High-elasticity compressible polylactic acid micro-nano fiber aerogel material as well as preparation method and application thereof
Through in-situ phase interfacial capacity-enhancing and aqueous polyurethane crosslinking technology of multi-element ring chain extender, a high-elastic compressible polylactic acid micro-nanofiber aerogel material was prepared, which solved the poor oil absorption selectivity of polylactic acid micro-nanofiber materials in oil-water separation. and environmental pollution problems have achieved efficient and long-term oil-water separation performance and reusable materials.
Patent Information
- Application Number
- CN202411145878.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-20
AI Technical Summary
The existing polylactic acid micro-nanofiber materials have problems such as poor oil absorption selectivity, low oil absorption capacity, poor oil retention rate, difficulty in recycling and poor recycling in oil-water separation applications. The electrospinning oil-water separation fiber membrane depends on the high non-degradable Molecular materials, causing secondary pollution of the environment.
High-pressure electrospinning is performed by using multi-ring chain extender in situ phase interface to increase the capacity of polylactic acid blended thermoplastic elastomer to form tough polylactic acid micro-nanofibers, and disperse them into tert-butanol aqueous solution through a homogenous disperser. , using aqueous polyurethane as a crosslinking agent to prepare highly elastic compressible polylactic acid micro-nanofiber aerogel materials to improve their mechanical properties and lipophilicity.
The prepared high elastic compressible polylactic acid micro-nanofiber aerogel material has excellent elastic recovery, high compressibility, high mechanical strength, large specific surface area, high porosity, superhydrophobicity and high lipophilicity, achieving Efficient oil-water separation performance and easy to recycle and reusable, solving the problems of material brittleness and environmental pollution.
Smart Images

Figure CN119019829A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of aerogel materials, in particular to a highly elastic and compressible polylactic acid micro-nano fiber aerogel material and a preparation method and application thereof. Background Art
[0002] In recent years, oily wastewater pollution caused by factory emissions, marine transportation and oil exploration has become increasingly common, which not only has a negative impact on the economy, but also causes extremely serious ecological damage. At the same time, it has caused irreversible harm to the environment, organisms and human health. At present, the discharge of oily wastewater continues to deteriorate the water environment. In order to solve the problem of waste oil pollution, a lot of research has been done on the methods and materials for oil-water separation. Traditional oil-water separation methods include gravity method, centrifugation method, air flotation method, biological treatment method and fiber membrane separation method. Fiber membrane separation method has the advantages of energy saving, high cost performance and easy mass production. At present, the preparation methods of fiber membranes for oil-water separation mainly include metal mesh method, sol-gel method and electrospinning method. Electrospinning is a simple and inexpensive method for preparing micro-nano fiber membranes. Micro / nano fiber membranes prepared by electrospinning have excellent filtration and adsorption capabilities due to their superior properties such as light weight, high porosity and large specific surface area, and show great potential in oil-water separation. However, most electrospun oil-water separation fiber membranes currently rely on non-degradable polymer materials synthesized from coal, petroleum and natural gas chemical raw materials, which brings secondary pollution to the environment. Therefore, it is crucial to prepare an efficient and green oil-water separation material using renewable, degradable and environmentally friendly raw materials.
[0003] Polylactic acid (PLA) is a thermoplastic biodegradable polymer material made by polymerizing small molecule lactic acid from biomass raw materials such as corn stalks, rice stalks, wheat stalks, sugarcane and cassava through microbial fermentation of vegetation. PLA has excellent biodegradability, biocompatibility, non-toxicity and renewability. Compared with current petrochemical plastics, it is more in line with the concept of sustainable development and economic circulation. At the same time, PLA has excellent hydrophobic properties, so the use of PLA to develop oil-water separation fiber membrane materials has significant advantages. Zhu Ranran et al. used PLA / PCL to prepare nanofiber membranes by electrospinning. When the PLA / (polycaprolactone) PCL blending ratio was 7:3, the prepared PLA nanofiber membranes had oil retention rates of 76.16%, 70.83% and 67.17% for motor oil, peanut oil and rapeseed oil, respectively (New Chemical Materials (2023), 51(04): 137-141). However, the mechanical properties of the product and the reusability of PLA-based adsorption materials were not analyzed. Meng Linlin et al. prepared a porous hollow polylactic acid nanofiber membrane using coaxial electrospinning technology. The tensile breaking strength, tearing, air permeability, and moisture permeability of the fiber membrane were tested. It was found that the tensile breaking strength of the porous hollow polylactic acid nanofiber membrane was 36.250 cN, the elongation at break was 3.238 mm, and the tearing strength of the porous hollow PLA nanofiber membrane was 90.16 cN. In the test of the adsorption performance of peanut oil, silicone oil, and motor oil, the oil retention rates of the porous hollow PLA nanofiber membrane were 42.51%, 37.89%, and 49.49%, respectively. Due to the brittleness of polylactic acid, the mechanical properties of the porous hollow PLA nanofiber membrane are not ideal, which leads to poor reusability of the porous hollow PLA nanofiber membrane in oil-water separation applications (Modern Textile Technology (2019), 27(3): 1-4). The application of polylactic acid micro-nano fiber materials in the field of oil-water separation mainly has problems such as poor oil absorption selectivity, low oil absorption capacity, poor oil retention rate, difficulty in recovery and poor recyclability, which seriously restricts their practical application. Therefore, it is urgent to develop a polylactic acid micro-nano fiber oil-water separation material with high mechanical properties and long-lasting effect.
[0004] Aerogel is a three-dimensional porous material with extremely low density, high porosity, high pore volume and adjustable mechanical properties. This structure is conducive to the storage of adsorbed oil and is an ideal material for oil-water separation. Biomass-based aerogels have the environmental protection, renewable and degradable characteristics of biomass materials and the advantages of three-dimensional porous structures. They have unique advantages in oil-water separation and have attracted widespread attention from researchers. For example, cellulose aerogel has an excellent porous structure and is currently widely used in the field of oil-water separation. However, natural cellulose has hydrophilic properties and requires complex hydrophobic modification and lipophilic modification or compounding to give it good oil absorption properties. At the same time, most biomass-based polymers lack intermolecular cross-linking in aqueous solution, and the aerogels prepared therefrom are difficult to form or have poor mechanical properties, which leads to unsatisfactory use of aerogel materials in aqueous solution environments. The invention prepares a highly elastic and compressible polylactic acid micro-nano fiber aerogel material, which combines the advantages of micro-nano fiber and aerogel material. First, a polycyclic chain extender is used to in-situ phase interface compatibilize polylactic acid blended thermoplastic elastomer to obtain a polylactic acid blended thermoplastic elastomer spinning precursor, and then high-voltage electrostatic spinning is used to obtain toughened polylactic acid micro-nano fiber; a homogenizer is used to crush and disperse the toughened polylactic acid micro-nano fiber into a tert-butyl alcohol aqueous solution to obtain a micro-nano fiber dispersion, and then the micro-nano fiber dispersion is used as a gel framework, and aqueous polyurethane is used as a micro-nano fiber crosslinking agent to prepare a toughened polylactic acid micro-nano fiber gel, and the aqueous polyurethane can synergistically improve the hydrophobicity and lipophilicity of the aerogel; finally, a highly elastic and compressible polylactic acid micro-nano fiber aerogel material is obtained by vacuum freeze drying. The prepared polylactic acid micro-nano fiber aerogel material has excellent elastic recovery, high compressibility, high mechanical strength, large specific surface area, high porosity, super hydrophobicity and lipophilicity, and has an efficient oil absorption effect. At the same time, in situ interfacial expansion significantly improved the mechanical properties of polylactic acid fibers and micro-nano fiber aerogels. The micro-nano fiber aerogel material exhibited long-term oil-water separation performance and was easy to recycle and reuse. Summary of the invention
[0005] The object of the present invention is to provide a method for preparing a highly elastic and compressible polylactic acid micro-nano fiber aerogel material to solve the problems raised in the above background technology.
