermal stability through formulation design Synergistic effect replaces traditional phthalates, paraffin chloride and tris(2-chloroethyl) phosphate to form an efficient flame retardant system.
It has achieved improvements in environmental protection, plasticization and flame retardant performance, met strict environmental protection standards, and at the same time reduced production costs and improved the physical and safety performance of the products.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of new materials, in particular to a covering rubber composition for a mining PVC whole-core flame-retardant conveyor belt, a covering rubber and a preparation method thereof, and a conveyor belt. Background Art
[0002] At present, the world economic growth is slowing down, the downward pressure on the domestic economy is increasing, the prices of raw materials and energy are fluctuating at a high level, and the pressure on environmental protection is increasing. The conveyor belt industry has always been suffering from serious homogeneity, overcapacity and low-price competition. The rising prices of raw materials, energy and labor costs have led to a continuous decline in the profitability of enterprises and a serious squeeze on profit margins. This unsustainable development trend runs counter to the requirements of high-quality development at this stage and should be taken seriously by the industry.
[0003] In order to improve the profitability of enterprises, first, to achieve the "dual carbon" goal in my country's economic development, the whole industry should work together to accelerate the low-carbon transformation, conform to the general trend of scientific and technological revolution and industrial transformation, adhere to the principles of innovation, coordination, green, openness and sharing, and find opportunities from green development; second, it is necessary to increase the export of conveyor belt products, expand the international market share, actively layout mid-to-high-end products from a long-term perspective, accelerate the export of high-end products, strive to change from "winning by quantity" to "winning by quality", occupy a favorable position for enterprise development, and establish a high-quality brand image. Therefore, conveyor belt companies should focus on the bottleneck of green development and promote the low-carbon development of the industry with technological innovation. Break through the key technical bottleneck of green materials and strengthen the development of environmentally friendly conveyor belt products.
[0004] Under the green and sustainable trend, countries are increasingly stringent in controlling chemicals, which directly affects companies’ cross-border trade and product life cycles. Therefore, how to avoid “regrettable substitutions” and establish a green supply chain is a huge challenge facing the entire manufacturing industry.
[0005] At present, the plasticizers used in the PVC covering rubber of domestic PVC whole core conveyor belts are mostly phthalates and chlorinated paraffins, the flame retardants are mostly tris(2-chloroethyl) phosphate, and the heat stabilizers are mostly lead salts such as di-salt and tri-salt. In recent years, my country's requirements for environmental protection have become increasingly stringent. At the same time, the EU's REACH regulations and the US's environmental protection policies have extremely strict restrictions and controls on phthalates, chlorinated paraffins, tris(2-chloroethyl) phosphate and lead salts. Therefore, domestic conveyor belt companies should self-check the harmful additive components in PVC conveyor belt products and supply chains in order to find green alternatives in time and adjust the industrial layout in advance. This requires the development and design of a mining environmentally friendly PVC whole core flame retardant conveyor belt covering rubber that can meet the increasingly stringent environmental protection requirements at home and abroad. At the same time, the covering rubber also needs to meet the requirements of flame retardant performance of mining PVC whole core flame retardant conveyor belts, and the prior art has not yet found a mining PVC whole core flame retardant conveyor belt covering rubber that can meet environmental protection requirements and have excellent flame retardant performance. Summary of the invention
[0006] In view of this, the technical problem to be solved by the present invention is to provide a mining PVC whole-core flame-retardant conveyor belt covering rubber composition, covering rubber and its preparation method and conveyor belt. The covering rubber provided by the present invention is not only environmentally friendly, but also has high plasticizing effect and thermal stability, and excellent flame retardant performance.
[0007] The present invention provides a mining PVC whole core flame retardant conveyor belt covering rubber composition, which comprises, by weight:
[0008] 100 parts of polyvinyl chloride SG-3 resin;
[0009] 25-55 parts of chloropalm oil methyl ester;
[0010] 15-30 parts of triisopropylphenyl phosphate;
[0011] Epoxidized soybean oil 4-10 parts;
[0012] 3-6 parts of antimony trioxide;
[0013] 5~7 parts of rare earth composite stabilizer.
[0014] Preferably, in parts by weight, it comprises:
[0015] 100 parts of polyvinyl chloride SG-3 resin;
[0016] 40-50 parts of chloropalm oil methyl ester;
[0017] 20-30 parts of triisopropylphenyl phosphate;
[0018] Epoxidized soybean oil 8-10 parts;
[0019] 3-6 parts of antimony trioxide;
[0020] 5~7 parts of rare earth composite stabilizer.
[0021] The mining PVC whole-core flame-retardant conveyor belt covering rubber composition of the present invention develops and uses environmentally friendly raw materials to replace harmful chemical raw materials in the original product in a green way. At the same time, the raw materials selected for replacement can achieve functional synergy through formula design, thereby preparing the environmentally friendly PVC whole-core conveyor belt covering rubber.
