Composite coating for enhancing adhesive force of ink, preparation method of composite coating and image printing method

By using composite coatings with modified acrylic resin, polyurethane resin and other components in inkjet printing technology, the problem of insufficient ink adhesion and coating stability on the surface of high-density materials is solved, and efficient ink adhesion and image printing effects are achieved .

CN119019897APending Publication Date: 2024-11-26DONGGUAN TUCHUANG INTELLIGENT MFG CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411053804.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Traditional inkjet printing technology is difficult to achieve effective adhesion of ink and coating stability on the surface of high-density materials, resulting in poor printing effect and poor durability. The existing coating formula has problems of environmental protection and insufficient stability.

Method used

Using a composite coating, including modified acrylic resin, polyurethane resin, isocyanate crosslinking agent, ethyl acetate, cyclohexanone, ethylene glycol monoethyl ether acetate, n-butyl acetate, tackifier and silane coupling agent, By optimizing the ratio and process preparation method, a coating is formed to enhance the adhesion of the ink.

Benefits of technology

It significantly improves the adhesion, wear resistance and chemical resistance of the coating, shortens drying time, improves printing quality and production efficiency, and ensures firm adhesion of the ink on the surface of high-density materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides a composite coating for enhancing ink adhesion, a preparation method thereof and an image printing method, and relates to the field of ink-jet printing.The composite coating comprises, by weight, 20-30% of modified acrylic resin, 5-10% of polyurethane resin, 15% of ethyl acetate, 10% of cyclohexanone and 10% of ethylene glycol monoethyl ether acetate. 20-30% of n-butyl acetate, 1-3% of an isocyanate cross-linking agent and 5% of a tackifier. According to the composite coating, by using the modified acrylic resin, the polyurethane resin, the isocyanate cross-linking agent and optimizing the ratio of a solvent system, various performance indexes of a coating are remarkably improved, for example, the adhesive force is remarkably enhanced, the wear resistance and the chemical resistance are greatly improved, meanwhile, the drying time is effectively shortened, and the service life of the coating is prolonged. Not only can the overall performance of the coating be improved, but also the production efficiency can be remarkably improved. Before an image is subjected to ink-jet printing, the composite coating is sprayed on the surface of a printing medium, so that the adhesive force of ink can be effectively increased, and the image printing quality is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of inkjet printing, and in particular to a composite coating for enhancing ink adhesion, a preparation method thereof, and an image printing method. Background Art

[0002] Inkjet printing technology is a technology widely used in various printing needs. It accurately sprays tiny ink droplets onto the printing medium through the nozzle on the print head to form images or text. The core advantages of inkjet printing technology are its high resolution, flexibility and adaptability to various media. Whether it is paper, textiles, plastic films, or other special materials, inkjet printing technology can provide high-quality printing results. However, when printing on high-density material surfaces, such as acrylic, glass, etc., traditional inkjet printing technology faces some challenges, especially in terms of ink adhesion and coating stability. The surface of high-density materials is usually smooth and lacks pores, which makes it difficult for ink to adhere effectively. This not only affects the clarity and color performance of the printed image, but also causes the ink to peel off or erase easily during the drying process. In order to solve this problem, a layer of coating is usually printed on the surface of these high-density materials. The role of this coating is to increase the roughness and affinity of the surface so that the subsequent ink jetting can adhere firmly to it.

[0003] An existing coating formula includes acrylic resin, toluene, xylene, ethylene glycol monoethyl ether acetate (EGMEA) and n-butyl acetate. Acrylic resin is the main film-forming substance of the coating, which provides the mechanical strength and durability of the coating. Toluene and xylene are used as solvents to dissolve the resin and other components, reduce the viscosity of the coating, and make the coating easy to apply. Ethylene glycol monoethyl ether acetate is used to control the drying speed of the coating, improve the flatness and gloss of the coating, and n-butyl acetate is used to adjust the fluidity and drying time of the coating. Although this coating formula solves the problem of ink adhesion to a certain extent, it still has some shortcomings. For example, toluene and xylene are volatile and have certain toxicity, which may affect the environment and human health; the coating has poor stability, resulting in the coating falling off or deterioration during use. At the same time, the drying speed and fluidity of the coating are difficult to accurately control, resulting in problems such as uneven coating surface and insufficient gloss. These problems seriously affect the printing effect and durability of inkjet printing on high-density material surfaces. Summary of the invention

[0004] The invention provides a composite coating for enhancing ink adhesion, a preparation method thereof and an image printing method, so as to overcome the shortcomings of the coating in the prior art, such as being environmentally unfriendly and having poor stability.

[0005] As one aspect of the present invention, an embodiment of the present invention provides a composite coating for enhancing ink adhesion, wherein the composite coating comprises the following components by weight percentage: 20-30% of modified acrylic resin, 5-10% of polyurethane resin, 15% of ethyl acetate, 10% of cyclohexanone, 10% of ethylene glycol monoethyl ether acetate, 20-30% of n-butyl acetate, 1-3% of isocyanate crosslinker, and 5% of tackifier.

[0006] Preferably, the isocyanate cross-linking agent includes any one or more of hexamethylene diisocyanate trimer, isophorone diisocyanate trimer, toluene diisocyanate trimer, and hydrogenated diphenylmethane diisocyanate trimer.

[0007] Preferably, the tackifier comprises any one or more of polyamide resin, chlorinated polypropylene, polyisobutylene, hydrogenated rosin glycerol ester, and SIS copolymer.

[0008] Preferably, the composite coating further comprises: 1-2% by weight of a silane coupling agent and 0.1-0.5% by weight of a surfactant.

[0009] Preferably, the silane coupling agent includes any one or more of γ-aminopropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, and γ-cyanoethyltriethoxysilane.

[0010] Preferably, the surfactant includes any one or more of a silicone surfactant, a phosphate ester surfactant, a fatty acid soap surfactant, and a nonionic surfactant.