[0006] In a first aspect, the present invention provides a highly elastic and compressible polylactic acid micro-nano fiber aerogel material, characterized in that the highly elastic and compressible polylactic acid micro-nano fiber aerogel material is a three-dimensional network composed of toughened polylactic acid micro-nano fibers and aqueous polyurethane, wherein the toughened polylactic acid micro-nano fibers are the gel frame and the aqueous polyurethane is used as a cross-linked network.
[0007] In a second aspect, the present invention provides a method for preparing a highly elastic and compressible polylactic acid micro-nano fiber aerogel material, which comprises the following steps:
[0008] S1: dissolving polylactic acid and thermoplastic elastomer in a compound solvent to obtain a polymer solution, adding a polycyclic chain extender to the polymer solution, ultrasonically dispersing the solution for in-situ phase interface volume expansion, and vacuum degassing to obtain a spinning precursor solution;
[0009] S2: The spinning precursor solution is subjected to high-voltage electrospinning to obtain toughened polylactic acid micro-nanofibers;
[0010] S3: Use a homogenizer to disperse the toughened polylactic acid micro-nano fibers into a tert-butyl alcohol aqueous solution, add aqueous polyurethane as a cross-linking agent into the aqueous solution to obtain a toughened polylactic acid micro-nano fiber hydrogel, and vacuum freeze-dry the hydrogel material to obtain a highly elastic and compressible polylactic acid micro-nano fiber aerogel material.
[0011] Preferably, the compound solvent in step S1 is composed of tetrahydrofuran and N,N'-dimethylformamide, and the mass ratio is 1-3:1; the amount of the polylactic acid and the thermoplastic elastomer in the compound solvent in step S1 is 10-15wt%, and the mass ratio of the polylactic acid and the thermoplastic elastomer is 3:2; the amount of the polycyclic chain extender in the polylactic acid and the thermoplastic elastomer in step S1 is 0.5-2wt%.
[0012] Preferably, the ultrasonic dispersion treatment conditions in step S1 are: the power is set to 500-1200 W, and the treatment time is 1-10 h.
[0013] Preferably, the thermoplastic elastomer in step S1 is at least one of aliphatic polyether urethane TPU, aromatic polyether urethane TPU, aliphatic polycarbonate urethane TPU, and aromatic polycarbonate urethane TPU, and the polycyclic chain extender is styrene-glycidyl methacrylate oligomer.
[0014] Preferably, the high-voltage electrospinning parameters in step S2 are set as follows: high-voltage electrostatic 10-20 kV, a pushing speed of 1-5 ml / h, a receiving distance of 8-15 cm, and a spinning needle according to any one of the models 19G, 20G, 21G, 22G, and 23G.
[0015] Preferably, in step S3, the amount of the toughened polylactic acid micro-nano fibers in the tert-butyl alcohol aqueous solution is 0.5-2 wt %.
[0016] Preferably, the tert-butanol aqueous solution in step S3 is composed of tert-butanol and aqueous solution in a mass ratio of 1:4, and the processing conditions of the homogenizer are: 10000-20000 rpm, and the processing time is 0.5-2h.
[0017] Preferably, in step S3, the mass ratio of the waterborne polyurethane to the toughened polylactic acid micro-nanofibers is 0.1-1:1, and the waterborne polyurethane is at least one of aromatic isocyanate type WPU, aliphatic isocyanate type WPU, and alicyclic isocyanate type WPU.
[0018] In a third aspect, the present invention provides an application of a highly elastic and compressible polylactic acid micro-nano fiber aerogel material, and an application of a highly elastic and compressible polylactic acid nanofiber aerogel material prepared using the aforementioned highly elastic and compressible polylactic acid nanofiber aerogel material in the field of oil-water separation.
[0019] The highly elastic and compressible polylactic acid micro-nano fiber aerogel material of the present invention has the following beneficial effects:
[0020] (1) The structure with the advantages of both micro-nano fibers and aerogels was constructed by using polylactic acid electrospinning micro-nano fibers and aerogel molding, so as to prepare polylactic acid micro-nano fiber aerogel materials with excellent elastic recovery, high compressibility, high mechanical strength, large specific surface area, high porosity, super hydrophobicity and high lipophilicity.
[0021] (2) In the construction stage of polylactic acid electrospinning micro-nanofibers, the epoxy groups contained in the polycyclic chain extender molecules are used, which have high reactivity. During the in-situ compatibilization reaction, the epoxy groups open the ring and react with the functional groups (-OH and -COOH) of polylactic acid and thermoplastic elastomer to form new -CO-ester chemical bonds, thus realizing the covalent bridging between polylactic acid, thermoplastic elastomer and polycyclic chain extender. The polycyclic chain extender is used for in-situ phase interface compatibilization and synergistic electrospinning to prepare toughened polylactic acid micro-nanofibers. In-situ phase interface compatibilization significantly improves the mechanical properties of polylactic acid fibers and polylactic acid micro-nanofiber aerogel materials. In the construction of polylactic acid micro-nanofiber aerogel, water-based polyurethane as a cross-linking agent of the gel framework further improves the mechanical properties of polylactic acid micro-nanofiber aerogels, and significantly improves the lipophilicity of polylactic acid micro-nanofibers.
[0022] (3) Using renewable, degradable and environmentally friendly polylactic acid as raw material, polylactic acid electrospun micro-nano fibers and aerogel molding are used to construct an elastic compressible polylactic acid micro-nano fiber aerogel material with high oil absorption capacity and long-lasting oil absorption effect. The present invention solves the problem of poor product application effect caused by the brittleness of polylactic acid fibers, and solves the problem that electrospun oil-water separation fiber membranes rely on non-degradable polymer materials synthesized from coal, petroleum and natural gas chemical raw materials, as well as the secondary environmental pollution caused by oil-water separation materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The scanning electron microscope image and water contact angle photo of toughened polylactic acid micro-nanofibers;
[0024] Figure 2 This is a scanning electron microscope image of a highly elastic and compressible polylactic acid micro-nano fiber aerogel material;
[0025] Figure 3 The contact angles of highly elastic and compressible polylactic acid micro-nano fiber aerogel materials with water and oil;
[0026] Figure 4 The compression rebound stress-strain diagram and height retention rate diagram of highly elastic compressible polylactic acid micro-nano fiber aerogel material;
[0027] Figure 5 This is the infrared spectrum of highly elastic and compressible polylactic acid micro-nano fiber aerogel material;
[0028] Figure 6 The oil absorption in water and cyclic adsorption performance diagram of highly elastic and compressible polylactic acid micro-nano fiber aerogel material;
[0029] Figure 7 This is a dynamic separation data diagram of an immiscible oil-water mixture of a highly elastic and compressible polylactic acid micro-nano fiber aerogel material;
[0030] Figure 8 This is the mixed-phase oil-water emulsion separation data diagram of highly elastic and compressible polylactic acid micro-nanofiber aerogel material. DETAILED DESCRIPTION
[0031] The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, but should not be construed as limiting the present invention.
