Gap reflective film capable of improving photoelectric efficiency and preparation method thereof
The three-dimensional crosslinking network is constructed by modifying polyvinylidene fluoride and copolymethyl methacrylate, which solves the problems of microstructure defects and low light reflection efficiency in the production process of the gap reflective film, and improves the photoelectric efficiency and material performance.
Patent Information
- Application Number
- CN202411496784.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-25
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing gap reflective films have problems of microstructure defects and low light reflection efficiency in the production process, especially in the roll-to-roll heat rolling process, which is short contact time and insufficient rigid segments due to the fast production speed.
Modified polyvinylidene fluoride and copolymethyl methacrylate are used as substrate layer materials, and a three-dimensional cross-linking network is constructed through bifunctional group phenyl phosphate modification and nanotitanium dioxide to increase the mechanical properties of the material and the resistance to UV. Magneto-controlled sputtering deposition method or vacuum evaporation method to prepare the reflective layer to reduce microstructure defects.
It improves photoelectric efficiency and the mechanical properties of the material, reduces microstructure defects, extends service life, and improves thermal stability and flame retardant properties.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of intermittent reflective films, in particular to an intermittent reflective film for improving photoelectric efficiency and a preparation method thereof. Background Art
[0002] By laying gap reflective film on the surface of photovoltaic cell welding strips and the gap between cell strings, the microstructure set on the gap reflective film can effectively reflect the light irradiated on the surface of welding strips and the gap between cell strings and converge to the cell surface, thereby improving the utilization rate of light energy, especially improving the utilization rate of light energy in weak light environment.
[0003] The gap reflective film is used to improve the light utilization rate mainly by coating on the microstructure layer, so as to reflect and utilize the light, and the microstructure layer with a preset prism shape can better converge the reflected light and thus improve the photoelectric efficiency; there are currently two mainstream preparation technologies for microstructures, namely roll-to-roll hot rolling process and UV curing molding process. Since the UV curing molding process is prone to incomplete curing of the microstructured adhesive layer during the curing shrinkage and the control of the UV adhesive dosage, resulting in uneven refractive index inside the microstructure, there are still many bottlenecks in the large-scale application of this process; and the roll-to-roll hot rolling process also has certain problems during use, mainly because during the production process, after the rolling speed increases, the contact time between the microstructure layer film and the mold roller is short, resulting in it not reaching the required state of irreversible deformation, resulting in the rebound phenomenon of some microstructures after rolling, resulting in defects in the final prepared microstructure layer, which in turn affects the reflected light efficiency, and directly heating or pressurizing the mold roller is prone to surface collapse defects and high and low pyramid defects, resulting in certain problems in its large-scale rapid production. Summary of the invention
[0004] The object of the present invention is to provide a gap reflective film for improving photoelectric efficiency and a preparation method thereof, so as to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: A gap reflective film for improving photoelectric efficiency, characterized in that it comprises the following components by mass ratio: 6.5-7.5 of copolymerized methyl methacrylate, 2.5-3.5 of modified polyvinylidene fluoride resin and 0.06-0.08 of modified nano titanium dioxide.
[0006] As an optimization, the copolymerized methyl methacrylate is prepared by copolymerizing hindered amino methacrylate, methyl methacrylate and allyl triethoxysilane in a molar ratio of 1:2~2.2:0.25~0.35.
[0007] As an optimization, the modified polyvinylidene fluoride resin is prepared by pre-irradiating polyvinylidene fluoride and then grafting bifunctional phenyl phosphate.
[0008] A method for preparing a gap reflective film for improving photoelectric efficiency, wherein the gap reflective film is prepared by the following steps: S1. Add difunctional phenyl phosphate to dioxane at a mass ratio of 1:3-3.5, stir evenly to prepare a difunctional phenyl phosphate solution for standby use; place polyvinylidene fluoride in a nitrogen atmosphere. 60 Pre-irradiation is performed in a Co irradiation room, and after the pre-irradiation is completed, it is stored at a temperature of 0-5°C for standby use; under nitrogen protection and a temperature of 50-55°C, the pre-irradiated polyvinylidene fluoride is added to a bifunctional phenyl phosphate solution with a mass of 20-22 times that of the polyvinylidene fluoride, and the reaction is stirred for 4-6 hours. After the reaction is completed, the filtered product is placed in a Soxhlet extractor, washed with toluene and refluxed for 12-14 hours, and after washing and reflux, it is vacuum dried to constant weight at a temperature of 80-85°C to obtain a modified polyvinylidene fluoride resin; S2. Weigh hindered amino methacrylate, methyl methacrylate and allyl triethoxysilane in a molar ratio of 1:2-2.2:0.25-0.35, add hindered amino methacrylate, methyl methacrylate and allyl triethoxysilane to toluene with a mass of 6-7 times of methyl methacrylate, add azobisisobutyronitrile with a mass of 0.001-0.003 times of methyl methacrylate after ultrasonic dispersion for 15-20 minutes, stir and react at a temperature of 80-90°C for 1-1.5 hours, and then keep the temperature at 55-65°C for 36-48 hours to obtain copolymerized methyl methacrylate; S3, weighing copolymerized methyl methacrylate, modified polyvinylidene fluoride resin and modified nano titanium dioxide in a mass ratio of 6.5-7.5:2.5-3.5:0.06-0.08, first adding copolymerized methyl methacrylate and modified polyvinylidene fluoride resin to tetrahydrofuran (20-22 times the mass of copolymerized methyl methacrylate) and stirring to dissolve, then adding modified nano titanium dioxide, and then adding trifluoromethylsulfonic acid catalyst (1.5%-2% times the mass of copolymerized methyl methacrylate), stirring and reacting at a temperature of 60-70°C for 18-20h, then naturally cooling to room temperature, and drying the reactants in a vacuum oven to constant weight to obtain a base material masterbatch; S4. The base material masterbatch is subjected to high-temperature multi-layer cast co-extrusion to obtain a polymer film, and then the polymer film is rolled through a mold roller using a roll-to-roll hot rolling process to obtain a polymer film with a microstructure; a reflective layer is prepared on the side of the polymer film surface with a microstructure using a magnetron sputtering deposition method or a vacuum evaporation method, and an adhesive layer is obtained on the other side of the polymer film surface by cast co-extrusion treatment, and then a gap reflective film is obtained by a slitting and winding device.