[0011] As a second aspect of the present invention, an embodiment of the present invention provides a method for preparing a composite coating for enhancing ink adhesion, which mainly comprises the following steps:

[0012] Weigh the following components by weight percentage: modified acrylic resin: 20-30%, polyurethane resin: 5-10%, ethyl acetate: 15%, cyclohexanone: 10%, ethylene glycol monoethyl ether acetate: 10%, n-butyl acetate: 20-30%, isocyanate crosslinking agent: 1-3%, tackifier: 5%;

[0013] Add modified acrylic resin and polyurethane resin into a container and stir;

[0014] Gradually add ethyl acetate and cyclohexanone and continue stirring until the solution is homogeneous;

[0015] Add ethylene glycol monoethyl ether acetate and n-butyl acetate and keep stirring;

[0016] Slowly add the isocyanate crosslinker to mix it thoroughly with the resin and solvent;

[0017] Add the tackifier and continue stirring until all components are evenly mixed to form a uniform coating solution;

[0018] Filter the mixed coating solution through a filter cloth or filter to remove insoluble impurities from the mixing process.

[0019] Preferably, before adding the tackifier and continuing stirring until all components are uniformly mixed to form a uniform coating solution, the process further comprises:

[0020] The weight percentages are 1-2% of silane coupling agent and 0.1-0.5% of surfactant.

[0021] Preferably, before adding 1-2% by weight of a silane coupling agent and 0.1-0.5% by weight of a surfactant, the method further comprises: microencapsulating the silane coupling agent, specifically comprising:

[0022] Dissolving the silane coupling agent in the oil phase to obtain a capsule-core mixed solution;

[0023] Dissolving any one or more of polylactic acid, polyvinyl alcohol, gelatin, and sodium alginate in an aqueous phase to obtain a capsule wall mixture, and adding an emulsifier to the capsule wall mixture;

[0024] Adding the capsule core mixed liquid into the capsule wall mixed liquid and stirring to form a uniform emulsion;

[0025] A crosslinking agent is added to the emulsion, and after reacting for a first preset time, a curing agent is added and the reaction is continued for a second preset time to obtain silane coupling agent microcapsules.

[0026] In a third aspect, an embodiment of the present invention provides an image printing method, which mainly includes the following steps:

[0027] Spraying the composite coating as described in any one of the first aspect or the composite coating prepared by the second aspect onto the surface of the printing medium to form a coating;

[0028] The printing nozzle is controlled to spray ink onto the coating surface to form an image.

[0029] In summary, the embodiment of the present invention provides a composite coating for enhancing ink adhesion, a preparation method thereof, and an image printing method. The composite coating comprises the following components by weight percentage: 20-30% of modified acrylic resin, 5-10% of polyurethane resin, 15% of ethyl acetate, 10% of cyclohexanone, 10% of ethylene glycol monoethyl ether acetate, 20-30% of n-butyl acetate, 1-3% of isocyanate crosslinking agent, and 5% of a tackifier composite coating. The composite coating significantly improves various performance indicators of the coating by using modified acrylic resin, polyurethane resin, isocyanate crosslinking agent and optimizing the ratio of the solvent system, such as significantly enhanced adhesion, greatly improved wear resistance and chemical resistance, and effectively shortened drying time, which can not only improve the overall performance of the coating, but also significantly improve production efficiency. Spraying the composite coating on the surface of the printing medium before inkjet printing the image can effectively increase the ink adhesion and thus improve the image printing quality. DETAILED DESCRIPTION

[0030] The features and exemplary embodiments of various aspects of the present invention will be described in detail below. In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention will be further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only configured to explain the present invention and are not configured to limit the present invention. For those skilled in the art, the present invention can be implemented without the need for some of these specific details. The following description of the embodiments is only to provide a better understanding of the present invention by illustrating examples of the present invention.

[0031] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the statement "include..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.

[0032] The first aspect of the present invention provides a composite coating for enhancing ink adhesion, wherein the composite coating comprises the following components by weight percentage: modified acrylic resin: 20-30%, polyurethane resin: 5-10%, ethyl acetate: 15%, cyclohexanone: 10%, ethylene glycol monoethyl ether acetate: 10%, n-butyl acetate: 20-30%, isocyanate crosslinking agent: 1-3%, and tackifier: 5%.

[0033] In the above composite coating, modified acrylic resin and polyurethane resin are film-forming substances in the composite coating. Modified acrylic resin provides the basic structure and adhesion of the coating, giving the coating excellent mechanical strength and durability. It can form a uniform and stable coating on the surface of high-density materials, thereby enhancing the adhesion of ink on these surfaces and improving the clarity and durability of the printing effect.

[0034] The role of polyurethane resin is to provide excellent flexibility and wear resistance, enhance the elasticity and mechanical properties of the coating. It can improve the impact resistance and durability of the coating, making the coating more adaptable and stable on the surface of high-density materials, thereby ensuring that the subsequent inkjet printing ink can adhere firmly and maintain long-term effects.

[0035] In other embodiments, modified epoxy resin, polyester resin components may be added or used to replace modified acrylic resin, polyurethane resin as the film-forming substance in the composite coating.

[0036] In the above composite coating, ethyl acetate is used as a solvent, and its main function is to dissolve the resin and other components, reduce the viscosity of the coating, and make it easy to apply. Ethyl acetate has moderate volatility and can evaporate quickly during the drying process of the coating to form a uniform coating, thereby improving the smoothness and stability of the coating and ensuring that the coating can provide a good foundation for subsequent inkjet printing.

[0037] In the above composite coating, cyclohexanone is used as a solvent, and its main function is to assist in dissolving the resin and other components and adjusting the viscosity and fluidity of the coating. Cyclohexanone has a high solubility and a moderate volatilization rate, which helps to form a uniform coating and control the drying speed of the coating, thereby improving the smoothness and flatness of the coating and ensuring that the inkjet printed ink can be evenly distributed on the coating and firmly adhered.