[0022] The mining PVC whole-core flame-retardant conveyor belt covering rubber composition of the present invention uses polyvinyl chloride SG-3 resin as the main material. The SG-3 resin is a general suspension resin with good comprehensive performance, high mechanical properties, electrical insulation performance, low water absorption, low air permeability, and resistance to corrosion by general chemicals. At the same time, it is a loose resin with good processing performance, high oil absorption, easy plasticization, good dry fluidity, easy measurement, simple processing technology, and excellent product performance, and is suitable for extrusion molding.
[0023] The mining PVC whole core flame retardant conveyor belt covering rubber composition of the present invention uses chloropalm oil methyl ester, triisopropylphenyl phosphate and epoxy soybean oil as the plasticizing system, wherein chloropalm oil methyl ester is used as the main plasticizer, and epoxy soybean oil and triisopropylphenyl phosphate are used as auxiliary plasticizers. In particular, chloropalm oil methyl ester belongs to synthetic plant ester, the raw material comes from natural oils and fats, does not contain harmful metals and phthalates, and has passed the European SGS (RoHS, PAHs, REACH regulations) certification; the raw material of epoxy soybean oil comes from natural oils and fats, which complies with the US PDA food additive regulations. Both are environmentally friendly plasticizers, and at the same time, they are low in price and have excellent product performance. Under the condition of reasonable formula design, the production cost of the enterprise can be greatly reduced while ensuring product quality. The combination of chloropalm oil methyl ester, triisopropyl phosphate and epoxidized soybean oil replaces the phthalate plasticizers and auxiliary plasticizers chlorinated paraffin and tri(2-chloroethyl) phosphate in the conventional plasticizing system, weakening the secondary bonds between PVC polymer molecules, namely the van der Waals force, thereby increasing the mobility of the PVC polymer molecular chain and reducing the crystallinity of the PVC polymer molecular chain, that is, increasing the plasticity of the PVC polymer, which is mainly manifested in the decrease of the hardness, modulus, conversion temperature and brittle temperature of the PVC polymer, and the improvement of elongation, flexibility and toughness.
[0024] The mining PVC whole core flame retardant conveyor belt covering rubber composition of the present invention uses triisopropylphenyl phosphate as a flame retardant, and antimony trioxide and chloro-substituted palm oil methyl ester in the plasticizer system are compounded to achieve chlorine-antimony synergistic flame retardancy, which together constitute the flame retardant system of the composition formula. The flame retardant system of the present invention replaces tri(2-chloroethyl) phosphate with triisopropylphenyl phosphate, which has a high phosphorus content as a phosphorus-based flame retardant. During the combustion process, it mainly generates phosphoric acid and metaphosphoric acid and dehydrates the polymer into carbon, or forms a non-combustible glassy substance to cover the surface of the material to isolate oxygen and combustible gases, reduce the heat feedback of the flame, and thus reduce the degree of degradation reaction of the substrate to achieve flame retardancy; and triisopropylphenyl phosphate has very low toxicity, is basically close to non-toxic, and is biodegradable, which is beneficial to protecting the environment and the health of users. When methyl chlorinated palm oil and antimony trioxide are compounded, in addition to the gas phase flame retardant effect of chlorine itself, antimony oxychloride generated by the reaction of hydrogen chloride and antimony oxide during the combustion process can be decomposed into antimony trichloride in a three-step endothermic reaction within a wide temperature range. Both antimony chloride and hydrogen chloride are high-density flame-retardant gases, which can not only dilute the oxygen in the air, but also cover the surface of the material, isolate the air, and reduce the burning rate of the material or make it self-extinguishing. In addition, antimony trichloride can promote the carbonization reaction of the condensed phase. The carbon layer can cover the surface of the substrate, which can reduce the thermal radiation and heat conduction of the flame to the substrate, slow down the thermal decomposition of the polymer, reduce the generation and escape of gas-phase combustible substances into the flame zone, and reduce the intensity of combustion.
[0025] The PVC whole core flame retardant conveyor belt covering rubber composition for mining of the present invention replaces the lead salt stabilizer with a rare earth composite stabilizer, and the rare earth composite stabilizer is a new type of non-toxic heat stabilizer for PVC, which is synthesized by carboxylates or fatty acid salts of rare earth elements as the main components, and its mechanism is to capture hydrogen chloride and replace allyl chloride atoms. In addition, the epoxy soybean oil in the above-mentioned plasticizing system also serves as an auxiliary heat stabilizer, and its own epoxy group is an absorber of hydrogen chloride, which can react with allyl chloride to partially remove the allyl group, thereby delaying the degradation of PVC. In certain embodiments of the present invention, the rare earth composite stabilizer is synthesized by rare earth element salts as the main components, and is specifically selected from one or more of carboxylates of rare earth elements, fatty acid salts of rare earth elements and oxides of rare earth elements.