[0009] As an optimization, the parameters set in the pre-irradiation process are that the radiation source activity is 30000 Ci and the dose rate is 200 Gy / min.
[0010] As an optimization, the mold roller temperature during the roll-to-roll hot rolling process is 120° C. and the speed is 1-30 m / min.
[0011] As an optimization, the preparation method of the modified nano titanium dioxide is as follows: adding nano titanium dioxide powder to anhydrous ethanol at a mass ratio of 1:10, ultrasonically dispersing for 5 to 15 minutes, stirring at 20 to 30°C for 5 to 15 minutes, adding tetraethyl silicate and 25% ammonia water by mass, heating to 60 to 80°C and reacting for 3 to 5 hours, and after the reaction is completed, washing and drying after centrifugal filtration to obtain modified nano titanium dioxide.
[0012] As an optimization, the mass ratio of the nano titanium dioxide powder to tetraethyl silicate is 2.5-3:1, and the volume ratio of the anhydrous ethanol to 25% ammonia water is 8-9:1.
[0013] As an optimization, the preparation method of the hindered amino methacrylate is: at a temperature of 0~5°C, tetramethylpiperidinol and triethylamine are added to tetrahydrofuran in a mass ratio of 1:0.4~0.6:20~22, stirred evenly, and 1.4~1.6 times the mass of tetramethylpiperidinol acryloyl chloride is uniformly added dropwise within 1~1.5 hours, and after the addition is completed, the reaction is stirred for 6~8 hours and then allowed to stand and filtered, and the filtered product is recrystallized with an excess mass fraction of 50% ethanol solution, and the recrystallized product is placed in a vacuum oven and dried to constant weight to obtain hindered amino methacrylate.
[0014] As an optimization, the preparation method of the bifunctional phenyl phosphate is as follows: 3-aminopropyltriethoxysilane is added to tetrahydrofuran at a mass ratio of 1:2.4~2.6, stirred evenly, configured to a 3-aminopropyltriethoxysilane solution, and allowed to stand for use; 2,2'-diallylbisphenol A is added to tetrahydrofuran at a mass ratio of 1:1.5~1.8, stirred evenly, configured to a 2,2'-diallylbisphenol A solution, and allowed to stand for use; at a temperature of -5~0°C, phenyl dichlorophosphate is added to tetrahydrofuran at a mass ratio of 1:3.2~3.5, stirred for 0.5~0.8h, and then , add triethylamine in an amount of 1 to 1.2 times the mass of phenyl dichlorophosphate, stir evenly and uniformly add 3-aminopropyltriethoxysilane solution in an amount of 2.8 to 3 times the mass of phenyl dichlorophosphate within 2 to 2.5 hours, continue stirring for 3 to 5 hours after the addition is complete, stir evenly and uniformly add 2,2'-diallylbisphenol A solution in an amount of 1.3 to 1.5 times the mass of phenyl dichlorophosphate within 2 to 2.5 hours, continue stirring and react for 3 to 5 hours after the addition is complete, heat to 25 to 35°C after the reaction is complete, continue stirring and react for 8 to 12 hours, filter after the reaction is complete, and evaporate the filtrate to remove unreacted monomers to obtain difunctional phenyl phosphate.