[0038] In the above-mentioned composite coating, ethylene glycol monoethyl ether acetate is used as a solvent. Its main function is to provide a higher boiling point to control the drying speed of the coating, thereby improving the flatness and glossiness of the coating. Its slow evaporation characteristics help to form a more uniform and stable coating surface, ensuring that the coating will not have bubbles or unevenness during the coating and drying process.

[0039] In other embodiments, one or more of ethylene glycol monopropyl ether acetate, propylene glycol monomethyl ether acetate, and propylene glycol monoethyl ether acetate may be added or used to replace ethylene glycol monoethyl ether acetate as the solvent.

[0040] In the above composite coating, n-butyl acetate is used as the main solvent, and its main function is to provide excellent dissolving power, help dissolve the resin and other components, and adjust the fluidity and drying time of the coating. N-butyl acetate has a moderate volatilization rate, which ensures that the coating has good fluidity during the coating process and forms a uniform coating, thereby improving the ink adhesion and overall printing effect of inkjet printing. In other embodiments, one or more of isopropyl acetate, ethyl acetate, and propyl acetate can also be added or used to replace n-butyl acetate as the main solvent.

[0041] In the above-mentioned composite coating, the role of the isocyanate crosslinker is to form a crosslinked structure through a chemical reaction, thereby enhancing the mechanical strength, chemical resistance and wear resistance of the coating. The isocyanate crosslinker can undergo a crosslinking reaction with the resin component in the coating to form a stable and strong three-dimensional network structure. This crosslinked structure significantly improves the durability and adhesion of the coating, making it more adhesive and impact-resistant on the surface of high-density materials, thereby ensuring that the inkjet printed ink can firmly adhere to the coating and maintain long-term stability and excellent printing effects.

[0042] Preferably, the isocyanate crosslinking agent includes any one or more of hexamethylene diisocyanate trimer (HDI Trimer), isophorone diisocyanate trimer (IPDI Trimer), toluene diisocyanate trimer (TDI Trimer), and hydrogenated diphenylmethane diisocyanate trimer (H12MDI Trimer).

[0043] In the above composite coating, the tackifier is used to improve the adhesion and mechanical properties of the coating. The tackifier can increase the adhesion of the coating to the surface of high-density materials, so that the coating can firmly adhere to smooth surfaces such as acrylic and glass, thereby ensuring that the subsequent inkjet printing ink can be stably adhered. In addition, the tackifier can enhance the flexibility and wear resistance of the coating, making the coating less likely to crack or peel off under mechanical stress, thereby extending the service life of the coating.

[0044] Preferably, the tackifier comprises any one or more of polyamide resin, chlorinated polypropylene, polyisobutylene, hydrogenated rosin glycerol ester, and SIS copolymer.

[0045] In addition, in some embodiments, in order to make the coating have better adhesion and stability, 1-2% by weight of silane coupling agent and 0.1-0.5% by weight of surfactant can be added to the above composite coating. Silane coupling agent can form chemical bonds between inorganic materials (such as glass, ceramics) and organic resins (such as acrylic resins, polyurethane resins), significantly enhancing the adhesion of the coating to the surface of the substrate. By promoting the chemical bonding between the coating and the surface of the substrate, the silane coupling agent improves the mechanical strength and durability of the coating and reduces the performance degradation caused by peeling and wear. Silane coupling agent can also form a stable interface layer on the surface of the coating, increasing the weather resistance and chemical resistance of the coating. Surfactants can reduce the surface tension of the coating, allowing the coating to spread more evenly on the surface of the substrate, thereby forming a smooth and uniform coating. By reducing the surface tension of the coating, surfactants can improve the wettability of the coating to the surface of the substrate, allowing the coating to better adhere to the smooth and high-density material surface (such as acrylic and glass), and prevent the coating from having defects such as shrinkage cavities, fish eyes, pinholes, etc. during the drying process, ensuring the uniformity and flatness of the coating.

[0046] In some embodiments, before adding the silane coupling agent to the composite coating, the silane coupling agent is first microencapsulated, specifically comprising the following steps:

[0047] Dissolving a silane coupling agent in an oil phase solvent to obtain a capsule core mixed solution;

[0048] Dissolving any one or more of polylactic acid, polyvinyl alcohol, gelatin, and sodium alginate in an aqueous solvent to obtain a capsule wall mixture, and adding an emulsifier to the capsule wall mixture;

[0049] Adding the capsule core mixed liquid into the capsule wall mixed liquid and stirring to form a uniform emulsion;

[0050] A crosslinking agent is added to the emulsion, and after reacting for a first preset time, a curing agent is added and the reaction is continued for a second preset time to obtain silane coupling agent microcapsules.

[0051] Specifically, the oily solvent may be a solvent such as ethanol, isopropanol, etc., and the silane coupling agent is dissolved in the oily solvent and completely dissolved to form a uniform capsule core mixture; the aqueous solvent may be a deionized water or a water-ethanol mixed solvent, etc., and any one or more solvents selected from polylactic acid, polyvinyl alcohol, gelatin, and sodium alginate are added to the aqueous solvent, preferably, stirred at a temperature of 50-60 degrees Celsius until completely dissolved to obtain a capsule wall mixture, and an emulsifier (such as Tween 80) is added to the capsule wall mixture, and stirred evenly; then the capsule core mixture is slowly added to the capsule wall mixture, and stirred with a high-speed stirrer Preferably, the stirring speed is 1000-2000rpm, and the stirring is continued for 10-15 minutes. After a uniform emulsion is formed, a crosslinking agent, such as glutaraldehyde or CaCl2, is added to the emulsion to carry out a crosslinking reaction. The reaction time (first preset time) is 30-60 minutes, and then a curing agent (such as glutaraldehyde, etc.) is added for further curing. The reaction is continued for a second preset time, preferably 1-2 hours. Further, a filter or a centrifuge is used to separate the microcapsules from the emulsion, and the microcapsules are washed multiple times with deionized water or an appropriate solvent to remove the residual crosslinking agent and unreacted substances, and finally silane coupling agent microcapsules are obtained.