[0026] The PVC whole-core flame-retardant conveyor belt covering rubber composition for mining provided by the present invention also includes:
[0027] Chlorinated polyethylene 6-10 parts;
[0028] 8-12 parts of nitrile rubber;
[0029] 4~8 parts of antistatic agent;
[0030] 6~16 parts of flame retardant additives;
[0031] 0.5~2 parts of lubricant;
[0032] 1~3 parts of filler.
[0033] The PVC whole core flame retardant conveyor belt covering rubber composition for mining of the present invention further comprises chlorinated polyethylene. The chlorinated polyethylene of the present invention not only plays the role of a modifier, but also, as one of the components of the flame retardant system, plays the same flame retardant role as chloropalm oil methyl ester in the flame retardant system, that is, it can be compounded with antimony trioxide and chloropalm oil methyl ester in the plasticizer system to achieve chlorine-antimony synergistic flame retardancy, and together constitute the flame retardant system of the composition formula.
[0034] The mining PVC whole core flame retardant conveyor belt covering rubber composition of the present invention also includes nitrile rubber and antistatic agent. Among them, the nitrile rubber is used as a kind of modifier in the present invention to play the effect of toughening, elasticity and wear resistance. The antistatic agent can improve the antistatic performance of the covering rubber. In certain embodiments of the present invention, the antistatic agent is a surfactant type antistatic agent, specifically selected from one or more of cationic antistatic agents, anionic antistatic agents, nonionic antistatic agents, amphoteric antistatic agents and polymer permanent antistatic agents.
[0035] The mining PVC whole core flame retardant conveyor belt covering rubber composition of the present invention also includes a flame retardant additive, which can further improve the flame retardant system of the composition formula. Specifically, the flame retardant additive includes one or more of aluminum hydroxide and zinc borate; wherein the zinc borate is specifically hydrated zinc borate, and its flame retardant mechanism is to release bound water at the combustion temperature, which plays a cooling and heat absorption role; the borate melts and seals the surface of the combustion object to form a glass covering layer, or works together with other flame retardant components to generate a dense carbon layer, which is heat-insulating and oxygen-insulating; it has a certain smoke suppression ability and reduces the amount of smoke; it can have a synergistic effect with other flame retardants, such as chlorine-based flame retardants, and has a flame retardant synergistic effect; it reduces the generation of high-temperature droplets and prevents secondary fires; it is an environmentally friendly flame retardant with the characteristics of non-toxicity, low water solubility, high thermal stability, low strength, low density, and good dispersibility. The flame retardant principle of the aluminum hydroxide is that it absorbs heat and decomposes to release water after being heated. A large amount of water vapor is released into the external environment of the substrate, which can dilute the air and combustible gases. In this process, a large amount of heat can be absorbed, so that the temperature of the substrate is difficult to increase and is maintained above the ignition point, thereby preventing or delaying the occurrence of fire. At the same time, the aluminum oxide remaining after decomposition is very stable and can be covered on the surface of the substrate as a barrier layer, which can play the role of heat insulation, oxygen isolation and smoke suppression.
[0036] The PVC solid core flame retardant conveyor belt covering rubber composition for mining of the present invention further comprises a lubricant and a filler. Specifically, the lubricant comprises one or more of stearic acid, zinc stearate, calcium stearate and polyethylene wax; and the filler comprises one or more of carbon black, calcium carbonate, talc and titanium dioxide.
[0037] In some embodiments of the present invention, the mining PVC whole-core flame-retardant conveyor belt covering rubber composition includes: 100 parts of polyvinyl chloride SG-3 resin; 25-55 parts of chloropalm oil methyl ester; 15-30 parts of triisopropylphenyl phosphate; 4-10 parts of epoxidized soybean oil; 3-6 parts of antimony trioxide; 5-7 parts of rare earth composite stabilizer; 8-12 parts of nitrile rubber; 4-8 parts of antistatic agent; 3-10 parts of aluminum hydroxide; 3-6 parts of zinc borate; 6-10 parts of chlorinated polyethylene; 0.5-2 parts of stearic acid; 1-3 parts of carbon black.
[0038] In some other embodiments of the present invention, the mining PVC whole-core flame-retardant conveyor belt covering rubber composition includes: 100 parts of polyvinyl chloride SG-3 resin; 40-50 parts of chloropalm oil methyl ester; 20-30 parts of triisopropylphenyl phosphate; 8-10 parts of epoxidized soybean oil; 3-6 parts of antimony trioxide; 5-7 parts of rare earth composite stabilizer; 8-12 parts of nitrile rubber; 4-8 parts of antistatic agent; 3-10 parts of aluminum hydroxide; 3-6 parts of zinc borate; 6-10 parts of chlorinated polyethylene; 0.5-2 parts of stearic acid; and 1-3 parts of carbon black.