[0015] Compared with the prior art, the beneficial effects achieved by the present invention are: The present application adopts polyvinylidene fluoride and polymethyl methacrylate as the main materials of the substrate layer, wherein polyvinylidene fluoride has the advantages of non-stickiness, non-water absorption, high insulation strength, high barrier to gases such as oxygen, resistance to ozone and resistance to natural aging, etc., while copolymerized methyl methacrylate has the advantages of low cohesive energy and flexible molecular chain, etc.; however, in order to avoid the problem of microstructural defects caused by fast production speed in the roll-to-roll hot rolling process, the above two substrates are modified in a targeted manner. The main reason for the microstructural defects in the roll-to-roll process is that the contact time between the mold roller and the film is short after the production speed is increased, resulting in failure to reach the glass The high chemical transition temperature and insufficient rigid segments in the substrate lead to rebound and collapse defects. Therefore, the present invention first uses difunctional phenyl phosphate to modify polyvinylidene fluoride, provides rigid segments through difunctional phenyl phosphate, introduces rigid segments by copolymerizing hindered amino methacrylate and methyl methacrylate, thereby improving the mechanical properties of the substrate, and finally uses a sol-gel method to construct a three-dimensional cross-linked network around modified nano-titanium dioxide with modified polyvinylidene fluoride resin and copolymerized methyl methacrylate, and the added modified nano-titanium dioxide also serves as a rigid filler to further improve the mechanical properties of the material; Since the modified polyvinylidene fluoride resin and copolymerized methyl methacrylate construct a dense three-dimensional cross-linked network around the nano-titanium dioxide, it is different from the traditional blended polymer and block copolymer, and the substrate has a wider glass transition temperature range, mainly because the traditional blended or block polymer will have phase separation when reaching the glass transition temperature, resulting in only a single or two glass transition temperatures; and the special structure of the cross-linked copolymer constructed in the present application makes the phase interface unclear, so it has a wider glass transition temperature, resulting in a gradual change in its mechanical properties, and the sudden change shown by the non-blended or block copolymer also reduces the collapse defects in the production process; In the process of constructing the rigid segment of the present application, hindered amines and hindered phenols are respectively used, so that it has good UV resistance and improves the service life of the overall substrate. Dichlorophenyl phosphate is used as a bridging group of the hindered phenol, and 3-aminopropyltriethoxysilane is connected. Dichlorophenyl phosphate is used as a phosphorus source, and 3-aminopropyltriethoxysilane is used as a nitrogen source and a silicon source, thereby constructing a nitrogen, phosphorus, and silicon flame retardant synergistic effect, thereby improving the thermal stability and flame retardant properties of the overall material. DETAILED DESCRIPTION
[0016] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0017] In order to more clearly illustrate the method provided by the present invention, the following examples are provided in detail. The raw materials used in the experimental part of the following examples are as follows: Table 1 - Raw materials used in the experimental part
[0018] Example 1
[0019] S1. Add nano titanium dioxide powder to anhydrous ethanol at a mass ratio of 1:10, ultrasonically disperse for 5 minutes, stir for 5 minutes at 20°C, add tetraethyl silicate and 25% ammonia water by mass, heat to 60°C and react for 3 hours. After the reaction, centrifuge and filter, wash and dry to obtain modified nano titanium dioxide; wherein the mass ratio of nano titanium dioxide powder to tetraethyl silicate is 2.5:1, and the volume ratio of anhydrous ethanol to 25% ammonia water by mass is 8:1; S2. At a temperature of 0°C, add tetramethylpiperidinol and triethylamine to tetrahydrofuran in a mass ratio of 1:0.4:20, stir evenly, and uniformly add 1.4 times the mass of tetramethylpiperidinol in acryloyl chloride within 1 hour. After the addition is complete, stir and react for 6 hours, then let stand and filter. Recrystallize the filtered product with an excess of 50% by mass ethanol solution, and dry the recrystallized product in a vacuum oven to constant weight to obtain hindered amino methacrylate. S3. Add 3-aminopropyltriethoxysilane to tetrahydrofuran at a mass ratio of 1:2.4, stir evenly, and prepare a 3-aminopropyltriethoxysilane solution, and let it stand for use; add 2,2'-diallylbisphenol A to tetrahydrofuran at a mass ratio of 1:1.5, stir evenly, and prepare a 2,2'-diallylbisphenol A solution, and let it stand for use; at a temperature of -5°C, add phenyl dichlorophosphate to tetrahydrofuran at a mass ratio of 1:3.2, stir for 0.5h, and then add dichlorophosphate. 1 times the mass of phenyl chlorophosphate, triethylamine, stir evenly, and uniformly add 3-aminopropyltriethoxysilane solution with a mass of 2.8 times the mass of phenyl dichlorophosphate within 2 hours, continue stirring for 3 hours after the addition is complete, stir evenly, and uniformly add 2,2'-diallylbisphenol A solution with a mass of 1.3 times the mass of phenyl dichlorophosphate within 2 hours, continue stirring and react for 3 hours after the addition is complete, heat to 25°C after the reaction is complete, continue stirring and react for 8 hours, filter after the reaction is complete, and remove unreacted monomers by rotary evaporation of the filtrate to obtain bifunctional phenyl phosphate; S4. Add difunctional phenyl phosphate to dioxane at a mass ratio of 1:3, and stir evenly to prepare a difunctional phenyl phosphate solution for standby use; in a nitrogen atmosphere, place polyvinylidene fluoride in a 60 Pre-irradiation was performed in a Co irradiation chamber, and the parameters set during the pre-irradiation process were that the radiation source activity was 30000Ci and the dose rate was 200Gy / min. After the pre-irradiation was completed, the solution was placed at a temperature of 0°C for storage for future use; under nitrogen protection and a temperature of 50°C, the pre-irradiated polyvinylidene fluoride was added to a bifunctional phenyl phosphate solution with a mass 20 times that of the polyvinylidene fluoride, and the reaction was stirred for 4 hours. After the reaction was completed, the filtered product was placed in a Soxhlet extractor, washed with toluene and refluxed for 12 hours, and after washing and refluxed, the solution was vacuum dried at a temperature of 80°C to constant weight to obtain a modified polyvinylidene fluoride resin; S5. Weigh hindered amino methacrylate, methyl methacrylate and allyl triethoxysilane in a molar ratio of 1:2:0.25, add hindered amino methacrylate, methyl methacrylate and allyl triethoxysilane to toluene with a mass of 6 times that of methyl methacrylate, add azobisisobutyronitrile with a mass of 0.001 times that of methyl methacrylate after ultrasonic dispersion for 15 minutes, stir and react at a temperature of 80°C for 1 hour, and then keep the temperature at 55°C for 36 hours to obtain copolymerized methyl methacrylate; S6. Weigh copolymerized methyl methacrylate, modified polyvinylidene fluoride resin and modified nano titanium dioxide in a mass ratio of 6.5:2.5:0.06. First, add copolymerized methyl methacrylate and modified polyvinylidene fluoride resin into tetrahydrofuran (20 times the mass of copolymerized methyl methacrylate) and stir to dissolve. Then add modified nano titanium dioxide. Then add trifluoromethylsulfonic acid catalyst (1.5% the mass of copolymerized methyl methacrylate). Stir the reaction at 60°C for 18 hours, then cool naturally to room temperature. Dry the reactants in a vacuum oven to constant weight to obtain the base material masterbatch.