[0052] Microencapsulation technology makes silane coupling agents more stable during the mixing and storage of composite coatings by encapsulating them in tiny capsule structures, avoiding degradation and reaction caused by direct contact with air and moisture. This not only prolongs the storage life of silane coupling agents. In the actual application of composite coatings, microencapsulated silane coupling agents can gradually release their active ingredients. When the composite coating is applied to the surface of the substrate and begins to dry, the microcapsules gradually break and release the silane coupling agent. This process allows the silane coupling agent to be more evenly distributed throughout the coating, enhancing the adhesion between the coating and the substrate, especially on high-density and smooth surfaces (such as glass and metal). The adhesion effect is significantly improved. In addition, microencapsulation technology can also trigger the release of silane coupling agents under specific environmental conditions (such as temperature changes, pH changes or mechanical stress), making composite coatings more adaptable in different application scenarios. For example, in a high temperature environment, microcapsules can release silane coupling agents faster, improving the heat resistance and adhesion of the coating; in a humid environment, microcapsules can effectively prevent the hydrolysis of silane coupling agents and improve the water resistance of the coating. At the same time, since the microcapsules can control the release rate of the silane coupling agent, the problem of over-use or under-use is avoided, and the economy and use efficiency of the coating are improved.

[0053] A second aspect of the present application provides a method for preparing a composite coating for enhancing ink adhesion, characterized in that it comprises the following steps:

[0054] Weigh the following components by weight percentage: modified acrylic resin: 20-30%, polyurethane resin: 5-10%, ethyl acetate: 15%, cyclohexanone: 10%, ethylene glycol monoethyl ether acetate: 10%, n-butyl acetate: 20-30%, isocyanate crosslinking agent: 1-3%, tackifier: 5%;

[0055] Add modified acrylic resin and polyurethane resin into a container and stir, and gradually add ethyl acetate and cyclohexanone, and continue stirring until the solution is uniform;

[0056] Add ethylene glycol monoethyl ether acetate and n-butyl acetate and keep stirring;

[0057] Slowly add the isocyanate crosslinker to mix it thoroughly with the resin and solvent;

[0058] Add the tackifier and continue stirring until all components are evenly mixed to form a uniform coating solution;

[0059] Filter the mixed coating solution through a filter cloth or filter to remove insoluble impurities from the mixing process.

[0060] Preferably, during the preparation process, 1-2% by weight of a silane coupling agent and 0.1-0.5% by weight of a surfactant are also added.

[0061] The following is further described in conjunction with specific embodiments. The raw materials involved in the following specific embodiments, unless otherwise specified, can all be commercially available. The instruments used, unless otherwise specified, can all be commercially available. The processes involved, unless otherwise specified, are all routinely selected by those skilled in the art.

[0062] Example 1

[0063] 1. Raw material preparation, as shown in Table 1:

[0064] Table 1

[0065] Components Weight percentage (%) Modified acrylic resin 20 Polyurethane resin 10 Ethyl acetate 15 Cyclohexanone 10 Ethylene glycol monoethyl ether acetate 10 n-Butyl acetate 29 Isocyanate crosslinker 1 Tackifier 5

[0066] 2. Mixed resin:

[0067] Modified acrylic resin (20%) and polyurethane resin (10%) were weighed according to weight percentage.

[0068] Add the modified acrylic resin and polyurethane resin into the stirring container and start stirring. Set the stirring speed to 300-500 rpm and continue stirring for 5 minutes.

[0069] 3. Add solvent:

[0070] Under continuous stirring, ethyl acetate (15%) and cyclohexanone (10%) were gradually added. The addition time of each solvent was about 5 minutes to ensure thorough mixing. The stirring speed was maintained at 300-500 rpm for 10 minutes to ensure a uniform solution.

[0071] 4. Add other solvents:

[0072] Continue stirring and gradually add ethylene glycol monoethyl ether acetate (10%) and n-butyl acetate (29%). The addition time of each solvent is about 5 minutes. Maintain the stirring speed at 300-500rpm and stir for 15 minutes to ensure that all solvents are evenly mixed with the resin.

[0073] 5. Add cross-linking agent:

[0074] Slowly add isocyanate crosslinker (1%). The addition time of the crosslinker is about 5 minutes to ensure that it is fully mixed with the resin and solvent. Adjust the stirring speed to 200-300rpm and stir for 10 minutes to ensure uniform mixing.

[0075] 6. Adding viscosity enhancer:

[0076] Weigh the viscosity enhancer (5%) by weight and gradually add it into the stirring container. Adjust the stirring speed to 200-300 rpm and stir for 10 minutes until all components are evenly mixed.

[0077] 7. Filtering:

[0078] Filter the mixed coating solution through a filter cloth or filter (pore size 10-20 microns) to remove insoluble impurities during the mixing process. The filtered coating should be clear and free of particles.

[0079] Example 2

[0080] 1. Raw material preparation, as shown in Table 2:

[0081] Table 2

[0082] Components Weight percentage (%) Modified acrylic resin 25 Polyurethane resin 8 Ethyl acetate 15 Cyclohexanone 10 Ethylene glycol monoethyl ether acetate 10 n-Butyl acetate 25 Isocyanate crosslinker 2 Tackifier 5

[0083] 2. Mixed resin:

[0084] Modified acrylic resin (25%) and polyurethane resin (8%) were weighed according to weight percentage.