[0039] The present invention also provides a mining PVC whole-core flame-retardant conveyor belt covering rubber, which is obtained from the mining PVC whole-core flame-retardant conveyor belt covering rubber composition described in any of the above technical solutions.
[0040] The present invention also provides a method for preparing the above-mentioned mining PVC solid-core flame-retardant conveyor belt covering rubber, comprising the following steps:
[0041] S1) pulverizing the mining PVC solid core flame retardant conveyor belt covering rubber composition described in any of the above technical solutions to obtain a powder;
[0042] S2) Granulating the powder obtained in step S1) to obtain a PVC solid-core flame-retardant conveyor belt covering rubber for mining.
[0043] The present invention firstly powders the mining PVC whole core flame retardant conveyor belt covering rubber composition described in any of the above technical solutions to obtain powder. Specifically, chloro-palm oil methyl ester, triisopropylphenyl phosphate and epoxy soybean oil in the composition are used as A material, polyvinyl chloride SG-3 resin and rare earth composite stabilizer are used as B material, and antimony trioxide is used as C material. First, the A material and 0.4 to 0.6 times of the total weight of the B material are mixed within 60°C for 10 min~15 min, and then the remaining B material is added for high-speed stirring. When the temperature rises to 75°C~85°C, the C material is added, and the powder is discharged and cooled when the temperature continues to rise to 100°C~105°C to obtain powder. In certain embodiments of the present invention, the A material and half of the total weight of the B material are first mixed within 60°C for 10 min, and then the remaining B material is added for high-speed stirring, and the C material is added when the temperature rises to 80°C, and the powder is discharged and cooled when the temperature continues to rise to 105°C to obtain powder. If the composition further comprises chlorinated polyethylene, nitrile rubber, an antistatic agent, aluminum hydroxide, zinc borate, stearic acid and carbon black, the antistatic agent is incorporated into the A material, the stearic acid is incorporated into the B material, and the aluminum hydroxide, zinc borate, carbon black and nitrile rubber are incorporated into the C material during powder making.
[0044] After the powder is obtained in the present invention, the obtained powder is granulated to obtain a PVC whole core flame retardant conveyor belt covering rubber for mining. Specifically, the granulation is extrusion granulation. In certain embodiments of the present invention, the obtained powder is extruded and granulated in a screw extruder, and the temperature is controlled at 115±5°C in zone 1, 115±5°C in zone 2, 125±5°C in zone 3, 125±5°C in zone 4, 130±5°C in zone 5, 130±5°C in zone 6, 125±5°C in zone 7, 120±5°C in zone 8, 110±5°C in zone 9, 95±5°C in zone 10, 95±5°C in zone 11, 95±5°C in zone 12, 95±5°C in zone 13, and 95±5°C in the material temperature zone to obtain a PVC whole core flame retardant conveyor belt covering rubber for mining.
[0045] The present invention also provides a mining PVC solid-core flame-retardant conveyor belt, which comprises a belt core and a covering rubber layer covering the surface of the belt core; the covering rubber layer is formed by the above-mentioned mining PVC solid-core flame-retardant conveyor belt covering rubber or the mining PVC solid-core flame-retardant conveyor belt covering rubber obtained by the above-mentioned preparation method.
[0046] The preparation method of the PVC whole core flame retardant conveyor belt for mining provided by the present invention comprises the following steps: extruding the above-mentioned PVC whole core flame retardant conveyor belt for mining on the belt core to obtain the PVC whole core flame retardant conveyor belt for mining. In certain embodiments of the present invention, the above-mentioned PVC whole core flame retardant conveyor belt for mining covering rubber is delivered to the extruder, and the temperature is controlled at 120±5℃ in zone 1, 135±5℃ in zone 2, 145±5℃ in zone 3, 155±5℃ in zone 4, 165±5℃ in zone 5 and 175±5℃ in zone 6, and the covering rubber is extruded on the belt core to obtain the PVC whole core flame retardant conveyor belt for mining.
[0047] The present invention provides a mining PVC whole core flame retardant conveyor belt covering rubber composition, covering rubber and its preparation method and conveyor belt. The covering rubber made of the mining PVC whole core flame retardant conveyor belt covering rubber composition provided by the present invention belongs to environmentally friendly covering rubber, which uses environmentally friendly new materials to replace the harmful additive components currently commonly used in some industries to achieve green substitution, breaks through key technical bottlenecks around green materials, responds to increasingly stringent environmental protection policies and regulations at home and abroad, and enables enterprises to better develop the international market. Among the environmentally friendly new materials used, chloropalm oil methyl ester is used as a plasticizer to replace traditional phthalate plasticizers and chlorinated paraffin, triisopropylphenyl phosphate is used as a flame retardant to replace traditional tris (2-chloroethyl) phosphate, rare earth composite stabilizers are used to replace traditional lead salt stabilizers, and epoxy soybean oil is used as an auxiliary plasticizer and auxiliary stabilizer. Through a certain formula design, it can synergize with each other to improve plasticizing efficiency, enhance thermal stability, excellent flame retardant performance, and difficult to spread in case of fire, reduce the processing cost and quality cost of the enterprise, and at the same time ensure that the physical and safety performance of the covering layer meets industry standards. DETAILED DESCRIPTION
[0048] The present invention discloses a mining PVC whole core flame retardant conveyor belt covering rubber composition, covering rubber and its preparation method and conveyor belt. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It is particularly important to point out that all similar replacements and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the method and application of this article without departing from the content, spirit and scope of the present invention to realize and apply the technology of the present invention.