[0020] Example 2
[0021] S1. Add nano titanium dioxide powder to anhydrous ethanol at a mass ratio of 1:10, ultrasonically disperse for 10 minutes, stir at 25°C for 10 minutes, add tetraethyl silicate and 25% ammonia water by mass, heat to 70°C and react for 4 hours, centrifuge and filter after the reaction, wash and dry to obtain modified nano titanium dioxide; wherein the mass ratio of nano titanium dioxide powder to tetraethyl silicate is 2.8:1, and the volume ratio of anhydrous ethanol to 25% ammonia water by mass is 8.5:1; S2. At a temperature of 3°C, add tetramethylpiperidinol and triethylamine to tetrahydrofuran in a mass ratio of 1:0.5:21, stir evenly, and uniformly add 1.5 times the mass of tetramethylpiperidinol of acryloyl chloride within 1.2 hours. After the addition is complete, stir and react for 7 hours, then let stand and filter. Recrystallize the filtered product with an excess of 50% by mass of ethanol solution, and dry the recrystallized product in a vacuum oven to constant weight to obtain hindered amino methacrylate. S3. Add 3-aminopropyltriethoxysilane to tetrahydrofuran at a mass ratio of 1:2.5, stir evenly, and prepare a 3-aminopropyltriethoxysilane solution, and let it stand for use; add 2,2'-diallylbisphenol A to tetrahydrofuran at a mass ratio of 1:1.6, stir evenly, and prepare a 2,2'-diallylbisphenol A solution, and let it stand for use; at a temperature of -3°C, add phenyl dichlorophosphate to tetrahydrofuran at a mass ratio of 1:3.4, stir for 0.6h, and then add phenyl dichlorophosphate. The mixture was stirred evenly, and a 3-aminopropyltriethoxysilane solution with a mass of 2.9 times that of phenyl dichlorophosphate was added dropwise at a uniform rate within 2.2 hours. After the addition was completed, stirring was continued for 4 hours. The mixture was stirred evenly, and a 2,2'-diallylbisphenol A solution with a mass of 1.4 times that of phenyl dichlorophosphate was added dropwise at a uniform rate within 2.2 hours. After the addition was completed, stirring was continued for 4 hours. After the reaction was completed, the mixture was heated to 30°C, and stirring was continued for 10 hours. After the reaction was completed, the filtrate was filtered and the unreacted monomers were removed by rotary evaporation to obtain difunctional phenyl phosphate. S4. Add difunctional phenyl phosphate to dioxane at a mass ratio of 1:3.2, and stir evenly to prepare a difunctional phenyl phosphate solution for standby use; in a nitrogen atmosphere, place polyvinylidene fluoride in a 60 Pre-irradiation was performed in a Co irradiation chamber, and the parameters set during the pre-irradiation process were that the radiation source activity was 30000Ci and the dose rate was 200Gy / min. After the pre-irradiation was completed, the polyvinylidene fluoride was stored at a temperature of 3°C for standby use; under nitrogen protection and a temperature of 52°C, the pre-irradiated polyvinylidene fluoride was added to a bifunctional phenyl phosphate solution with a mass of 21 times that of the polyvinylidene fluoride, and the reaction was stirred for 5 hours. After the reaction was completed, the filtered product was placed in a Soxhlet extractor, washed with toluene and refluxed for 13 hours, and after washing and reflux, it was vacuum dried at a temperature of 82°C to constant weight to obtain a modified polyvinylidene fluoride resin; S5. Weigh hindered amino methacrylate, methyl methacrylate and allyl triethoxysilane in a molar ratio of 1:2.1:0.3, add hindered amino methacrylate, methyl methacrylate and allyl triethoxysilane to toluene (6.5 times the mass of methyl methacrylate), add azobisisobutyronitrile (0.002 times the mass of methyl methacrylate) after ultrasonic dispersion for 18 minutes, stir and react at 85°C for 1.2 hours, and then keep the reaction at 60°C for 42 hours to obtain copolymerized methyl methacrylate; S6. Weigh copolymerized methyl methacrylate, modified polyvinylidene fluoride resin and modified nano titanium dioxide in a mass ratio of 7:3:0.07. First, add copolymerized methyl methacrylate and modified polyvinylidene fluoride resin into tetrahydrofuran (21 times the mass of copolymerized methyl methacrylate) and stir to dissolve. Then add modified nano titanium dioxide. Then, add trifluoromethylsulfonic acid catalyst (1.8% the mass of copolymerized methyl methacrylate). Stir the reaction at 65°C for 19 hours, then cool naturally to room temperature. Dry the reactants in a vacuum oven to constant weight to obtain a base material masterbatch.