[0032] In a first aspect, in one embodiment of the present invention, a highly elastic and compressible polylactic acid micro-nanofiber aerogel material is provided, which is composed of a three-dimensional network composed of toughened polylactic acid micro-nanofiber and aqueous polyurethane, wherein the toughened polylactic acid micro-nanofiber is a gel framework and the aqueous polyurethane is a cross-linked network.
[0033] In the second aspect, the embodiment of the present invention provides a method for preparing a highly elastic and compressible polylactic acid micro-nano fiber aerogel material, wherein a polylactic acid blended thermoplastic elastomer is in-situ phase-interface-compatibilized in a compound solvent using a multicyclic chain extender to obtain a polylactic acid blended thermoplastic elastomer spinning precursor; the spinning precursor is subjected to high-voltage electrostatic spinning to obtain toughened polylactic acid micro-nano fibers; the toughened polylactic acid micro-nano fibers crushed by a homogenizer are dispersed in a tert-butyl alcohol aqueous solution to obtain a micro-nano fiber dispersion, which is then used as a gel framework, and aqueous polyurethane is used as a micro-nano fiber crosslinking agent to prepare a toughened polylactic acid micro-nano fiber gel, and finally a highly elastic and compressible polylactic acid micro-nano fiber aerogel material is obtained by vacuum freeze drying. The polylactic acid micro-nano fiber aerogel material has the advantages of both polylactic acid micro-nano fibers and aerogel materials, and has a high specific surface area of micro-nano fibers and a high porosity of aerogels. In-situ interfacial compatibilization significantly improves the mechanical properties of polylactic acid fibers and polylactic acid micro-nano fiber aerogel materials. The highly elastic compressible polylactic acid micro-nano fiber aerogel material has excellent elastic recovery, high compressibility, high mechanical strength, large specific surface area, high porosity, super hydrophobicity and high oleophilicity, and is applied in the field of oil-water separation to show efficient oil absorption effect. The highly elastic compressible polylactic acid micro-nano fiber aerogel material shows long-term oil-water separation performance, and is easy to recycle and reuse.
[0034] Specifically, the highly elastic compressible polylactic acid micro-nano fiber aerogel material comprises the following steps:
[0035] S1: dissolving polylactic acid and thermoplastic elastomer in a composite solvent prepared by tetrahydrofuran and N,N'-dimethylformamide in a mass ratio of 1 to 3:1, wherein the amount of polylactic acid and thermoplastic elastomer in the composite solvent is 10 to 15 wt%, and the mass ratio of polylactic acid and thermoplastic elastomer is 3:2; adding a polycyclic chain extender to the polymer solution, wherein the amount of the polycyclic chain extender in the polylactic acid and thermoplastic elastomer is 0.5 to 2 wt%. Ultrasonic dispersion of the solution is performed for in-situ phase interface compatibilization, and vacuum degassing is performed to obtain a spinning precursor solution.
[0036] S2: The spinning precursor solution is subjected to high-voltage electrospinning to obtain toughened polylactic acid micro-nanofibers;
[0037] S3: Use a homogenizer to disperse the toughened polylactic acid micro-nano fibers into a tert-butanol aqueous solution. The tert-butanol aqueous solution is composed of tert-butanol and an aqueous solution in a mass ratio of 1:4. The amount of toughened polylactic acid micro-nano fibers in the tert-butanol aqueous solution is 0.5-2wt%; continue to add water-based polyurethane as a cross-linking agent to the tert-butanol aqueous solution, the mass ratio of the water-based polyurethane to the toughened polylactic acid micro-nano fibers is 0.1-1:1, and a toughened polylactic acid micro-nano fiber hydrogel is obtained. The hydrogel material is vacuum freeze-dried to obtain a highly elastic and compressible polylactic acid micro-nano fiber aerogel material.
[0038] In a preferred embodiment of the present invention, the thermoplastic elastomer is at least one of aliphatic polyether urethane TPU, aromatic polyether urethane TPU, aliphatic polycarbonate urethane TPU, and aromatic polycarbonate urethane TPU, but is not limited thereto; the polycyclic chain extender is styrene-glycidyl methacrylate oligomer.
[0039] In a preferred embodiment of the present invention, in the above steps, the ultrasonic dispersion treatment conditions are: the power is set to 500-1200W, and the treatment time is 1-10h.
[0040] In a preferred embodiment of the present invention, in the above steps, the high-voltage electrospinning parameters are set as follows: high-voltage electrostatic 10-20 kV, a pushing speed of 1-5 ml / h, a receiving distance of 8-15 cm, and a spinning needle according to any one of the models 19G, 20G, 21G, 22G, and 23G, but not limited thereto.
[0041] In a preferred embodiment of the present invention, in the above steps, the processing conditions of the homogenizer are: 10000-20000 rpm, and the processing time is 0.5-2h.
[0042] In a preferred embodiment of the present invention, in the above steps, the waterborne polyurethane is at least one of aromatic isocyanate type WPU, aliphatic isocyanate type WPU, and alicyclic isocyanate type WPU, but is not limited thereto.
[0043] In the third aspect, the present invention provides an application of a highly elastic compressible polylactic acid micro-nano fiber aerogel material prepared by the aforementioned method in the field of oil-water separation. The highly elastic compressible polylactic acid micro-nano fiber aerogel material has excellent elastic recovery, high compressibility, high mechanical strength, large specific surface area, high porosity, super hydrophobicity and high lipophilicity, and is applied to the field of oil-water separation to show efficient oil absorption effect. The highly elastic compressible polylactic acid micro-nano fiber aerogel material exhibits long-term oil-water separation performance, and is also easy to recycle and reusable.
[0044] The following embodiments are some specific implementation cases of the present invention in practical applications, but are not limited thereto.
[0045] Embodiment 1:
[0046] This embodiment provides a method for preparing a highly elastic and compressible polylactic acid micro-nano fiber aerogel material, which specifically includes the following steps:
[0047] Step 1: Preparation of in-situ phase interface compatibilized spinning precursor solution
[0048] Polylactic acid and aliphatic polyether urethane TPU are dissolved in a compound solvent obtained by tetrahydrofuran and N, N'-dimethylformamide in a mass ratio of 2:1, the amount of polylactic acid and aliphatic polyether urethane TPU in the compound solvent is 14wt%, and the mass ratio of polylactic acid to thermoplastic elastomer is 3:2; chain extender styrene-methacrylate glycidyl oligomer is added to the polymer solution, and the amount of styrene-methacrylate glycidyl oligomer in polylactic acid and thermoplastic elastomer is 1wt%. The solution is ultrasonically dispersed for in-situ phase interface compatibilization, the ultrasonic power is set to 1000W, and the processing time is 5h. Vacuum degassing is performed to obtain a spinning precursor solution.
[0049] Step 2: Strengthening polylactic acid micro-nanofibers
[0050] The spinning precursor liquid is loaded into the syringe for high-voltage electrospinning. The high voltage electrostatic is 15kV, the pushing speed is 2ml / h, the receiving distance is 10cm, and the spinning needle is 20G according to the model to obtain toughened polylactic acid micro-nano fibers.