[0049] The present invention prepares a covering rubber film in accordance with the steps of powder making, granulation and sheet extrusion, and performs a performance test on the obtained covering rubber film to verify the performance of the covering rubber of the present invention in a mining PVC solid core flame retardant conveyor belt.
[0050] 1) Powder making: Chloromethyl palm oil, triisopropyl phosphate, epoxy soybean oil, and antistatic agent are grouped as material A; polyvinyl chloride SG-3 resin, rare earth composite stabilizer, and stearic acid are grouped as material B; carbon black, antimony trioxide, aluminum hydroxide, zinc borate, chlorinated polyethylene, and powdered nitrile rubber are grouped as material C. Add material A and 1 / 2 of material B to the mixer respectively, start low-speed stirring, stir for 10 minutes and control the temperature within 60°C, then add the remaining 1 / 2 of material B, start high-speed stirring, add material C when the temperature reaches 80°C, and discharge the powder and cool it when the temperature reaches 105°C.
[0051] 2) Granulation: The powder obtained by pulverizing is conveyed to the screw extruder. The temperature of zone 1 is controlled at 115±5℃, zone 2 is 115±5℃, zone 3 is 125±5℃, zone 4 is 125±5℃, zone 5 is 130±5℃, zone 6 is 130±5℃, zone 7 is 125±5℃, zone 8 is 120±5℃, zone 9 is 110±5℃, zone 10 is 95±5℃, zone 11 is 95±5℃, zone 12 is 95±5℃, zone 13 is 95±5℃ and the material temperature zone is 95±5℃. The temperature of the main and auxiliary extruders is adjusted within the set range according to the extrusion volume to ensure that the pellets are evenly dispersed and the plasticization quality is qualified. The pelletizer adjusts the speed in time according to the size of the pellets.
[0052] 3) Extrusion: Cool the prepared pellets and then convey them to the extruder. The temperature of zone 1 is controlled at 120±5℃, zone 2 is 135±5℃, zone 3 is 145±5℃, zone 4 is 155±5℃, zone 5 is 165±5℃, and zone 6 is 175±5℃. During the extrusion process, the extruder temperature is adjusted in time according to the appearance of the covering rubber.
[0053] In a specific implementation manner of the present invention, the antistatic agent used is KJ-100 produced by Zhenghe Chemical; and the stabilizer used is the rare earth modified composite stabilizer produced by Keao Plastics.
[0054] The present invention will be further described below in conjunction with embodiments:
[0055] Example 1
[0056] A formula for an environmentally friendly PVC whole-core flame-retardant conveyor belt covering rubber for mining is composed of the following ingredients in parts by weight: 100 parts of polyvinyl chloride SG-3 resin, 45 parts of chloropalm oil methyl ester, 25 parts of triisopropylphenyl phosphate, 10 parts of epoxy soybean oil, 4 parts of antimony trioxide, 6 parts of rare earth composite stabilizer, 7 parts of aluminum hydroxide, 4 parts of zinc borate, 7 parts of chlorinated polyethylene, 8 parts of powdered nitrile rubber, 6 parts of antistatic agent, 1 part of stearic acid, and 1 part of carbon black.
[0057] Chloropalm oil methyl ester, triisopropylphenyl phosphate, epoxy soybean oil, and antistatic agent are classified as material A; polyvinyl chloride SG-3 resin, rare earth composite stabilizer, and stearic acid are classified as material B; carbon black, antimony trioxide, aluminum hydroxide, zinc borate, chlorinated polyethylene, and powdered nitrile rubber are classified as material C. Add material A and 1 / 2 of material B to the mixer respectively, start low-speed stirring, stir for 10 minutes to control the temperature within 60°C, then add the remaining 1 / 2 of material B, start high-speed stirring, add material C when the temperature reaches 80°C, and discharge and cool the powder when the temperature reaches 105°C. The obtained powder is transported to the granulating screw extruder, and the extruder and pelletizer are adjusted to obtain pellets according to the granulation method and conditions in 2) above. After cooling the pellets, transport them to the extruder and extrude them according to the extrusion method and conditions in 3) above to obtain the covering rubber film.