[0085] Add the modified acrylic resin and polyurethane resin into the stirring container and start stirring. Set the stirring speed to 300-500 rpm and continue stirring for 5 minutes.

[0086] 3. Add solvent:

[0087] Under continuous stirring, ethyl acetate (15%) and cyclohexanone (10%) were gradually added. The addition time of each solvent was about 5 minutes to ensure thorough mixing. The stirring speed was maintained at 300-500 rpm for 10 minutes to ensure a uniform solution.

[0088] 4. Add other solvents:

[0089] Continue stirring and gradually add ethylene glycol monoethyl ether acetate (10%) and n-butyl acetate (25%). The addition time of each solvent is about 5 minutes. Maintain the stirring speed at 300-500rpm and stir for 15 minutes to ensure that all solvents are evenly mixed with the resin.

[0090] 5. Add cross-linking agent:

[0091] Slowly add isocyanate crosslinker (2%). The addition time of the crosslinker is about 5 minutes to ensure that it is fully mixed with the resin and solvent. Adjust the stirring speed to 200-300rpm and stir for 10 minutes to ensure uniform mixing.

[0092] 6. Adding viscosity enhancer:

[0093] Weigh the viscosity enhancer (5%) by weight and gradually add it into the stirring container. Adjust the stirring speed to 200-300 rpm and stir for 10 minutes until all components are evenly mixed.

[0094] 7. Filtering:

[0095] Filter the mixed coating solution through a filter cloth or filter (pore size 10-20 microns) to remove insoluble impurities during the mixing process. The filtered coating should be clear and free of particles.

[0096] Example 3

[0097] 1. Raw material preparation: see Table 3

[0098] Table 3

[0099]

[0100]

[0101] 2. Mixed resin:

[0102] Modified acrylic resin (30%) and polyurethane resin (7%) were weighed according to weight percentage.

[0103] Add the modified acrylic resin and polyurethane resin into the stirring container and start stirring. Set the stirring speed to 300-500 rpm and continue stirring for 5 minutes.

[0104] 3. Add solvent:

[0105] Under continuous stirring, ethyl acetate (15%) and cyclohexanone (10%) were gradually added. The addition time of each solvent was about 5 minutes to ensure thorough mixing. The stirring speed was maintained at 300-500 rpm for 10 minutes to ensure a uniform solution.

[0106] 4. Add other solvents:

[0107] Continue stirring and gradually add ethylene glycol monoethyl ether acetate (10%) and n-butyl acetate (20%). The addition time of each solvent is about 5 minutes. Maintain the stirring speed at 300-500rpm and stir for 15 minutes to ensure that all solvents are evenly mixed with the resin.

[0108] 5. Add cross-linking agent:

[0109] Slowly add isocyanate crosslinker (3%). The addition time of the crosslinker is about 5 minutes to ensure that it is fully mixed with the resin and solvent. Adjust the stirring speed to 200-300rpm and stir for 10 minutes to ensure uniform mixing.

[0110] 6. Adding viscosity enhancer:

[0111] Weigh the viscosity enhancer (5%) by weight and gradually add it into the stirring container. Adjust the stirring speed to 200-300 rpm and stir for 10 minutes until all components are evenly mixed.

[0112] 7. Filtering:

[0113] Filter the mixed coating solution through a filter cloth or filter (pore size 10-20 microns) to remove insoluble impurities during the mixing process. The filtered coating should be clear and free of particles.

[0114] Example 4

[0115] In this embodiment 4, the components further include a silane coupling agent and a surfactant.

[0116] 1. Raw material preparation, see Table 4:

[0117] Table 4

[0118] Components Weight percentage (%) Modified acrylic resin 20 Polyurethane resin 10 Ethyl acetate 15 Cyclohexanone 10 Ethylene glycol monoethyl ether acetate 10 n-Butyl acetate 27.5 Isocyanate crosslinker 1 Tackifier 5 Silane coupling agent 1 Surfactants 0.5

[0119] 2. Mixed resin:

[0120] Modified acrylic resin (20%) and polyurethane resin (10%) were weighed according to weight percentage.

[0121] Add the modified acrylic resin and polyurethane resin into the stirring container and start stirring. Set the stirring speed to 300-500 rpm and continue stirring for 5 minutes.

[0122] 3. Add solvent:

[0123] Under continuous stirring, ethyl acetate (15%) and cyclohexanone (10%) were gradually added. The addition time of each solvent was about 5 minutes to ensure thorough mixing. The stirring speed was maintained at 300-500 rpm for 10 minutes to ensure a uniform solution.

[0124] 4. Add other solvents:

[0125] Continue stirring and gradually add ethylene glycol monoethyl ether acetate (10%) and n-butyl acetate (28.5%). The addition time of each solvent is about 5 minutes. Maintain the stirring speed at 300-500rpm and stir for 15 minutes to ensure that all solvents are evenly mixed with the resin.

[0126] 5. Add cross-linking agent:

[0127] Slowly add isocyanate crosslinker (1.5%). The addition time of the crosslinker is about 5 minutes to ensure that it is fully mixed with the resin and solvent. Adjust the stirring speed to 200-300rpm and stir for 10 minutes to ensure uniform mixing.

[0128] 6. Add silane coupling agent and surfactant:

[0129] Add silane coupling agent (1%) and surfactant (0.5%) and continue stirring to ensure that they are evenly dispersed in the coating.

[0130] 7. Adding tackifier:

[0131] Weigh the viscosity enhancer (5%) by weight and gradually add it into the stirring container. Adjust the stirring speed to 200-300 rpm and stir for 10 minutes until all components are evenly mixed.

[0132] 8. Filtering:

[0133] Filter the mixed coating solution through a filter cloth or filter (pore size 10-20 microns) to remove insoluble impurities during the mixing process. The filtered coating should be clear and free of particles.