[0051] Step 3: Preparation of highly elastic and compressible polylactic acid micro-nanofiber aerogel
[0052] The toughened polylactic acid micro-nano fibers are dispersed into a tert-butanol aqueous solution using a homogenizer. The tert-butanol aqueous solution is composed of tert-butanol and an aqueous solution in a mass ratio of 1:4. The amount of toughened polylactic acid micro-nano fibers in the tert-butanol aqueous solution is 1wt%. The homogenizer treatment conditions are: 15000rpm, and the treatment time is 1h. The tert-butanol aqueous solution is continued to add aliphatic isocyanate type WPU as a cross-linking agent, and the mass ratio of aliphatic isocyanate type WPU to toughened polylactic acid micro-nano fibers is 0.5:1 to obtain toughened polylactic acid micro-nano fiber hydrogel. The hydrogel material is vacuum freeze-dried to obtain a highly elastic and compressible polylactic acid micro-nano fiber aerogel material.
[0053] Embodiment 2:
[0054] This embodiment provides a method for preparing a highly elastic and compressible polylactic acid micro-nano fiber aerogel material, which specifically includes the following steps:
[0055] Step 1: Preparation of in-situ phase interface compatibilized spinning precursor solution
[0056] Polylactic acid and aromatic polyether urethane TPU are dissolved in a compound solvent obtained by tetrahydrofuran and N, N'-dimethylformamide in a mass ratio of 3:1, the amount of polylactic acid and aromatic polyether urethane TPU in the compound solvent is 10wt%, and the mass ratio of polylactic acid to thermoplastic elastomer is 3:2; chain extender styrene-methacrylate glycidyl oligomer is added to the polymer solution, and the amount of styrene-methacrylate glycidyl oligomer in polylactic acid and thermoplastic elastomer is 1.5wt%. The solution is ultrasonically dispersed for in-situ phase interface compatibilization, the ultrasonic power is set to 1500W, and the processing time is 3h. Vacuum degassing is performed to obtain a spinning precursor solution.
[0057] Step 2: Strengthening polylactic acid micro-nanofibers
[0058] The spinning precursor liquid is loaded into the syringe for high-voltage electrospinning. The high voltage electrostatic is 12kV, the pushing speed is 1.5ml / h, the receiving distance is 9cm, and the spinning needle is model 22G to obtain toughened polylactic acid micro-nano fibers.
[0059] Step 3: Preparation of highly elastic and compressible polylactic acid micro-nanofiber aerogel
[0060] The toughened polylactic acid micro-nano fibers are dispersed into a tert-butanol aqueous solution using a homogenizer. The tert-butanol aqueous solution is composed of tert-butanol and an aqueous solution in a mass ratio of 1:4. The amount of toughened polylactic acid micro-nano fibers in the tert-butanol aqueous solution is 1.5wt%. The processing conditions of the homogenizer are: 10000rpm, and the processing time is 1h. The tert-butanol aqueous solution is continued to add aromatic isocyanate type WPU as a cross-linking agent, and the mass ratio of aromatic isocyanate type WPU to toughened polylactic acid micro-nano fibers is 0.2:1 to obtain toughened polylactic acid micro-nano fiber hydrogel. The hydrogel material is vacuum freeze-dried to obtain a highly elastic and compressible polylactic acid micro-nano fiber aerogel material.
[0061] Embodiment 3:
[0062] This embodiment provides a method for preparing a highly elastic and compressible polylactic acid micro-nano fiber aerogel material, which specifically includes the following steps:
[0063] Step 1: Preparation of in-situ phase interface compatibilized spinning precursor solution
[0064] Polylactic acid and aliphatic polycarbonate urethane TPU are dissolved in a compound solvent obtained by tetrahydrofuran and N, N'-dimethylformamide in a mass ratio of 2:1, the amount of polylactic acid and aliphatic polycarbonate urethane TPU in the compound solvent is 14wt%, and the mass ratio of polylactic acid to thermoplastic elastomer is 3:2; chain extender styrene-methacrylate glycidyl oligomer is added to the polymer solution, and the amount of styrene-methacrylate glycidyl oligomer in polylactic acid and thermoplastic elastomer is 1.6wt%. The solution is ultrasonically dispersed for in-situ phase interface compatibilization, the ultrasonic power is set to 1100W, and the processing time is 8h. Vacuum degassing is performed to obtain a spinning precursor solution.
[0065] Step 2: Strengthening polylactic acid micro-nanofibers
[0066] The spinning precursor liquid is loaded into the syringe for high-voltage electrospinning. The high voltage electrostatic is 13kV, the pushing speed is 2.2ml / h, the receiving distance is 12cm, and the spinning needle is model 22G to obtain toughened polylactic acid micro-nano fibers.
[0067] Step 3: Preparation of highly elastic and compressible polylactic acid micro-nanofiber aerogel
[0068] The toughened polylactic acid micro-nanofibers were dispersed into a tert-butanol aqueous solution using a homogenizer. The tert-butanol aqueous solution was composed of tert-butanol and an aqueous solution in a mass ratio of 1:4. The amount of toughened polylactic acid micro-nanofibers in the tert-butanol aqueous solution was 1.7wt%. The homogenizer treatment conditions were 18000rpm and 1h. The tert-butanol aqueous solution was then added with alicyclic isocyanate type WPU as a cross-linking agent. The mass ratio of alicyclic isocyanate type WPU to toughened polylactic acid micro-nanofibers was 0.6:1 to obtain toughened polylactic acid micro-nanofibers hydrogel. The hydrogel material was vacuum freeze-dried to obtain a highly elastic and compressible polylactic acid micro-nanofibers aerogel material.
[0069] Embodiment 4:
[0070] This embodiment provides a method for preparing a highly elastic and compressible polylactic acid micro-nano fiber aerogel material, which specifically includes the following steps:
[0071] Step 1: Preparation of in-situ phase interface compatibilized spinning precursor solution
[0072] Polylactic acid and aromatic polycarbonate urethane TPU are dissolved in a compound solvent prepared by tetrahydrofuran and N,N'-dimethylformamide at a mass ratio of 1.5:1, the amount of polylactic acid and aromatic polycarbonate urethane TPU in the compound solvent is 11wt%, and the mass ratio of polylactic acid to thermoplastic elastomer is 3:2; chain extender styrene-methacrylate glycidyl oligomer is added to the polymer solution, and the amount of styrene-methacrylate glycidyl oligomer in polylactic acid and thermoplastic elastomer is 1.8wt%. The solution is ultrasonically dispersed for in-situ phase interface compatibilization, the ultrasonic power is set to 900W, and the processing time is 6h. Vacuum degassing is performed to obtain a spinning precursor solution.
[0073] Step 2: Strengthening polylactic acid micro-nanofibers
[0074] The spinning precursor liquid is loaded into the syringe for high-voltage electrospinning. The high-voltage electrostatic is 14kV, the pushing speed is 2.3ml / h, the receiving distance is 9cm, and the spinning needle is model 23G to obtain toughened polylactic acid micro-nano fibers.
[0075] Step 3: Preparation of highly elastic and compressible polylactic acid micro-nanofiber aerogel
[0076] The toughened polylactic acid micro-nano fibers are dispersed into a tert-butanol aqueous solution using a homogenizer. The tert-butanol aqueous solution is composed of tert-butanol and an aqueous solution in a mass ratio of 1:4. The amount of toughened polylactic acid micro-nano fibers in the tert-butanol aqueous solution is 1.8wt%. The homogenizer treatment conditions are: 19000rpm, and the treatment time is 1.2h. The tert-butanol aqueous solution is continued to add aromatic isocyanate type WPU as a cross-linking agent, and the mass ratio of aromatic isocyanate type WPU to toughened polylactic acid micro-nano fibers is 0.7:1 to obtain toughened polylactic acid micro-nano fiber hydrogel. The hydrogel material is vacuum freeze-dried to obtain a highly elastic and compressible polylactic acid micro-nano fiber aerogel material.
