High-performance nano natural stone powder finish coating and construction method thereof

By adding nano-titanium dioxide and flexible waterproof sealing materials to natural stone powder finishing coatings, the problems of easy hollowing, powdering, and unsatisfactory hardness and wear resistance of traditional finishing materials are solved, achieving high-performance self-cleaning and improved anti-wear properties.

CN119019875APending Publication Date: 2024-11-26SOUTHERN CONSTR CO LTD OF CHINA CONSTR EIGHTH ENG DIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411184140.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Traditional finishing materials are prone to hollowing, powdering, and peeling, especially in humid environments, and contain harmful chemicals that affect the environment and human health; natural stone powder coatings have unsatisfactory hardness, wear resistance, and weather resistance.

Method used

High-performance nano-natural stone powder finishing coating is adopted. By adding 5% nano-titanium dioxide to the stone powder material, the particle size is less than 50 nanometers. The surface effect and volume effect of nanomaterials are used to enhance the particle bonding force. Combined with flexible waterproof sealing material and crack-resistant cloth, a dense surface layer is formed.

Benefits of technology

It improves the hardness, abrasion resistance and weather resistance of the coating, has self-cleaning properties, enhances the surface layer's resistance, reduces agglomeration, and is suitable for humid environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019875A_ABST
    Figure CN119019875A_ABST
Patent Text Reader

Abstract

The invention discloses a high-performance nano natural stone powder finish coating and a construction method thereof, the high-performance nano natural stone powder finish coating comprises powder and water, the mass ratio of the powder to the water is 2: 1, the powder comprises 95% of stone powder surface material and 5% of nano titanium dioxide, and the mass ratio of the stone powder surface material to the nano titanium dioxide is 1: 1, and the mass ratio of the stone powder surface material to the nano titanium dioxide is 1: 1. The stone powder surface material comprises 50%-60% of heavy calcium carbonate, 25%-35% of ash calcium, 8%-10% of quartz stone powder, 2%-4% of light calcium carbonate, 1.2%-1.8% of white cement and 0.4%-0.6% of rubber powder. The problem that an existing natural stone powder coating is not ideal in hardness, abrasion resistance and weather resistance is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building construction, and in particular to a high-performance nano natural stone powder finishing paint and a construction method thereof. Background Art

[0002] In the construction industry, traditional finishing materials such as cement plaster, plaster mortar and interior wall paint have many disadvantages, such as easy hollowing, powdering and falling off, especially in humid environments. In addition, these materials often contain harmful chemicals, posing a potential threat to the environment and human health. As people's requirements for green environmental protection and living quality increase, it is particularly important to develop a new, environmentally friendly and durable finishing material.

[0003] As a new type of environmentally friendly material, natural stone powder has been gradually recognized by the market for its excellent performance since it entered the construction industry in the 1990s. Natural stone powder is mainly made of natural carbonate monoclinic mineral hard stone through selection, processing and grinding. The main component is hydrated calcium carbonate (CaCO3), with a content of not less than 95%. It is characterized by being strong, fire-resistant, water-resistant, moisture-proof, breathable, easy to clean, and free of chemical and radioactive pollution. It is an ideal finishing material.

[0004] However, the surface characteristics of natural stone powder make it easy to absorb water during use, resulting in poor hydrophobicity of the coating. In addition, the bonding force between the particles of natural stone powder is weak, which will affect the hardness, wear resistance and weather resistance of the coating.

[0005] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0006] In order to overcome the defects of the prior art, a high-performance nano-natural stone powder finishing paint and a construction method thereof are provided to solve the problems of unsatisfactory hardness, wear resistance and weather resistance of the existing natural stone powder coatings.