[0134] Example 5

[0135] In this embodiment 5, the components further include a silane coupling agent and a surfactant.

[0136] 1. Raw material preparation, see Table 5:

[0137] Table 5

[0138] Components Weight percentage (%) Modified acrylic resin 25 Polyurethane resin 8 Ethyl acetate 15 Cyclohexanone 10 Ethylene glycol monoethyl ether acetate 10 n-Butyl acetate 23 Isocyanate crosslinker 2 Tackifier 5 Silane coupling agent 1.5 Surfactants 0.5

[0139] 2. Mixed resin:

[0140] Modified acrylic resin (25%) and polyurethane resin (8%) were weighed according to weight percentage.

[0141] Add the modified acrylic resin and polyurethane resin into the stirring container and start stirring. Set the stirring speed to 300-500 rpm and continue stirring for 5 minutes.

[0142] 3. Add solvent:

[0143] Under continuous stirring, ethyl acetate (15%) and cyclohexanone (10%) were gradually added. The addition time of each solvent was about 5 minutes to ensure thorough mixing. The stirring speed was maintained at 300-500 rpm for 10 minutes to ensure a uniform solution.

[0144] 4. Add other solvents:

[0145] Continue stirring and gradually add ethylene glycol monoethyl ether acetate (10%) and n-butyl acetate (23%). The addition time of each solvent is about 5 minutes. Maintain the stirring speed at 300-500rpm and stir for 15 minutes to ensure that all solvents are evenly mixed with the resin.

[0146] 5. Add cross-linking agent:

[0147] Slowly add isocyanate crosslinker (2%). The addition time of the crosslinker is about 5 minutes to ensure that it is fully mixed with the resin and solvent. Adjust the stirring speed to 200-300rpm and stir for 10 minutes to ensure uniform mixing.

[0148] 6. Add silane coupling agent and surfactant:

[0149] Add silane coupling agent (1.5%) and surfactant (0.5%) and continue stirring to ensure that they are evenly dispersed in the coating.

[0150] 7. Adding tackifier:

[0151] Weigh the viscosity enhancer (5%) by weight and gradually add it into the stirring container. Adjust the stirring speed to 200-300 rpm and stir for 10 minutes until all components are evenly mixed.

[0152] 8. Filtering:

[0153] Filter the mixed coating solution through a filter cloth or filter (pore size 10-20 microns) to remove insoluble impurities during the mixing process. The filtered coating should be clear and free of particles.

[0154] Example 6

[0155] In this Example 6, the components further include a silane coupling agent and a surfactant.

[0156] 1. Raw material preparation, see Table 6:

[0157] Table 6

[0158]

[0159]

[0160] 2. Mixed resin:

[0161] Modified acrylic resin (30%) and polyurethane resin (5%) were weighed according to weight percentage.

[0162] Add the modified acrylic resin and polyurethane resin into the stirring container and start stirring. Set the stirring speed to 300-500 rpm and continue stirring for 5 minutes.

[0163] 3. Add solvent:

[0164] Under continuous stirring, ethyl acetate (15%) and cyclohexanone (10%) were gradually added. The addition time of each solvent was about 5 minutes to ensure thorough mixing. The stirring speed was maintained at 300-500 rpm for 10 minutes to ensure a uniform solution.

[0165] 4. Add other solvents:

[0166] Continue stirring and gradually add ethylene glycol monoethyl ether acetate (10%) and n-butyl acetate (20.8%). The addition time of each solvent is about 5 minutes. Maintain the stirring speed at 300-500rpm and stir for 15 minutes to ensure that all solvents are evenly mixed with the resin.

[0167] 5. Add cross-linking agent:

[0168] Slowly add isocyanate crosslinker (2%). The addition time of the crosslinker is about 5 minutes to ensure that it is fully mixed with the resin and solvent. Adjust the stirring speed to 200-300rpm and stir for 10 minutes to ensure uniform mixing.

[0169] 6. Add silane coupling agent and surfactant:

[0170] Add silane coupling agent (1.5%) and surfactant (0.5%) and continue stirring to ensure that they are evenly dispersed in the coating.

[0171] 7. Adding tackifier:

[0172] Weigh the viscosity enhancer (5%) by weight and gradually add it into the stirring container. Adjust the stirring speed to 200-300 rpm and stir for 10 minutes until all components are evenly mixed.

[0173] 8. Filtering:

[0174] Filter the mixed coating solution through a filter cloth or filter (pore size 10-20 microns) to remove insoluble impurities during the mixing process. The filtered coating should be clear and free of particles.

[0175] Comparative Example 1

[0176] The components of the existing coating are shown in Table 7. This comparative example is prepared according to the existing coating components, wherein the components and weight percentages are shown in Table 8:

[0177] Table 7

[0178] Acrylic resin 25-35% Toluene 5% Xylene 10% Ethylene glycol monoethyl ether acetate 10% n-Butyl acetate 30-40%

[0179] Table 8

[0180]

[0181]

[0182] Performance comparison:

[0183] The coatings prepared in Examples 1 to 6 of the present invention and Comparative Example 1 were tested for performance, including:

[0184] Test 1: Adhesion test (ASTM D3359)

[0185] Test method: Use the cross-hatch method to test the adhesion of the coating on the substrate and score the adhesion. The adhesion score is divided into 0-5, where the higher the value, the better the surface adhesion.

[0186] Test 2: Abrasion test (ASTM D4060)

[0187] Test method: Use Taber abrasion tester to measure the wear resistance of coating. Wear resistance is expressed by abrasion rate (mg / 1000 cycles). The higher the value, the worse the surface wear resistance.

[0188] Test 3: Chemical resistance test

[0189] Test method: Expose the coating to common chemicals (such as ethanol, acetone, hydrochloric acid) and observe its stability. Chemical resistance is expressed by chemical tolerance time, and the higher the value, the better the chemical resistance.