[0077] Embodiment 5:
[0078] This embodiment provides a method for preparing a highly elastic and compressible polylactic acid micro-nano fiber aerogel material, which specifically includes the following steps:
[0079] Step 1: Preparation of in-situ phase interface compatibilized spinning precursor solution
[0080] Polylactic acid and aliphatic polyether urethane TPU are dissolved in a compound solvent obtained by tetrahydrofuran and N, N'-dimethylformamide at a mass ratio of 2.5:1, the amount of polylactic acid and aliphatic polyether urethane TPU in the compound solvent is 14wt%, and the mass ratio of polylactic acid to thermoplastic elastomer is 3:2; chain extender styrene-methacrylate glycidyl oligomer is added to the polymer solution, and the amount of styrene-methacrylate glycidyl oligomer in polylactic acid and thermoplastic elastomer is 1.9wt%. The solution is ultrasonically dispersed for in-situ phase interface compatibilization, the ultrasonic power is set to 1150W, and the processing time is 9h. Vacuum degassing is performed to obtain a spinning precursor solution.
[0081] Step 2: Strengthening polylactic acid micro-nanofibers
[0082] The spinning precursor liquid is loaded into the syringe for high-voltage electrospinning. The high voltage electrostatic is 19kV, the pushing speed is 1.1ml / h, the receiving distance is 14cm, and the spinning needle is 20G according to the model to obtain toughened polylactic acid micro-nano fibers.
[0083] Step 3: Preparation of highly elastic and compressible polylactic acid micro-nanofiber aerogel
[0084] The toughened polylactic acid micro-nanofibers were dispersed into a tert-butanol aqueous solution using a homogenizer. The tert-butanol aqueous solution was composed of tert-butanol and an aqueous solution in a mass ratio of 1:4. The amount of toughened polylactic acid micro-nanofibers in the tert-butanol aqueous solution was 1.9wt%. The homogenizer treatment conditions were 19500rpm and 1.6h. The tert-butanol aqueous solution was then added with aliphatic isocyanate type WPU as a cross-linking agent. The mass ratio of aliphatic isocyanate type WPU to toughened polylactic acid micro-nanofibers was 0.8:1 to obtain toughened polylactic acid micro-nanofibers hydrogel. The hydrogel material was vacuum freeze-dried to obtain a highly elastic and compressible polylactic acid micro-nanofibers aerogel material.
[0085] Embodiment 6:
[0086] This embodiment provides a method for preparing a highly elastic and compressible polylactic acid micro-nano fiber aerogel material, which specifically includes the following steps:
[0087] Step 1: Preparation of in-situ phase interface compatibilized spinning precursor solution
[0088] Polylactic acid and aromatic polycarbonate urethane TPU are dissolved in a compound solvent obtained by tetrahydrofuran and N, N'-dimethylformamide in a mass ratio of 3:1, the amount of polylactic acid and aromatic polyether urethane TPU in the compound solvent is 15wt%, and the mass ratio of polylactic acid to thermoplastic elastomer is 3:2; chain extender styrene-methacrylate glycidyl oligomer is added to the polymer solution, and the amount of styrene-methacrylate glycidyl oligomer in polylactic acid and thermoplastic elastomer is 2wt%. The solution is ultrasonically dispersed for in-situ phase interface compatibilization, the ultrasonic power is set to 1200W, and the processing time is 10h. And vacuum degassing is carried out to obtain a spinning precursor solution.
[0089] Step 2: Strengthening polylactic acid micro-nanofibers
[0090] The spinning precursor liquid is loaded into the syringe for high-voltage electrospinning. The high voltage electrostatic is 20kV, the pushing speed is 5ml / h, the receiving distance is 15cm, and the spinning needle is model 19G to obtain toughened polylactic acid micro-nano fibers.
[0091] Step 3: Preparation of highly elastic and compressible polylactic acid micro-nanofiber aerogel
[0092] The toughened polylactic acid micro-nano fibers are dispersed into a tert-butanol aqueous solution using a homogenizer. The tert-butanol aqueous solution is composed of tert-butanol and an aqueous solution in a mass ratio of 1:4. The amount of toughened polylactic acid micro-nano fibers in the tert-butanol aqueous solution is 2wt%. The homogenizer treatment conditions are: 20,000 rpm, and the treatment time is 2 h. The tert-butanol aqueous solution is continued to add alicyclic isocyanate type WPU as a cross-linking agent, and the mass ratio of alicyclic isocyanate type WPU to toughened polylactic acid micro-nano fibers is 1:1 to obtain toughened polylactic acid micro-nano fiber hydrogel. The hydrogel material is vacuum freeze-dried to obtain a highly elastic and compressible polylactic acid micro-nano fiber aerogel material.
[0093] Experimental example:
[0094] Taking the highly elastic compressible polylactic acid micro-nano fiber aerogel material prepared in the above Example 1 as an example, further research and analysis are carried out. The highly elastic compressible polylactic acid micro-nano fiber aerogel material is applied to the field of oil-water separation. In order to comprehensively study the oil-water separation effect of the highly elastic compressible polylactic acid micro-nano fiber aerogel material, three experiments are designed: oil absorption in water of highly elastic compressible polylactic acid micro-nano fiber aerogel, dynamic separation of immiscible oil-water mixture, and separation of miscible oil-water emulsion.
[0095] 1. Oil absorption experiment: Use a beaker to weigh 10g of dimethyl silicone oil, vacuum pump oil, n-hexane, petroleum ether, cyclohexane and 150mL of deionized water respectively, and mix them thoroughly to form an oil-water emulsion. Take a 0.1g body of highly elastic and compressible polylactic acid micro-nano fiber aerogel material and immerse it completely in the prepared oil-water emulsion to ensure that the material fully absorbs the oil. Take the soaked material out of the beaker and let it hang until no droplets drip from the material to ensure that all excess liquid has been removed. After ensuring that no droplets fall, weigh the treated material and record its mass. The oil adsorption capacity of the highly elastic and compressible polylactic acid micro-nano fiber aerogel material is calculated by formula (1).
[0096]
[0097] Wherein: Q is the oil adsorption capacity (g / g), m1 is the mass of the highly elastic and compressible polylactic acid micro-nano fiber aerogel material body before adsorption, i.e. 0.1 g, and m2 is the mass of the highly elastic and compressible polylactic acid micro-nano fiber aerogel material sample immersed in the oil-water emulsion and suspended until no droplets fall.
[0098] 2. Non-mixable oil-water mixture separation experiment: Dimethyl silicone oil, vacuum pump oil, n-hexane, petroleum ether, cyclohexane and deionized water were mixed in a ratio of 9:1 to prepare a non-mixable oil-water mixture. This step ensures the uniformity of the test mixture so that the performance of the separation material can be accurately evaluated. Cut a circular cylindrical high elastic compressible polylactic acid micro-nano fiber aerogel material with a diameter of 4 cm to fit the inner diameter of the separation device. Fix the prepared material in the separation unit (filter element), which has an inner diameter of 4 cm. This design ensures that the oil-water mixture can be separated uniformly through the material. Using the material as a filter element, a separation experiment was carried out under the action of gravity through a vacuum filtration device, and the separation flux was calculated by observing and recording the volume of filtrate collected within 1 minute. The water content of the filtrate was measured using a Karl Fisher moisture analyzer to calculate the efficiency of oil-water separation.