[0022] Example 3
[0023] S1. Add nano titanium dioxide powder to anhydrous ethanol at a mass ratio of 1:10, ultrasonically disperse for 15 minutes, stir at 30°C for 15 minutes, add tetraethyl silicate and 25% ammonia water by mass, heat to 80°C and react for 5 hours, centrifuge and filter after the reaction, wash and dry to obtain modified nano titanium dioxide; wherein the mass ratio of nano titanium dioxide powder to tetraethyl silicate is 3:1, and the volume ratio of anhydrous ethanol to 25% ammonia water by mass is 9:1; S2. At a temperature of 5°C, add tetramethylpiperidinol and triethylamine to tetrahydrofuran in a mass ratio of 1:0.6:22, stir evenly, and uniformly add 1.6 times the mass of tetramethylpiperidinol of acryloyl chloride within 1.5 hours. After the addition is complete, stir and react for 8 hours, then filter and let stand. Recrystallize the filtered product with an excess of 50% by mass of ethanol solution, and dry the recrystallized product in a vacuum oven to constant weight to obtain hindered amino methacrylate. S3. Add 3-aminopropyltriethoxysilane to tetrahydrofuran at a mass ratio of 1:2.6, stir evenly, and prepare a 3-aminopropyltriethoxysilane solution, and let it stand for use; add 2,2'-diallylbisphenol A to tetrahydrofuran at a mass ratio of 1:1.8, stir evenly, and prepare a 2,2'-diallylbisphenol A solution, and let it stand for use; at a temperature of 0°C, add phenyl dichlorophosphate to tetrahydrofuran at a mass ratio of 1:3.5, stir for 0.8h, and then add dichlorophosphoric acid 1.2 times the mass of phenyl ester triethylamine, stir evenly and uniformly add 3-aminopropyltriethoxysilane solution with 3 times the mass of phenyl dichlorophosphate within 2.5 hours, continue stirring for 5 hours after the addition is complete, stir evenly and uniformly add 2,2'-diallylbisphenol A solution with 1.5 times the mass of phenyl dichlorophosphate within 2.5 hours, continue stirring and react for 5 hours after the addition is complete, heat to 35°C after the reaction is complete, continue stirring and react for 12 hours, filter after the reaction is complete, and remove unreacted monomers by rotary evaporation of the filtrate to obtain difunctional phenyl phosphate; S4. Add difunctional phenyl phosphate to dioxane at a mass ratio of 1:3.5, stir evenly to prepare a difunctional phenyl phosphate solution for standby use; place polyvinylidene fluoride in a nitrogen atmosphere. 60 Pre-irradiation was performed in a Co irradiation chamber, and the parameters set during the pre-irradiation process were that the radiation source activity was 30000Ci and the dose rate was 200Gy / min. After the pre-irradiation was completed, the solution was stored at a temperature of 5°C for standby use; under nitrogen protection and a temperature of 55°C, the pre-irradiated polyvinylidene fluoride was added to a bifunctional phenyl phosphate solution with a mass of 22 times that of the polyvinylidene fluoride, and the reaction was stirred for 6 hours. After the reaction was completed, the filtered product was placed in a Soxhlet extractor, washed with toluene and refluxed for 14 hours, and after washing and reflux, the product was vacuum dried to constant weight at a temperature of 85°C to obtain a modified polyvinylidene fluoride resin; S5. Weigh hindered amino methacrylate, methyl methacrylate and allyl triethoxysilane in a molar ratio of 1:2.2:0.35, add hindered amino methacrylate, methyl methacrylate and allyl triethoxysilane to toluene with a mass of 7 times that of methyl methacrylate, add azobisisobutyronitrile with a mass of 0.003 times that of methyl methacrylate after ultrasonic dispersion for 20 minutes, stir and react at a temperature of 90°C for 1.5 hours, and then keep the reaction at a temperature of 65°C for 48 hours to obtain copolymerized methyl methacrylate; S6. Weigh copolymerized methyl methacrylate, modified polyvinylidene fluoride resin and modified nano titanium dioxide in a mass ratio of 7.5:3.5:0.08. First, add copolymerized methyl methacrylate and modified polyvinylidene fluoride resin into tetrahydrofuran (22 times the mass of copolymerized methyl methacrylate) and stir to dissolve. Then add modified nano titanium dioxide. Then, add trifluoromethylsulfonic acid catalyst (2% the mass of copolymerized methyl methacrylate). Stir the reaction at 70°C for 20 hours, then cool naturally to room temperature. Dry the reactants in a vacuum oven to constant weight to obtain a base material masterbatch.