[0190] Test 4: Drying time test

[0191] Test Method: Measure the touch-free and through-drying time of the coating at room temperature.

[0192] The test results are shown in Table 9:

[0193] Table 9

[0194]

[0195]

[0196] Result analysis:

[0197] Embodiment 1:

[0198] (1) Adhesion: The modified acrylic resin and polyurethane resin together provide basic adhesion, but due to the low content of isocyanate crosslinker, the crosslinking network is not dense enough, resulting in an adhesion score of 4.

[0199] (2) Abrasion rate: Since the polyurethane resin provides flexibility and wear resistance, and the modified acrylic resin increases the hardness of the coating, combined with the use of a tackifier, the abrasion rate is 30 mg / 1000 cycles.

[0200] (3) Chemical resistance time: The basic chemical stability of modified acrylic resin and polyurethane resin, coupled with a low content of isocyanate crosslinker, makes the chemical resistance time 40 hours.

[0201] (4) Drying time: Ethyl acetate and n-butyl acetate were used as the main solvents, and cyclohexanone and ethylene glycol monoethyl ether acetate were used to assist in controlling the volatilization rate. The surface drying time was 23 minutes and the actual drying time was 6 hours.

[0202] Embodiment 2:

[0203] (1) Adhesion: The proportion of modified acrylic resin was increased and the isocyanate crosslinker was increased to 2% to form a denser crosslinking network. The adhesion score was improved to 4.5.

[0204] (2) Wear rate: The proportion of polyurethane resin was slightly reduced, but the proportion of modified acrylic resin was increased, and the amount of isocyanate cross-linking agent was increased, and the wear rate was reduced to 29 mg / 1000 cycles.

[0205] (3) Chemical resistance time: The chemical stability is slightly improved, and the addition of isocyanate cross-linking agent extends the chemical resistance time to 42 hours.

[0206] (4) Drying time: The solvent ratio remains unchanged, but due to the change in the resin ratio, the surface drying time changes slightly to 25 minutes, and the actual drying time is shortened to 6.5 hours

[0207] Embodiment 3:

[0208] (1) Adhesion: The highest ratio of modified acrylic resin and isocyanate crosslinker formed a strong crosslinking network, and the adhesion score reached 5.

[0209] (2) Wear rate: The wear rate is further reduced to 26 mg / 1000 cycles, thanks to the high proportion of modified acrylic resin and sufficient isocyanate crosslinker.

[0210] (3) Chemical resistance time: The chemical resistance time is extended to 45 hours, showing higher chemical stability.

[0211] (4) Drying time: The solvent ratio is optimized, the drying time is shortened, the surface drying time is 24 minutes, and the actual drying time is 6 hours.

[0212] Embodiment 4:

[0213] (1) Adhesion: The addition of silane coupling agent significantly improved the chemical bonding between the coating and the substrate, and the adhesion score was increased to 5.

[0214] (2) Wear rate: Silane coupling agent and surfactant increase the mechanical strength and uniformity of the coating, and the wear rate is significantly reduced to 20 mg / 1000 cycles.

[0215] (3) Chemical resistance time: Silane coupling agent enhances chemical stability and the resistance time is increased to 50 hours.

[0216] (4) Drying time: Surfactants make the coating dry more evenly, shortening the surface drying time to 22 minutes and the actual drying time to 5.5 hours.

[0217] Embodiment 5:

[0218] (1) Adhesion: The increase in silane coupling agent content further enhances adhesion.

[0219] (2) Wear rate: The wear rate was further reduced to 18 mg / 1000 cycles, indicating that the uniform distribution of the surfactant was significant.

[0220] (3) Chemical resistance time: The chemical resistance time is extended to 52 hours, and the chemical stability is significantly enhanced.

[0221] (4) Drying time: The surface drying time and the actual drying time are further shortened, the surface drying time is 20 minutes, and the actual drying time is 5 hours.

[0222] Embodiment 6:

[0223] (1) Adhesion: The highest proportion of silane coupling agent achieves optimal adhesion.

[0224] (2) Wear rate: The wear rate is the lowest, at 16 mg / 1000 cycles, showing excellent wear resistance.

[0225] (3) Chemical resistance time: The chemical resistance time is the longest, reaching 55 hours, showing excellent chemical stability.

[0226] (4) Drying time: Both surface drying time and actual drying time are the shortest, optimizing production efficiency.

[0227] Experimental summary:

[0228] By improving the formula, many properties of the ink adhesion coating are significantly improved: 1) Adhesion: The reasonable ratio of modified acrylic resin, polyurethane resin and isocyanate crosslinker plays a key role in improving adhesion. The modified acrylic resin provides good substrate adhesion, while the polyurethane resin enhances the flexibility and mechanical strength of the coating. The isocyanate crosslinker (such as HDI trimer) undergoes a cross-linking reaction with the resin during the coating curing process to form a strong network structure, which greatly improves the adhesion of the coating. The addition of silane coupling agent further enhances the chemical bonding between the coating and the substrate, so that the adhesion score reaches 5 in Examples 4-6. 2) Wear resistance: Wear resistance is mainly affected by modified acrylic resin and polyurethane resin. The modified acrylic resin provides basic hardness, while the polyurethane resin gives the coating good flexibility and balanced mechanical properties. The introduction of the isocyanate crosslinker forms a dense structure through cross-linking, which improves the hardness and wear resistance of the coating. In Examples 4-6, the addition of silane coupling agent and surfactant further improves the mechanical strength and uniformity of the coating, significantly reduces the wear rate, and exhibits excellent wear resistance. 3) Chemical resistance: The chemical resistance of the coating is jointly affected by modified acrylic resin, polyurethane resin and isocyanate crosslinking agent. Modified acrylic resin and polyurethane resin provide basic chemical stability, while isocyanate crosslinking agent significantly improves the chemical stability and tolerance of the coating by forming a dense crosslinking network. The addition of silane coupling agent further enhances the chemical stability of the coating, significantly prolongs the chemical tolerance time of Examples 4-6, and exhibits excellent chemical resistance. 4) Drying time: The optimization of drying time is mainly achieved by adjusting the solvent system. Ethyl acetate and n-butyl acetate, as the main solvents, have a faster volatilization rate, which shortens the drying time of the coating. Cyclohexanone and ethylene glycol monoethyl ether acetate help adjust the overall volatilization rate to ensure the flatness and gloss of the coating. In Examples 4-6, the addition of surfactants makes the coating more uniform during the drying process, further shortens the surface drying and actual drying time, and improves production efficiency.