[0099] 3. Mixed phase oil-water emulsion separation experiment: 0.5 g of Span 80 surfactant was accurately weighed and mixed with 1 mL of deionized water in 99 mL of silicone oil (oil-based medium), and then the mixture was subjected to ultrasonic emulsification for two consecutive hours to prepare a stable surfactant-stabilized emulsion. Using a mixed phase oil-water emulsion separation device, i.e., a separation device consisting of a peristaltic pump and a separation unit, the highly elastic and compressible polylactic acid micro-nano fiber aerogel material was fixed in a separation unit with a diameter of 20 mm, and the separation efficiency and permeation flow rate of the highly elastic and compressible polylactic acid micro-nano fiber aerogel material were tested. By adjusting the external driving pressure, precise control of the separation conditions can be achieved.
[0100] The quantitative analysis of permeate flow rate adopts formula (2).
[0101]
[0102] Where J is the permeate flow rate, the unit is ml / (m 2 ·min). V represents the volume of filtrate per unit time (mL), a represents the test area (m 2 ), t is time (min). The final evaluation of separation performance was performed by measuring the water content in the filtrate using a Karl Fischer moisture analyzer, thereby accurately characterizing the application performance of highly elastic and compressible polylactic acid micro-nanofiber aerogel materials in oil-in-water emulsion separation.
[0103] The toughened polylactic acid micro-nano fibers provided in Example 1 were subjected to scanning electron microscopy to observe the in-situ interface compatibilization effect of polylactic acid, and the contact angle of the fibers was tested. The results are as follows: Figure 1 shown. Figure 1 (a) is a scanning electron microscope image of toughened polylactic acid micro-nano fibers. It can be seen from the figure that the diameter of toughened polylactic acid micro-nano fibers is distributed in 60nm-250nm, the fiber morphology is regular, the thickness is uniform, and there is no beading in the fibers. There is no phase interface separation between polylactic acid and thermoplastic elastomer. This is attributed to the use of epoxy groups in the polycyclic chain extender molecules, which have high reactivity. During the in-situ compatibilization reaction, the epoxy groups open the ring and react with the functional groups (-OH and -COOH) of polylactic acid and thermoplastic elastomer to form new chemical bonds, realizing the covalent bridging between polylactic acid, thermoplastic elastomer and polycyclic chain extender. The in-situ phase interface compatibilization of the polycyclic chain extender is coordinated with electrospinning to prepare toughened polylactic acid micro-nano fibers. At the same time, obvious cross-adhesion points appear between the fibers, which further improves the mechanical properties of the polylactic acid micro-nano fiber membrane. Selective surface superwettability is one of the important prerequisites for materials to achieve efficient oil-water separation. Figure 1 (b) is the contact angle diagram of toughened PLA micro-nanofibers with water. It can be seen from the figure that the contact angle of toughened PLA micro-nanofibers with water reaches 137°. Due to the hydrophobicity of PLA and thermoplastic elastomer, the toughened PLA micro-nanofibers have good hydrophobic effect. This observation result not only demonstrates the potential high performance of toughened PLA micro-nanofibers in simulated oil-water separation applications, but also highlights its multifunctional self-cleaning, separation, and filtration application potential in actual scenarios.
[0104] In order to demonstrate the structural stability, high specific surface area and porous structure of highly elastic and compressible polylactic acid micro-nanofiber aerogel materials, their micromorphology was characterized. Figure 2 This is a scanning electron microscope image of highly elastic and compressible polylactic acid micro-nanofiber aerogel material. Figure 2(a) is a microscopic morphology of a highly elastic and compressible polylactic acid micro-nano fiber aerogel material magnified 500 times. From the figure, it can be seen that the polylactic acid micro-nano fiber aerogel contains a large number of pores formed by cross-linking of polylactic acid micro-nano fibers. The toughened polylactic acid micro-nano fibers are broken into micro-nano short fibers by a homogenizer, which are then used as a gel framework. Aqueous polyurethane is used as a cross-linking agent for the micro-nano fibers. Through freeze drying, ice crystals formed by tert-butyl alcohol aqueous solution quickly sublimate to form a large number of pores. At the same time, the polylactic acid micro-nano fibers are cross-linked to form a three-dimensional porous structure. The polylactic acid micro-nano fiber aerogel has both the high specific surface area of polylactic acid micro-nano fibers and the porous structure and Figure 2 (b) is a microscopic morphology of a highly elastic compressible polylactic acid micro-nano fiber aerogel material magnified 1000 times and partially magnified 5000 times. It can be seen from the figure that in the highly elastic compressible polylactic acid micro-nano fiber aerogel material, the porous structure formed by cross-linking of micro-nano fibers and the state of cross-linking of waterborne polyurethane between fibers are shown. Waterborne polyurethane combines micro-nano fibers together through the action of a "bridging agent", thereby maintaining the stable morphology of the highly elastic compressible polylactic acid micro-nano fiber aerogel material and further increasing the mechanical compressibility and elastic recovery of the aerogel material.
[0105] Selective surface superwettability is one of the important prerequisites for materials to achieve efficient oil-water separation. In order to prove the hydrophobicity and oleophilicity of highly elastic and compressible polylactic acid micro-nanofiber aerogel materials, the contact angles of the materials with water and oil were tested. Figure 3 This is a diagram of the selective surface superwettability of highly elastic and compressible polylactic acid micro-nanofiber aerogel materials. Figure 3 (a) It can be seen that the toughened PLA micro-nanofibers show a certain degree of hydrophobicity, with a water contact angle of 137°, which is mainly due to the presence of a large number of hydrophobic ester and alkyl groups in the PLA molecular chain skeleton and the thermal elastomer molecular chain. In contrast, the surface of the PLA micro-nanofiber aerogel cross-linked by waterborne polyurethane has a multi-scale nanofiber / porous structure, showing extremely high superhydrophobicity. The highly elastic and compressible PLA micro-nanofiber aerogel material has a water contact angle of 152° in the air ( Figure 3 (b)), while the contact angle with oil is close to 0° ( Figure 3 (c)), which is attributed to the strong non-polarity of alkane or aromatic hydrocarbon groups in thermoplastic elastomers, which can form strong interactions with non-polar substances. This result reflects the super oleophilic / super hydrophobic selective wetting properties of highly elastic and compressible polylactic acid micro-nanofiber aerogel materials.
[0106] In order to demonstrate the mechanical properties of highly elastic and compressible polylactic acid micro-nanofiber aerogel materials, their compression recovery and elasticity were tested. Figure 4The compression-rebound stress-strain diagram of highly elastic compressible polylactic acid micro-nano fiber aerogel material and the height retention rate after cyclic compression are shown in Figure 2. Figure 4 As can be seen from (a), the maximum stress of the material can reach 21 kPa when the first compression strain is 50%. When compressed for 10, 100, 500 and 1000 times, the maximum stress value of the material still reaches about 18.5 kPa, which is significantly higher than the same type of materials (Advanced functional materials (2024), 2412424: 1-9). At the same time, it can be seen that the area enclosed by the stress-strain curve is small when the material is compressed and rebounds, which shows that the polylactic acid micro-nano fiber aerogel material has low rebound response hysteresis and high elasticity. The polylactic acid micro-nano fiber aerogel material can achieve a compression effect of 50% strain, which reflects its high compressibility. The excellent mechanical properties of the highly elastic compressible polylactic acid micro-nano fiber aerogel material are mainly attributed to the stability of the three-dimensional porous structure of the toughened polylactic acid micro-nano fiber and aerogel cross-linked obtained by the in-situ phase interface expansion of the multi-ring chain extender. Figure 4 (b) is the height retention rate of the highly elastic compressible polylactic acid micro-nano fiber aerogel material after 1000 cycles of cyclic compression under a compression strain of 50%. It can be seen from the figure that its height retention rate reaches 66.7%, which further illustrates that the highly elastic compressible polylactic acid micro-nano fiber aerogel material has outstanding mechanical properties, which is attributed to the stability of the structure of the polylactic acid micro-nano fiber aerogel material. In summary, the excellent mechanical properties of the highly elastic compressible polylactic acid micro-nano fiber aerogel material are proved, which provides a basis for its filtration or external pressure-driven emulsion separation and material reuse in oil-water separation applications.