[0007] To achieve the above-mentioned purpose, a high-performance nano natural stone powder finishing paint is provided, comprising powder and water, wherein the mass ratio of the powder to the water is 2:1, and based on the mass of the powder, the powder comprises 95% of stone powder facing material and 5% of nano titanium dioxide, and based on the mass of the stone powder facing material, the stone powder facing material comprises 50% to 60% of heavy calcium, 25% to 35% of gray calcium, 8% to 10% of quartz stone powder, 2% to 4% of light calcium, 1.2% to 1.8% of white cement, and 0.4% to 0.6% of rubber powder.

[0008] Furthermore, the particle size of the nano titanium dioxide is less than 50 nanometers.

[0009] The present invention provides a construction method of a high-performance nano-natural stone powder finishing coating, comprising the following steps:

[0010] The stone powder surface material and nano titanium dioxide of the powder are respectively added with water and stirred and mixed evenly to obtain stone powder dispersion liquid and titanium dioxide dispersion liquid;

[0011] The stone powder dispersion and the titanium dioxide dispersion are uniformly mixed to obtain a high-performance nano-natural stone powder finishing coating;

[0012] Open a partition groove in the wall to be constructed;

[0013] A caulking strip is embedded in the dividing groove, and a receiving groove is formed on one side of the caulking strip away from the groove bottom of the dividing groove;

[0014] Filling the accommodating groove with a flexible waterproof sealing material;

[0015] Laying anti-crack cloth on the wall, wherein the anti-crack cloth covers the dividing groove;

[0016] A base layer is coated on the wall, and the base layer is coated on the anti-cracking cloth;

[0017] Applying a leveling layer on the base layer;

[0018] The high-performance nano natural stone powder finishing paint is applied to the leveling layer to form a surface layer.

[0019] Furthermore, the leveling layer is a natural stone powder leveling layer.

[0020] Furthermore, the base layer includes natural stone powder and coarse aggregate, and the mass ratio of the natural stone powder to the coarse aggregate is 3 to 5:1.

[0021] The beneficial effect of the present invention is that the high-performance nano-natural stone powder finishing paint of the present invention adds 5% of the nano-grade additive nano-titanium dioxide to the stone powder surface, and enhances the bonding force between the stone powder particles through the surface effect and volume effect of the nano-material, thereby improving the hardness, wear resistance and weather resistance of the coating. Nano-titanium dioxide has super hydrophilicity and super permanence, and is not easy to form water droplets on the surface of the natural stone powder surface layer, especially showing excellent self-cleaning performance in the south China region during the return of the south wind climate. At the same time, the density of the surface layer is enhanced, and the resistance of the natural stone powder surface layer is improved. The stone powder surface and the nano-titanium dioxide powder are added to the liquid separately, and are mixed and stirred after being stirred evenly, which can greatly reduce the agglomeration phenomenon of uneven fusion and stirring of the nano-titanium dioxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Other features, objects and advantages of the present application will become more apparent by reading the detailed description of non-limiting embodiments made with reference to the following drawings:

[0023] Figure 1 It is a schematic structural diagram of a wall to be constructed according to an embodiment of the present invention. DETAILED DESCRIPTION

[0024] The present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the relevant invention, rather than to limit the invention. It is also necessary to explain that, for ease of description, only the parts related to the invention are shown in the accompanying drawings.

[0025] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0026] The invention provides a high-performance nanometer natural stone powder finishing paint, comprising powder and water, wherein the mass ratio of the powder to the water is 2:1.

[0027] Taking the weight of the powder as 100%, the powder includes 95% stone powder fabric and 5% nano titanium dioxide.

[0028] Taking the mass of stone powder fabric as 100%, the stone powder fabric includes 50% to 60% heavy calcium cement, 25% to 35% gray calcium cement, 8% to 10% quartz stone powder, 2% to 4% light calcium cement, 1.2% to 1.8% white cement, and 0.4% to 0.6% rubber powder.

[0029] In this embodiment, the particle size of nano titanium dioxide is less than 50 nanometers.