[0058] The performance indicators of the cover rubber film prepared in Example 1 of the present invention are shown in Table 1:
[0059] Table 1
[0060]
[0061] In the alcohol torch combustion test, the covering rubber burned with flame for an average of 0.97 s and burned without flame for an average of 0.42 s.
[0062] The formula of Example 1 of the present invention uses environmentally friendly new materials to replace harmful additive components currently commonly used in some industries, thereby achieving green substitution. The physical and safety properties of the covering glue meet Australian standards and can be exported to open up international markets.
[0063] Comparative Example 1
[0064] A formula for an environmentally friendly PVC whole-core flame-retardant conveyor belt covering rubber for mining is composed of the following ingredients in parts by weight: 100 parts of polyvinyl chloride SG-3 resin, 55 parts of dioctyl phthalate, 25 parts of tri(2-chloroethyl) phosphate, 4 parts of antimony trioxide, 6 parts of rare earth composite stabilizer, 7 parts of aluminum hydroxide, 4 parts of zinc borate, 7 parts of chlorinated polyethylene, 8 parts of powdered nitrile rubber, 6 parts of antistatic agent, 1 part of stearic acid, and 1 part of carbon black.
[0065] Dioctyl phthalate, tri(2-chloroethyl) phosphate, and antistatic agent are classified as material A; polyvinyl chloride SG-3 resin, rare earth composite stabilizer, and stearic acid are classified as material B; carbon black, antimony trioxide, aluminum hydroxide, zinc borate, chlorinated polyethylene, and powdered nitrile rubber are classified as material C. Add material A and 1 / 2 of material B to the mixer respectively, start low-speed stirring, stir for 10 minutes to control the temperature within 60°C, then add the remaining 1 / 2 of material B, start high-speed stirring, add material C when the temperature reaches 80°C, and discharge the powder and cool when the temperature reaches 105°C. The obtained powder is transported to the granulating screw extruder, the extruder and pelletizer are adjusted to obtain pellets, and the pellets are cooled and transported to the extruder for sheet extrusion to obtain the covering rubber film.
[0066] The performance indicators of the cover rubber film prepared in this comparative example 1 are shown in Table 2:
[0067] Table 2
[0068]
[0069] In the alcohol torch combustion test, the covering rubber burned with flame for an average of 2.86 s and burned without flame for an average of 2.63 s.
[0070] Compared with Example 1, the covering glue formula of this comparative example 1 replaces the chloropalm oil methyl ester with dioctyl phthalate, replaces the epoxidized soybean oil with dioctyl phthalate, replaces the triisopropylphenyl phosphate with tri(2-chloroethyl) phosphate, and the other raw materials remain unchanged. The elongation at break and the tensile strength of the test piece are significantly reduced, and the time of flaming combustion and flameless combustion is significantly increased. It can be seen that when chloropalm oil methyl ester, triisopropylphenyl phosphate, and epoxidized soybean oil are used in conjunction to replace dioctyl phthalate and tri(2-chloroethyl) phosphate, the mechanical properties and flame retardancy of the covering glue can be significantly improved.
[0071] Comparative Example 2
[0072] A formula for an environmentally friendly PVC whole-core flame-retardant conveyor belt covering rubber for mining is composed of the following ingredients in parts by weight: 100 parts of polyvinyl chloride SG-3 resin, 55 parts of chloropalm oil methyl ester, 25 parts of triisopropylphenyl phosphate, 4 parts of antimony trioxide, 6 parts of rare earth composite stabilizer, 7 parts of aluminum hydroxide, 4 parts of zinc borate, 7 parts of chlorinated polyethylene, 8 parts of powdered nitrile rubber, 6 parts of antistatic agent, 1 part of stearic acid, and 1 part of carbon black.
[0073] Chloropalm oil methyl ester, triisopropyl phosphate, and antistatic agent are classified as material A; polyvinyl chloride SG-3 resin, rare earth composite stabilizer, and stearic acid are classified as material B; carbon black, antimony trioxide, aluminum hydroxide, zinc borate, chlorinated polyethylene, and powdered nitrile rubber are classified as material C. Add material A and 1 / 2 of material B to the mixer respectively, start low-speed stirring, stir for 10 minutes to control the temperature within 60°C, then add the remaining 1 / 2 of material B, start high-speed stirring, add material C when the temperature reaches 80°C, and discharge and cool the powder when the temperature reaches 105°C. The obtained powder is transported to the granulating screw extruder, the extruder and pelletizer are adjusted to obtain pellets, and the pellets are cooled and transported to the extruder for sheet extrusion to obtain the covering rubber film.
[0074] The performance indicators of the cover rubber film prepared in this comparative example 2 are shown in Table 3:
[0075] Table 3
[0076]
[0077] In the alcohol torch combustion test, the covering rubber burned with flame for an average of 1.23 s and burned without flame for an average of 0.69 s.