[0107] In order to demonstrate the in-situ phase interface enlargement and the stability of the composite of highly elastic and compressible polylactic acid micro-nanofiber aerogel materials through chemical reaction between polylactic acid and thermoplastic elastomer, its microchemical structure was characterized. Figure 5 This is the infrared spectrum of highly elastic and compressible polylactic acid micro-nano fiber aerogel material. For polylactic acid molecules, at 1755cm -1 The peaks at 1450 and 1365 cm are attributed to C=O. -1 The peak at 1180cm-1 is attributed to the -CH3 vibration peak, and the peak at 1080cm-1 is attributed to the -CO-ester group. -1 The obvious vibration peak is seen at 3325cm, which is attributed to the stretching peak of C-O-C in the polylactic acid molecule. -1 The peak observed at 1528 cm is associated with the -NH stretching vibration. -1 The peak at 1595 cm-1 can be attributed to the stretching vibration of -CN, while the peak at 1595 cm-1 can be attributed to the stretching vibration of -CN. -1The peaks at 2950 and 2870 cm indicate the -NH bending vibration of the polyurethane group in the thermoplastic elastomer. -1 The peaks at 1,700-1,730 cm correspond to the asymmetric and symmetric vibrations of the -CH2- group. -1 The double peak at 1725cm is related to the C=O stretching vibration. -1 The peak at 1700 cm -1 The peak is associated with the hydrogen-bonded carbonyl groups.
[0108] For the toughened polylactic acid micro-nanofiber molecules, the characteristic peak signals of the mixture of polylactic acid and thermoplastic elastomer can be clearly seen in the infrared spectrum, among which 3325, 2,950, 2,870, 1725, 1700, 1595 and 1528 cm -1 The vibration peaks at 1755, 1450, 1365 and 1080 cm are from thermoplastic elastomers, and the vibration peaks at 1180 cm are from polylactic acid molecules. -1 The peak at 1180cm is attributed to the -CO-ester group, and the peak signal intensity at this location is significantly higher than that of polylactic acid and thermoplastic elastomer. This is attributed to the fact that during the construction stage of electrospinning polylactic acid micro-nanofibers, the polycyclic chain extender molecules contain epoxy groups, which have high reactivity. During the in situ compatibilization reaction, the epoxy groups open the ring and react with the functional groups (-OH and -COOH) of polylactic acid and thermoplastic elastomer to form new -CO-ester chemical bonds, thereby making the 1180cm -1 The peak signal intensity at increased, which confirmed that the in-situ phase interface compatibilization between polylactic acid and thermoplastic elastomer was achieved through chemical reaction. The covalent bridging between polylactic acid, thermoplastic elastomer and polycyclic chain extender was realized by in-situ phase interface compatibilization of polycyclic chain extender and synergistic electrospinning to prepare toughened polylactic acid micro-nano fibers. The mechanical properties of polylactic acid fibers and polylactic acid micro-nano fiber aerogel materials were significantly improved by in-situ phase interface compatibilization and synergistic electrospinning technology. For highly elastic and compressible polylactic acid micro-nano fiber aerogel materials, they are mainly composed of toughened polylactic acid micro-nano fibers and waterborne polyurethane. The characteristic signal peaks of toughened polylactic acid micro-nano fiber molecules and waterborne polyurethane molecules can be observed in the highly elastic and compressible polylactic acid micro-nano fiber aerogel materials. Due to the presence of 1725cm in polyurethane -1 The peak of is related to the free carbonyl group, and the vibration signal of the free carbonyl group can be clearly seen in the infrared spectrum of waterborne polyurethane. It is worth noting that after toughening the polylactic acid micro-nano fiber molecules and waterborne polyurethane molecules, the 1725cm -1The peak signal intensity of was significantly enhanced, which indicated that the two were well compounded. In summary, the successful preparation of highly elastic and compressible polylactic acid micro-nano fiber aerogel material and its stable structure were proved by the microscopic chemical structure.
[0109] The highly elastic and compressible polylactic acid micro-nano fiber aerogel material is applied in the field of oil-water separation. The experimental results of oil absorption in water, dynamic separation of immiscible oil-water mixture and separation of miscible oil-water emulsion are shown in Figure 2. Figure 6 , Figure 7 and Figure 8 As shown. Figure 6 As shown in (a), the oil absorption capacities of highly elastic compressible polylactic acid micro-nanofiber aerogel material for silicone oil, vacuum pump oil, n-hexane, cyclohexane and petroleum ether are 21.0, 17.4, 17.5, 20.8 and 15.3 g·g, respectively. -1 , which is significantly higher than that of similar products that have been reported (Journal of Dispersion Science and Technology (2019), 41(2), 289–296 and Journal of Porous Materials (2022), 29: 241–247). This significantly improved oil absorption performance can be attributed to its high specific surface area and three-dimensional porous structure, which provides additional storage space for oil. The oil can quickly diffuse on the rough surface of the highly elastic and compressible polylactic acid micro-nanofiber aerogel material and further penetrate into the porous network. In addition, Figure 6 As shown in (b), the highly elastic compressible polylactic acid micro-nanofiber aerogel material still exhibits excellent and long-term oil absorption stability after 10 cycles of testing, which is attributed to the excellent mechanical properties of the material. These results not only demonstrate the application potential of highly elastic compressible polylactic acid micro-nanofiber aerogel materials in the field of oil-water separation, but also emphasize its long-term reliability as an environmental purification material. The excellent superhydrophobicity, superoleophilicity, waterproof adhesion, and unique micro-nanofiber high specific surface area and three-dimensional porous structure of highly elastic compressible polylactic acid micro-nanofiber aerogel materials make it a very promising candidate material in the field of oil-water separation. Using gravity drive, the phase-separated oil / water mixture can be effectively separated. The oil phase can quickly penetrate through the highly elastic compressible polylactic acid micro-nanofiber aerogel material, while the water phase is successfully repelled and retained by the surface of the bionic sponge. In the separation tests of five different oil-water mixtures (silicone oil / water, vacuum pump oil / water, n-hexane / water, cyclohexane / water and petroleum ether / water), the highly elastic and compressible polylactic acid micro-nanofiber aerogel material showed high separation flux characteristics, with permeation fluxes of 24032, 20628, 20854, 19532 and 22563 L·m, respectively. -2 ·h -1 (like Figure 7 This result highlights the high efficiency of highly elastic compressible polylactic acid micro-nanofiber aerogel materials in oil-water separation applications, especially in the treatment of oil-water mixtures containing oil phases with different densities and viscosities. It is worth noting that the density and viscosity of the oil are the key factors affecting the separation performance of highly elastic compressible polylactic acid micro-nanofiber aerogel materials sponge, especially for silicone oil / water mixtures, the higher separation flux may be due to the higher density of silicone oil (0.963 g cm -3 ) promotes the rapid penetration of its fluid. The unique high specific surface area and three-dimensional porous structure of highly elastic compressible polylactic acid micro-nano fiber aerogel material not only provides efficient oil-water separation ability, but also can still maintain a separation efficiency of up to 99.92% after 10 cycles of testing, showing its excellent separation stability, such as Figure 7 (b). This long-lasting performance indicates that highly elastic and compressible polylactic acid micro-nano fiber aerogel materials have the potential for long-term application in the field of oil-water separation, providing an effective way to achieve efficient, long-lasting and sustainable oil-water separation technology. Highly elastic and compressible polylactic acid micro-nano fiber aerogel materials with superhydrophobic and superoleophilic properties can effectively capture oil droplets at the micro-nano scale, thereby forming a stable oil layer, relying on the high specific surface area and three-dimensional porous structure of its micro-nano fibers. This adsorption mechanism promotes the formation of a composite interface between the fiber surface and the oil phase, and effectively prevents the adsorption of water molecules by enhancing the capillary retention force. Furthermore, with the help of the capillary effect, the oil phase can quickly pass through the three-dimensional porous structure of the polylactic acid micro-nano fiber aerogel, achieving efficient oil-in-water emulsion separation. Figure 8 (a) shows that when using highly elastic and compressible polylactic acid micro-nano fiber aerogel material as the filter medium, the moisture content of the filtrate treated by the highly elastic and compressible polylactic acid micro-nano fiber aerogel material is less than 60ppm, and the separation efficiency reaches 99%. Figure 8 As shown in (b), when the external driving pressure increases from 0 to 20 kPa, the permeation flux of the highly elastic compressible polylactic acid micro-nano fiber aerogel material for the (water / silicone oil) water-in-oil emulsion system reaches 1003, 2080, 3500, 4000, and 4800 L·m, respectively. -2 ·h -1 , the moisture content of the filtered liquid was kept below 88ppm. This result shows the importance of the high specific surface area structure of micro-nanofiber in highly elastic compressible polylactic acid micro-nanofiber aerogel materials, as well as the synergistic effect of superhydrophobic / superoleophilic selective wetting properties and the importance of interconnected porous channels, which together promote the excellent performance of highly elastic compressible polylactic acid micro-nanofiber aerogel materials in effectively intercepting emulsified water droplets and promoting rapid penetration of oil phase.