[0030] Reference Figure 1 As shown, the present invention provides a construction method of a high-performance nano-natural stone powder finishing coating, comprising the following steps:

[0031] S1. Add water to the stone powder surface material and nano titanium dioxide powder, stir and mix them evenly to obtain stone powder dispersion and titanium dioxide dispersion.

[0032] Prepare stone powder fabric and nano titanium dioxide powder, wherein the particle size of the nano titanium dioxide is 50nm. Weigh the stone powder fabric and nano titanium dioxide powder in a ratio of 95% and 5% respectively. Powder: water = 2: 1 (mass ratio).

[0033] Add the stone powder fabric and nano titanium dioxide powder into two different containers, then add equal proportions of clean water and stir evenly. An electric stirrer is used here, the speed is set to 500 rpm, and the stirring time is 15 minutes.

[0034] S2. Evenly mix the stone powder dispersion and the titanium dioxide dispersion to obtain a high-performance nano-natural stone powder finishing coating.

[0035] The evenly stirred stone powder dispersion and titanium dioxide dispersion were mixed together, and stirred again using an electric stirrer with the speed set to 800 rpm for 30 minutes.

[0036] S3. Open a partition groove in the wall 1 to be constructed.

[0037] When treating the wall base, a dividing groove is set up with a length of 3m in the vertical and horizontal directions of the wall surface. A dividing groove of 1cm wide and 1cm deep is cut in the masonry wall.

[0038] S4. A caulking strip 2 is embedded in the dividing groove, and a receiving groove is formed on one side of the caulking strip away from the groove bottom of the dividing groove.

[0039] In this embodiment, the caulking strip is made of PVC material.

[0040] S5, filling the accommodating groove with a flexible waterproof sealing material 3.

[0041] The PVC caulking strip is filled with flexible waterproof sealing material and is flush with the wall.

[0042] S6. Lay anti-cracking cloth 4 on the wall, and the anti-cracking cloth covers the dividing groove.

[0043] A 300mm wide anti-cracking cloth (such as alkali-resistant mesh cloth) is pasted on the caulking strips, and the alkali-resistant mesh cloth is pasted across the caulking strips, 150mm on each side.

[0044] S7, coating the wall with a base layer 5, which is covered with the anti-cracking cloth.

[0045] In this embodiment, the base layer includes natural stone powder and coarse aggregate, and the mass ratio of natural stone powder to coarse aggregate is 3 to 5:1.

[0046] The ratio of coarse aggregate stone powder to coarse aggregate in the base layer is between 3:1 and 5:1. This ratio range can be adjusted according to the specific performance requirements of the coating and the construction conditions. For example, in a coating that requires higher strength and thickness, the proportion of coarse aggregate can be appropriately increased; while in a coating that requires higher flatness and fineness, the proportion of coarse aggregate can be appropriately reduced.

[0047] The thickness of the base layer is 8 mm.

[0048] S8. Apply a leveling layer 6 on the base layer.

[0049] In this embodiment, the leveling layer is a natural stone powder leveling layer.

[0050] The thickness of the leveling layer is 1.5mm.

[0051] S9, applying high-performance nano natural stone powder finishing paint to the leveling layer to form a surface layer 7.

[0052] The thickness of the surface layer is 0.5 mm.

[0053] The particle size of nano titanium dioxide is one of the key factors affecting the performance of high-performance nano natural stone powder finish coatings. Nanomaterials with a particle size within the range of 50 nanometers are selected to ensure their uniform dispersion and stable presence in the coating. The purity of nanomaterials should not be less than 99% to reduce the impact of impurities on the performance of the coating.

[0054] Stone powder fabrics include heavy calcium (50% to 60%), gray calcium (25% to 35%), quartz powder (8% to 10%), light calcium (2% to 4%), white cement (1.2% to 1.8%), rubber powder (0.4% to 0.6%) and other raw materials. Mix the various raw materials evenly according to the formula ratio, and add appropriate amount of water or special liquid material to blend until a slurry with suitable viscosity and fluidity is formed.