[0024] Example 4
[0025] The only difference from Example 2 is step S6: polymethyl methacrylate, modified polyvinylidene fluoride resin and modified nano titanium dioxide are weighed in a mass ratio of 7:3:0.07, polymethyl methacrylate and modified polyvinylidene fluoride resin are first added to tetrahydrofuran (21 times the mass of polymethyl methacrylate) and stirred to dissolve, and then modified nano titanium dioxide is added, and then trifluoromethylsulfonic acid catalyst (1.8% times the mass of copolymerized methyl methacrylate) is added, and the reaction is stirred at 65°C for 19 hours and then naturally cooled to room temperature, and the reactants are placed in a vacuum oven and dried to constant weight to obtain a substrate masterbatch.
[0026] Example 5
[0027] The only difference from Example 2 is that in step S6: copolymerized methyl methacrylate, polyvinylidene fluoride resin and modified nano titanium dioxide are weighed in a mass ratio of 7:3:0.07, the copolymerized methyl methacrylate and polyvinylidene fluoride resin are first added to tetrahydrofuran (21 times the mass of copolymerized methyl methacrylate) and stirred to dissolve, and then the modified nano titanium dioxide is added, and then 1.8% times the mass of copolymerized methyl methacrylate trifluoromethanesulfonic acid catalyst is added, the reaction is stirred at a temperature of 65°C for 19 hours, and then naturally cooled to room temperature, and the reactants are placed in a vacuum oven and dried to constant weight to obtain a substrate masterbatch.
[0028] Example 6
[0029] The only difference from Example 2 is that in step S6: copolymerized methyl methacrylate, modified polyvinylidene fluoride resin and nano-titanium dioxide are weighed in a mass ratio of 7:3:0.07, the copolymerized methyl methacrylate and the modified polyvinylidene fluoride resin are first added to tetrahydrofuran (21 times the mass of the copolymerized methyl methacrylate) and stirred to dissolve, and then nano-titanium dioxide is added, and then trifluoromethylsulfonic acid catalyst (1.8% times the mass of the copolymerized methyl methacrylate) is added, and the reaction is stirred at a temperature of 65°C for 19 hours and then naturally cooled to room temperature, and the reactants are placed in a vacuum oven and dried to constant weight to obtain a substrate masterbatch.
[0030] Example 7
[0031] The only difference from Example 2 is that in step S6: copolymerized methyl methacrylate and modified polyvinylidene fluoride resin are weighed in a mass ratio of 7:3, and the copolymerized methyl methacrylate and modified polyvinylidene fluoride resin are first added to tetrahydrofuran (21 times the mass of copolymerized methyl methacrylate) and stirred to dissolve, and then trifluoromethylsulfonic acid catalyst (1.8% times the mass of copolymerized methyl methacrylate) is added, and the reaction is stirred at 65°C for 19 hours and then naturally cooled to room temperature, and the reactants are placed in a vacuum oven and dried to constant weight to obtain a substrate masterbatch.
[0032] Example 8
[0033] The only difference from Example 2 is that in step S6: copolymerized methyl methacrylate and modified nano-titanium dioxide are weighed in a mass ratio of 7:0.07, the copolymerized methyl methacrylate is first added to tetrahydrofuran (21 times the mass of the copolymerized methyl methacrylate) and stirred to dissolve, and then the modified nano-titanium dioxide is added, and then the trifluoromethanesulfonic acid catalyst (1.8% of the mass of the copolymerized methyl methacrylate) is added, and the reaction is stirred at a temperature of 65°C for 19 hours and then naturally cooled to room temperature, and the reactants are placed in a vacuum oven and dried to constant weight to obtain a substrate masterbatch.
[0034] Example 9
[0035] The only difference from Example 2 is that in step S6: modified polyvinylidene fluoride resin and modified nano titanium dioxide are weighed according to a mass ratio of 3:0.07, the modified polyvinylidene fluoride resin is first added to tetrahydrofuran (21 times the mass of the modified polyvinylidene fluoride resin) and stirred to dissolve, and then the modified nano titanium dioxide is added, and then 1.8% times the mass of copolymerized methyl methacrylate trifluoromethanesulfonic acid catalyst is added, and the reaction is stirred at a temperature of 65°C for 19 hours and then naturally cooled to room temperature, and the reactants are placed in a vacuum oven and dried to constant weight to obtain a substrate masterbatch.
[0036] Test Example 1 Anti-aging performance test: The base material masterbatch in the above Examples 1 to 9 is used to prepare a polymer film sample by high-temperature multi-layer casting co-extrusion; Test method for tensile fracture resistance: Test the tensile strength of polymer film according to GB / T1040, tensile rate 50mm / min, sample size 75×6.5×3mm 3 ; The polymer film was placed in a xenon lamp weathering test chamber with a set temperature of 40°C, a humidity of 38%, and an irradiation intensity of 230 W / m 2 , the distance is 26cm, and the aging time is 480h to simulate natural light to accelerate aging; after aging, the tensile strength test is carried out again, and the performance retention rate is calculated; Performance retention rate = tensile strength after aging / initial tensile strength; the results are shown in Table 2 below; Table 2 Test results of tensile strength and performance retention rate
[0037] From the comparison of the experimental data of Examples 1 to 3 in Table 2, it can be found that the polymer film prepared by the present invention has good tensile strength, and its mechanical properties are significantly better than those of Examples 4 to 9, and its performance remains good before and after aging, reflecting its excellent anti-aging ability.