[0078] Compared with Example 1, the covering glue formula of Comparative Example 2 replaces the epoxy soybean oil with chloro palm oil methyl ester, and the other raw materials remain unchanged. The elongation at break and the tensile strength of the test piece are reduced, and the flaming combustion and flameless combustion times are increased. At the same time, referring to Example 1 and Comparative Example 1, it can be seen that when epoxy soybean oil is used together with chloro palm oil methyl ester and triisopropylphenyl phosphate, there is a certain plasticizing and flame retardant synergistic effect, and the mechanical properties and flame retardant properties of the covering glue can be improved compared with the use of chloro palm oil methyl ester and triisopropylphenyl phosphate alone.
[0079] Comparative Example 3
[0080] A formula for an environmentally friendly PVC whole-core flame-retardant conveyor belt covering rubber for mining is composed of the following ingredients in parts by weight: 100 parts of polyvinyl chloride SG-3 resin, 45 parts of chloropalm oil methyl ester, 25 parts of tri(2-chloroethyl) phosphate, 10 parts of epoxy soybean oil, 4 parts of antimony trioxide, 6 parts of rare earth composite stabilizer, 7 parts of aluminum hydroxide, 4 parts of zinc borate, 7 parts of chlorinated polyethylene, 8 parts of powdered nitrile rubber, 6 parts of antistatic agent, 1 part of stearic acid, and 1 part of carbon black.
[0081] Chloropalm oil methyl ester, tri(2-chloroethyl) phosphate, epoxy soybean oil, and antistatic agent are classified as material A; polyvinyl chloride SG-3 resin, rare earth composite stabilizer, and stearic acid are classified as material B; carbon black, antimony trioxide, aluminum hydroxide, zinc borate, chlorinated polyethylene, and powdered nitrile rubber are classified as material C. Add material A and 1 / 2 of material B to the mixer respectively, start low-speed stirring, stir for 10 minutes to control the temperature within 60°C, then add the remaining 1 / 2 of material B, start high-speed stirring, add material C when the temperature reaches 80°C, and discharge and cool the powder when the temperature reaches 105°C. The obtained powder is transported to the granulating screw extruder, the extruder and the pelletizer are adjusted to obtain pellets, and the pellets are cooled and transported to the extruder for sheet extrusion to obtain the covering rubber film.
[0082] The performance indicators of the cover rubber film prepared in this comparative example 3 are shown in Table 4:
[0083] Table 4
[0084]
[0085] In the alcohol torch combustion test, the covering rubber burned with flame for an average of 1.53 s and burned without flame for an average of 0.89 s.
[0086] Compared with Example 1, the covering glue formula of Comparative Example 3 replaces the proportion of triisopropylphenyl phosphate with tri(2-chloroethyl) phosphate, and the proportions of other raw materials remain unchanged. The elongation at break and tensile strength of the test piece are reduced, and the flaming and flameless combustion times are increased. At the same time, referring to Example 1 and Comparative Example 1, it can be seen that triisopropylphenyl phosphate has a certain plasticizing and flame retardant synergistic effect when used together with chloropalm oil methyl ester and epoxidized soybean oil.
[0087] Comparative Example 4
[0088] A formula for an environmentally friendly PVC whole-core flame-retardant conveyor belt covering rubber for mining is composed of the following ingredients in parts by weight: 100 parts of polyvinyl chloride SG-3 resin, 45 parts of dioctyl phthalate, 25 parts of triisopropylphenyl phosphate, 10 parts of epoxy soybean oil, 4 parts of antimony trioxide, 6 parts of rare earth composite stabilizer, 7 parts of aluminum hydroxide, 4 parts of zinc borate, 7 parts of chlorinated polyethylene, 8 parts of powdered nitrile rubber, 6 parts of antistatic agent, 1 part of stearic acid, and 1 part of carbon black.
[0089] Dioctyl phthalate, triisopropylphenyl phosphate, epoxy soybean oil, and antistatic agent are classified as material A; polyvinyl chloride SG-3 resin, rare earth composite stabilizer, and stearic acid are classified as material B; carbon black, antimony trioxide, aluminum hydroxide, zinc borate, chlorinated polyethylene, and powdered nitrile rubber are classified as material C. Add material A and 1 / 2 of material B to the mixer respectively, start low-speed stirring, stir for 10 minutes to control the temperature within 60°C, then add the remaining 1 / 2 of material B, start high-speed stirring, add material C when the temperature reaches 80°C, and discharge the powder and cool when the temperature reaches 105°C. The obtained powder is transported to the granulating screw extruder, the extruder and pelletizer are adjusted to obtain pellets, and the pellets are cooled and transported to the extruder for sheet extrusion to obtain the covering rubber film.
[0090] The performance indicators of the cover rubber film prepared in this comparative example 4 are shown in Table 5:
[0091] Table 5
[0092]
[0093] In the alcohol torch combustion test, the covering rubber burned with flame for an average of 1.86 s and burned without flame for an average of 0.83 s.