[0055] Adding 5% of nano-grade additive nano titanium dioxide to the stone powder fabric can enhance the bonding force between the stone powder particles through the surface effect and volume effect of the nano material, thereby improving the hardness, wear resistance and weather resistance of the coating.

[0056] Nano-titanium dioxide is super hydrophilic and super permanent, and it is not easy to form water droplets on the surface of natural stone powder surface layer, especially in the south China region, it shows excellent self-cleaning performance. At the same time, it enhances the density of the surface layer and improves the anti-corrosion performance of the natural stone powder surface layer.

[0057] The stone powder fabric and nano titanium dioxide powder are added to the liquid material separately, stirred evenly and then mixed, which can greatly reduce the agglomeration phenomenon of the nano titanium dioxide caused by uneven fusion and stirring.

[0058] When the wall base is processed, a partition groove is built into the wall, and caulking strips are embedded and filled with flexible fillers. Anti-cracking cloth (such as alkali-resistant mesh cloth) is hung outside the caulking strips. On the one hand, it prevents irregular cracks caused by different expansion coefficients, contraction coefficients, deformation coefficients, and wall settlement between different materials, and guides the deformation of cracks in an orderly manner. On the other hand, the alkali-resistant mesh cloth can effectively prevent wall cracks from producing reflective cracks on natural stone powder paint.

[0059] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above technical features, but should also cover other technical solutions formed by any combination of the above technical features or their equivalent features without departing from the inventive concept. For example, the above features are replaced with (but not limited to) technical features with similar functions disclosed in the present application.

Claims

1. A high-performance nano-natural stone powder finishing paint, characterized in that: It includes powder and water, the mass ratio of the powder to the water is 2:1, based on the mass of the powder, the powder includes 95% of stone powder fabric and 5% of nano titanium dioxide, based on the mass of the stone powder fabric, the stone powder fabric includes 50%-60% of heavy calcium, 25%-35% of gray calcium, 8%-10% of quartz stone powder, 2%-4% of light calcium, 1.2%-1.8% of white cement, and 0.4%-0.6% of rubber powder.

2. The high-performance nano-natural stone powder finishing paint according to claim 1, characterized in that: The particle size of the nano titanium dioxide is less than 50 nanometers.

3. A construction method of a high-performance nano-natural stone powder finishing coating as claimed in any one of claims 1 to 2, characterized in that: The following steps are involved: The stone powder surface material and nano titanium dioxide of the powder are respectively added with water and stirred and mixed evenly to obtain stone powder dispersion and titanium dioxide dispersion; The stone powder dispersion and the titanium dioxide dispersion are uniformly mixed to obtain a high-performance nano-natural stone powder finishing coating; Open a partition groove in the wall to be constructed; A caulking strip is embedded in the dividing groove, and a receiving groove is formed on one side of the caulking strip away from the groove bottom of the dividing groove; Filling the accommodating groove with a flexible waterproof sealing material; Laying anti-crack cloth on the wall, wherein the anti-crack cloth covers the dividing groove; Coating a base layer on the wall, wherein the base layer is coated on the anti-cracking cloth; Applying a leveling layer on the base layer; The high-performance nano natural stone powder finishing paint is applied to the leveling layer to form a surface layer.

4. The construction method according to claim 3, characterized in that: The leveling layer is a natural stone powder leveling layer.

5. The construction method according to claim 3, characterized in that: The base layer includes natural stone powder and coarse aggregate, and the mass ratio of the natural stone powder to the coarse aggregate is 3 to 5:1.

Citation Information

Patent Citations

  • Dry powder type shell powder interior wall coating material and preparation method thereof

    CN103627261A

  • Nanometer stone water mill wall coating and construction method thereof

    CN106242461A

  • Stone powder whitewashing coating as well as preparation method and use method thereof

    CN113637341A

  • Non-asbestos interior wall facing coating as well as preparation method and application thereof