[0038] In Examples 4 and 5, since polymethyl methacrylate and polyvinylidene fluoride resins were not modified, their hindered amines and hindered phenols could only act alone, and their anti-aging properties were significantly inferior to those of the synergistic effect of hindered amines and hindered phenols. Although the nano-titanium dioxide was not modified in Example 6, since both the copolymerized methyl methacrylate and the modified polyvinylidene fluoride resin contained siloxane, they could still connect with the nano-titanium dioxide and build a cross-linked network around the nano-titanium dioxide. However, the nano-titanium dioxide was not modified, which resulted in poor dispersibility in the polymer system, so the performance was still reduced. In Example 7, nano titanium dioxide was not added. Although the copolymerization of methyl methacrylate and the siloxane in the modified polyvinylidene fluoride resin can still construct a cross-linked network, the lack of inorganic fillers and cross-linking centers still leads to a decrease in the final performance. In Examples 8 and 9, the copolymerized methyl methacrylate and modified polyvinylidene fluoride resin were removed respectively, which resulted in the same problems as in Examples 4 and 5. In addition, in Example 8, no polyvinylidene fluoride was added, which resulted in a more obvious degradation in the final performance.
[0039] Test Example 2 Surface microstructure defect test: The base material masterbatch in the above-mentioned Examples 1 to 9 is subjected to high-temperature multi-layer cast co-extrusion to obtain a polymer film, and then the polymer film is rolled by a mold roller using a roll-to-roll hot rolling process to obtain a polymer film with a microstructure; during the roll-to-roll hot rolling process, the mold roller temperature is 120° C. and the speed is 1-30 m / min; In the above-mentioned polymer film with microstructure preparation, five 4×4m 2 The microstructural defects on the square area are counted, and the defect rate of each polymer film is calculated. The final statistical result is the average defect rate of the five polymer films. Defect rate = number of microstructure defects / total amount of microstructure; the results are shown in Table 3 below; Table 3 Surface microstructure defect test results
[0040] From the comparison of experimental data in Table 3, it can be found that the defect rates in Examples 4 and 5 increased. The main reason should be that there were more soft segments without modification, and the overall collapse phenomenon was prone to occur. In Example 6, the final defect rate difference was large due to the poor dispersibility of nano-titanium dioxide, resulting in an increase in the final average defect rate. The defect rate in Example 7 increased slightly, mainly because a cross-linking center was constructed between the two polymers, which gave the final product a wider glass transition temperature; The defect rate increase phenomenon is more obvious in Examples 8 and 9, mainly because the glass transition temperature of the monomer is relatively fixed, the contact time is short in the rapid production process, and the glass transition temperature is not reached, resulting in rebound phenomenon.
[0041] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A gap reflective film for improving photoelectric efficiency, It is characterized in that Calculated by mass ratio, it includes the following components: 6.5-7.5 of copolymerized methyl methacrylate, 2.5-3.5 of modified polyvinylidene fluoride resin and 0.06-0.08 of modified nano titanium dioxide; The copolymerized methyl methacrylate is prepared by copolymerizing hindered amino methacrylate, methyl methacrylate and allyl triethoxysilane in a molar ratio of 1:2-2.2:0.25-0.35; The modified polyvinylidene fluoride resin is prepared by pre-irradiating polyvinylidene fluoride and then grafting bifunctional phenyl phosphate.
2. A method for preparing a gap reflective film for improving photoelectric efficiency, It is characterized in that The gap reflective film is prepared by the following steps: S1. Add difunctional phenyl phosphate to dioxane at a mass ratio of 1:3-3.5, stir evenly to prepare a difunctional phenyl phosphate solution for standby use; place polyvinylidene fluoride in a nitrogen atmosphere. 60 Pre-irradiation is performed in a Co irradiation room, and after the pre-irradiation is completed, it is stored at a temperature of 0-5°C for standby use; under nitrogen protection and a temperature of 50-55°C, the pre-irradiated polyvinylidene fluoride is added to a bifunctional phenyl phosphate solution with a mass of 20-22 times that of the polyvinylidene fluoride, and the reaction is stirred for 4-6 hours. After the reaction is completed, the filtered product is placed in a Soxhlet extractor, washed with toluene and refluxed for 12-14 hours, and after washing and reflux, it is vacuum dried to constant weight at a temperature of 80-85°C to obtain a modified polyvinylidene fluoride resin; S2. Weigh hindered amino methacrylate, methyl methacrylate and allyl triethoxysilane in a molar ratio of 1:2-2.2:0.25-0.35, add hindered amino methacrylate, methyl methacrylate and allyl triethoxysilane to toluene with a mass of 6-7 times of methyl methacrylate, add azobisisobutyronitrile with a mass of 0.001-0.003 times of methyl methacrylate after ultrasonic dispersion for 15-20 minutes, stir and react at a temperature of 80-90°C for 1-1.5 hours, and then keep the temperature at 55-65°C for 36-48 hours to obtain copolymerized methyl methacrylate; S3, weighing copolymerized methyl methacrylate, modified polyvinylidene fluoride resin and modified nano titanium dioxide in a mass ratio of 6.5-7.5:2.5-3.5:0.06-0.08, first adding copolymerized methyl methacrylate and modified polyvinylidene fluoride resin to tetrahydrofuran (20-22 times the mass of copolymerized methyl methacrylate) and stirring to dissolve, then adding modified nano titanium dioxide, and then adding trifluoromethylsulfonic acid catalyst (1.5%-2% times the mass of copolymerized methyl methacrylate), stirring and reacting at a temperature of 60-70°C for 18-20h, then naturally cooling to room temperature, and drying the reactants in a vacuum oven to constant weight to obtain a base material masterbatch; S4. The base material masterbatch is subjected to high-temperature multi-layer cast co-extrusion to obtain a polymer film, and then the polymer film is rolled through a mold roller using a roll-to-roll hot rolling process to obtain a polymer film with a microstructure; a reflective layer is prepared on the side of the polymer film surface with a microstructure using a magnetron sputtering deposition method or a vacuum evaporation method, and an adhesive layer is obtained on the other side of the polymer film surface by cast co-extrusion treatment, and then a gap reflective film is obtained by a slitting and winding device.