[0094] Compared with Example 1, the covering glue formula of Comparative Example 4 replaces the chloropalm oil methyl ester with dioctyl phthalate, and the other raw materials remain unchanged. The elongation at break and tensile strength of the test piece are reduced, and the flaming combustion and flameless combustion times are increased. At the same time, referring to Example 1 and Comparative Example 1, it can be seen that chloropalm oil methyl ester has a certain plasticizing and flame retardant synergistic effect when used together with triisopropylphenyl phosphate and epoxy soybean oil.
[0095] The performance test results of the covering glue formulations of the above-mentioned Example 1 and Comparative Examples 1 to 4 are listed in Table 6 for comparison:
[0096] Table 6
[0097]
[0098] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A PVC whole core flame retardant conveyor belt covering rubber composition for mining, characterized in that: In parts by weight, it includes: 100 parts of polyvinyl chloride SG-3 resin; 25-55 parts of chloropalm oil methyl ester; 15-30 parts of triisopropylphenyl phosphate; Epoxidized soybean oil 4-10 parts; 3-6 parts of antimony trioxide; 5~7 parts of rare earth composite stabilizer.
2. The PVC whole core flame retardant conveyor belt covering rubber composition for mining use according to claim 1, characterized in that: It also includes: Chlorinated polyethylene 6-10 parts; 8-12 parts of nitrile rubber; 4~8 parts of antistatic agent; 6~16 parts of flame retardant additives; 0.5~2 parts of lubricant; 1~3 parts of filler.
3. The PVC whole core flame retardant conveyor belt covering rubber composition for mining use according to claim 2, characterized in that: The flame retardant additive includes one or more of aluminum hydroxide, zinc borate, aluminum hydroxide, triphenyl phosphate, chlorinated paraffin, and tetrabromophthalate.
4. The PVC whole core flame retardant conveyor belt covering rubber composition for mining use according to claim 2, characterized in that: The lubricant includes one or more of stearic acid, zinc stearate, calcium stearate, and polyethylene wax.
5. The PVC whole core flame retardant conveyor belt covering rubber composition for mining use according to claim 2, characterized in that: The filler includes one or more of carbon black, calcium carbonate, talcum powder and titanium dioxide.
6. The mining PVC solid-core flame-retardant conveyor belt covering rubber composition according to any one of claims 1 to 5, comprising: 100 parts of polyvinyl chloride SG-3 resin; 25-55 parts of chloropalm oil methyl ester; 15-30 parts of triisopropylphenyl phosphate; Epoxidized soybean oil 4-10 parts; 3-6 parts of antimony trioxide; 5-7 parts of rare earth composite stabilizer; Chlorinated polyethylene 6-10 parts; 8-12 parts of nitrile rubber; 4~8 parts of antistatic agent; 3-10 parts of aluminum hydroxide; 3-6 parts of zinc borate; 0.5~2 parts of stearic acid; 1~3 parts of carbon black.
7. The PVC whole core flame retardant conveyor belt covering rubber composition for mining use according to claim 6, characterized in that: It includes: 100 parts of polyvinyl chloride SG-3 resin; 40-50 parts of chloropalm oil methyl ester; 20-30 parts of triisopropylphenyl phosphate; Epoxidized soybean oil 8-10 parts; 3-6 parts of antimony trioxide; 5-7 parts of rare earth composite stabilizer; Chlorinated polyethylene 6-10 parts; 8-12 parts of nitrile rubber; 4~8 parts of antistatic agent; 3-10 parts of aluminum hydroxide; 3-6 parts of zinc borate; 0.5~2 parts of stearic acid; 1~3 parts of carbon black.
8. PVC whole core flame retardant conveyor belt covering rubber for mining, characterized by: The invention is obtained from the mining PVC whole-core flame-retardant conveyor belt covering rubber composition described in any one of claims 1 to 7.
9. A method for preparing a PVC solid core flame retardant conveyor belt covering rubber for mining, characterized in that: The following steps are involved: S1) pulverizing the mining PVC solid core flame retardant conveyor belt covering rubber composition as claimed in any one of claims 1 to 7 to obtain a powder; S2) Granulating the powder obtained in step S1) to obtain a PVC solid-core flame-retardant conveyor belt covering rubber for mining.
10. PVC whole core flame retardant conveyor belt for mining, characterized by: It comprises a belt core and a covering rubber layer covering the surface of the belt core; The covering rubber layer is formed by the covering rubber of the mining PVC solid core flame retardant conveyor belt described in claim 8 or the covering rubber of the mining PVC solid core flame retardant conveyor belt obtained by the preparation method described in claim 9.
Citation Information
Cited By
Adhesive cement for PVC / PVG (polyvinyl chloride / polyvinyl chloride) whole-core flame-retardant conveyor belt joint as well as preparation method and application of adhesive cement
CN121471845A