[0110] The above describes in detail the structure, features and effects of the present invention based on the embodiments shown in the drawings. The above is only a preferred embodiment of the present invention, but the present invention is not limited to the scope of implementation shown in the drawings. Any changes made according to the concept of the present invention, or modifications to equivalent embodiments with equivalent changes, which still do not exceed the spirit covered by the description and drawings, should be within the protection scope of the present invention.
Claims
1. A highly elastic and compressible polylactic acid micro-nano fiber aerogel material, It is characterized in that The highly elastic and compressible polylactic acid micro-nano fiber aerogel material is a three-dimensional network composed of toughened polylactic acid micro-nano fibers and waterborne polyurethane, wherein the toughened polylactic acid micro-nano fibers serve as a gel framework and the waterborne polyurethane serves as a cross-linking network.
2. A method for preparing a highly elastic and compressible polylactic acid micro-nano fiber aerogel material, used for preparing the highly elastic and compressible polylactic acid micro-nano fiber aerogel material according to claim 1, It is characterized in that The following steps are involved: S1: dissolving polylactic acid and thermoplastic elastomer in a compound solvent to obtain a polymer solution, adding a polycyclic chain extender to the polymer solution, ultrasonically dispersing the solution for in-situ phase interface volume expansion, and vacuum degassing to obtain a spinning precursor solution; S2: The spinning precursor solution is subjected to high-voltage electrospinning to obtain toughened polylactic acid micro-nanofibers; S3: Use a homogenizer to disperse the toughened polylactic acid micro-nano fibers into a tert-butyl alcohol aqueous solution, add aqueous polyurethane as a cross-linking agent into the aqueous solution to obtain a toughened polylactic acid micro-nano fiber hydrogel, and vacuum freeze-dry the hydrogel material to obtain a highly elastic and compressible polylactic acid micro-nano fiber aerogel material.
3. The method for preparing the highly elastic and compressible polylactic acid micro-nano fiber aerogel material according to claim 2, It is characterized in that The composite solvent in step S1 is composed of tetrahydrofuran and N,N'-dimethylformamide in a mass ratio of 1 to 3:1; In step S1, the amount of the polylactic acid and the thermoplastic elastomer in the compounding solvent is 10-15wt%, and the mass ratio of the polylactic acid to the thermoplastic elastomer is 3:2; In step S1, the amount of the polycyclic chain extender in the polylactic acid and the thermoplastic elastomer is 0.5-2 wt%.
4. The method for preparing the highly elastic and compressible polylactic acid micro-nano fiber aerogel material according to claim 2, It is characterized in that The ultrasonic dispersion treatment conditions in step S1 are: the power is set to 500-1200W, and the treatment time is 1-10h.
5. The method for preparing the highly elastic and compressible polylactic acid micro-nano fiber aerogel material according to claim 2, It is characterized in that In step S1, the thermoplastic elastomer is at least one of aliphatic polyether urethane TPU, aromatic polyether urethane TPU, aliphatic polycarbonate urethane TPU, and aromatic polycarbonate urethane TPU, and the polycyclic chain extender is styrene-glycidyl methacrylate oligomer.
6. The method for preparing the highly elastic and compressible polylactic acid micro-nano fiber aerogel material according to claim 2, It is characterized in that The high-voltage electrospinning parameters in step S2 are set as follows: high-voltage electrostatic 10-20 kV, a pushing speed of 1-5 ml / h, a receiving distance of 8-15 cm, and a spinning needle of any one of 19G, 20G, 21G, 22G, and 23G.
7. The method for preparing the highly elastic and compressible polylactic acid micro-nano fiber aerogel material according to claim 2, It is characterized in that In step S3, the amount of the toughened polylactic acid micro-nano fibers in the tert-butyl alcohol aqueous solution is 0.5-2 wt %.
8. The method for preparing the highly elastic and compressible polylactic acid micro-nano fiber aerogel material according to claim 2 or 7, It is characterized in that The tert-butanol aqueous solution in step S3 is composed of tert-butanol and aqueous solution in a mass ratio of 1:
4. The processing conditions of the homogenizer are: 10000-20000 rpm, and the processing time is 0.5-2h.
9. The method for preparing the highly elastic and compressible polylactic acid micro-nano fiber aerogel material according to claim 2, It is characterized in that In step S3, the mass ratio of the waterborne polyurethane to the toughened polylactic acid micro-nanofibers is 0.1-1:1, and the waterborne polyurethane is at least one of aromatic isocyanate type WPU, aliphatic isocyanate type WPU, and alicyclic isocyanate type WPU.
10. Application of a highly elastic and compressible polylactic acid micro-nano fiber aerogel material, It is characterized in that Application of the highly elastic compressible polylactic acid nanofiber aerogel material prepared by using the highly elastic compressible polylactic acid nanofiber aerogel material described in claims 2 to 9 in the field of oil-water separation.
Citation Information
Patent Citations
Method for preparing 3D porous crosslinked composite aerosol assembled by thermo-bond reinforced nano-fibers
CN108892911A
Preparation method and application of polylactic acid hollow fiber aerogel
CN116103774A
Mother board
KR102711827B1
Core-sheath fibers and methods of making and using same
WO2014143866A1
Ion exchange-type nanofiber skeleton three-dimensional separation material having controllable structure, and preparation method for same
WO2021004458A1