3. The method for preparing the intermittent reflective film for improving photoelectric efficiency according to claim 2, It is characterized in that The parameters set during the pre-irradiation process are that the radiation source activity is 30000 Ci and the dose rate is 200 Gy / min.
4. The method for preparing the intermittent reflective film for improving photoelectric efficiency according to claim 2, It is characterized in that During the roll-to-roll hot rolling process, the mold roller temperature is 120° C. and the speed is 1-30 m / min.
5. The method for preparing the intermittent reflective film for improving photoelectric efficiency according to claim 2, It is characterized in that The preparation method of the modified nano titanium dioxide is as follows: adding nano titanium dioxide powder to anhydrous ethanol at a mass ratio of 1:10, ultrasonically dispersing for 5-15 minutes, stirring for 5-15 minutes at 20-30° C., adding tetraethyl silicate and 25% ammonia water by mass, heating to 60-80° C. and reacting for 3-5 hours, and after the reaction is completed, washing and drying after centrifugal filtration to obtain the modified nano titanium dioxide.
6. The method for preparing the interstitial reflective film for improving photoelectric efficiency according to claim 5, It is characterized in that The mass ratio of the nano titanium dioxide powder to tetraethyl silicate is 2.5-3:1, and the volume ratio of the anhydrous ethanol to 25% ammonia water is 8-9:
1.
7. The method for preparing the intermittent reflective film for improving photoelectric efficiency according to claim 2, It is characterized in that The preparation method of the hindered amino methacrylate comprises the following steps: adding tetramethyl piperidinol and triethylamine to tetrahydrofuran at a mass ratio of 1:0.4-0.6:20-22 at a temperature of 0-5°C, stirring evenly, and uniformly dropping acryloyl chloride in an amount of 1.4-1.6 times the mass of tetramethyl piperidinol within 1-1.5 hours, stirring the mixture for reaction for 6-8 hours after the dropping is completed, and then standing and filtering the mixture, recrystallizing the filtered product with an excess ethanol solution of 50% by mass, and drying the recrystallized product in a vacuum oven to a constant weight, thereby obtaining the hindered amino methacrylate.
8. The method for preparing the intermittent reflective film for improving photoelectric efficiency according to claim 2, It is characterized in that The preparation method of the bifunctional phenyl phosphate is as follows: 3-aminopropyl triethoxysilane is added to tetrahydrofuran at a mass ratio of 1:2.4-2.6, stirred evenly, configured to be a 3-aminopropyl triethoxysilane solution, and allowed to stand for use; 2,2'-diallyl bisphenol A is added to tetrahydrofuran at a mass ratio of 1:1.5-1.8, stirred evenly, configured to be a 2,2'-diallyl bisphenol A solution, and allowed to stand for use; under the condition of a temperature of -5-0°C, phenyl dichlorophosphate is added to tetrahydrofuran at a mass ratio of 1:3.2-3.5, stirred for 0.5-0.8h, and then added Add triethylamine in an amount of 1 to 1.2 times the mass of phenyl dichlorophosphate, stir evenly, and uniformly add 3-aminopropyltriethoxysilane solution in an amount of 2.8 to 3 times the mass of phenyl dichlorophosphate over 2 to 2.5 hours. After the addition is complete, continue stirring for 3 to 5 hours. Stir evenly, and uniformly add 2,2'-diallylbisphenol A solution in an amount of 1.3 to 1.5 times the mass of phenyl dichlorophosphate over 2 to 2.5 hours. After the addition is complete, continue stirring to react for 3 to 5 hours. After the reaction is complete, heat to 25 to 35°C, continue stirring to react for 8 to 12 hours. After the reaction is complete, filter and evaporate the filtrate to remove unreacted monomers to obtain difunctional phenyl phosphate.
Citation Information
Patent Citations
Preparation method of polyvinylidene fluoride-based thin film
CN104327433A
TiO2 nanoparticle modified PVDF (Polyvinylidene Fluoride) / PMMA composite thin film
CN106905648A
Wavelength conversion member, backlight unit, image display device, curable composition and cured product
CN111919142A
Super-weather-resistant reflective film and preparation method thereof
CN114634647A
Mono-layer pvdf film and preparation method thereof
KR1020110119417A