[0229] By optimizing the ratio of modified acrylic resin, polyurethane resin, isocyanate crosslinker and solvent system, and adding silane coupling agent and surfactant, the performance indicators of the coating have been significantly improved. The adhesion has been significantly enhanced, the wear resistance and chemical resistance have been greatly improved, and the drying time has been effectively shortened. These improvements not only improve the overall performance of the coating, but also significantly improve production efficiency.

[0230] A third aspect of the present application provides an image printing method, characterized in that the method comprises the following steps:

[0231] Spraying the composite coating as described in the first aspect or the composite coating prepared in the second aspect onto the surface of the printing medium to form a coating;

[0232] Control the print head to spray ink onto the coating surface to form an image

[0233] Specifically, by weight percentage, a composite coating comprising 20-30% of a modified acrylic resin, 5-10% of a polyurethane resin, 15% of ethyl acetate, 10% of cyclohexanone, 10% of ethylene glycol monoethyl ether acetate, 20-30% of n-butyl acetate, 1-3% of an isocyanate crosslinking agent, and 5% of a tackifier is obtained, or a composite coating prepared according to the composition ratio is sprayed on the surface of a printing medium (such as glass, an acrylic plate, etc.) to form a coating, and then a nozzle is controlled to spray color ink, white ink, black ink, or hot stamping ink, glossy ink, etc. onto the surface of the coating to form an image.

[0234] In another embodiment, a composite coating comprising 20-30% of a modified acrylic resin, 5-10% of a polyurethane resin, 15% of ethyl acetate, 10% of cyclohexanone, 10% of ethylene glycol monoethyl ether acetate, 20-30% of n-butyl acetate, 1-3% of an isocyanate crosslinking agent, 5% of a tackifier, 1-2% of a silane coupling agent, and 0.1-0.5% by weight of a surfactant, or a composite coating nozzle prepared according to the composition ratio forms a coating on the surface of a printing medium (such as glass, acrylic board, etc.), and then controls the nozzle to spray color ink, white ink, black ink, or hot stamping ink, glossy ink, etc. onto the coating surface to form an image.

[0235] Before spraying ink, a layer of the composite coating is sprayed on the surface of the printing medium, which can increase the roughness and affinity of the surface of the printing medium, so that the ink can be firmly attached to the printing medium.

[0236] The above is only a specific implementation of the present invention. Those skilled in the art can clearly understand that for the convenience and simplicity of description, the specific working process of the system, module and unit described above can refer to the corresponding process in the aforementioned method embodiment, and will not be repeated here. It should be understood that the protection scope of the present invention is not limited to this. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed by the present invention, and these modifications or replacements should be covered within the protection scope of the present invention.

Claims

1. A composite coating for enhancing ink adhesion, characterized in that: The composite coating comprises the following components by weight percentage: 20-30% of modified acrylic resin, 5-10% of polyurethane resin, 15% of ethyl acetate, 10% of cyclohexanone, 10% of ethylene glycol monoethyl ether acetate, 20-30% of n-butyl acetate, 1-3% of isocyanate crosslinking agent and 5% of tackifier.

2. The composite coating for enhancing ink adhesion according to claim 1, characterized in that: The isocyanate crosslinking agent includes any one or more of hexamethylene diisocyanate trimer, isophorone diisocyanate trimer, toluene diisocyanate trimer, and hydrogenated diphenylmethane diisocyanate trimer.

3. The composite coating for enhancing ink adhesion according to claim 1, characterized in that: The tackifier includes any one or more of polyamide resin, chlorinated polypropylene, polyisobutylene, hydrogenated rosin glycerol ester, and SIS copolymer.

4. The composite coating for enhancing ink adhesion according to any one of claims 1 to 3, characterized in that: The composite coating also includes: 1-2% by weight of a silane coupling agent and 0.1-0.5% by weight of a surfactant.

5. The composite coating for enhancing ink adhesion according to claim 4, characterized in that: The silane coupling agent includes any one or more of γ-aminopropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane and γ-cyanoethyltriethoxysilane.

6. The composite coating for enhancing ink adhesion according to claim 4, characterized in that: The surfactant includes any one or more of a silicone surfactant, a phosphate ester surfactant, a fatty acid soap surfactant, and a nonionic surfactant.

7. A method for preparing a composite coating for enhancing ink adhesion, characterized in that: The method comprises: Weigh the following components by weight percentage: modified acrylic resin: 20-30%, polyurethane resin: 5-10%, ethyl acetate: 15%, cyclohexanone: 10%, ethylene glycol monoethyl ether acetate: 10%, n-butyl acetate: 20-30%, isocyanate crosslinking agent: 1-3%, tackifier: 5%; Add modified acrylic resin and polyurethane resin into a container and stir; Gradually add ethyl acetate and cyclohexanone and continue stirring until the solution is homogeneous; Add ethylene glycol monoethyl ether acetate and n-butyl acetate and keep stirring; Slowly add the isocyanate crosslinker to mix it thoroughly with the resin and solvent; Add the tackifier and continue stirring until all components are evenly mixed to form a uniform coating solution; Filter the mixed coating solution through a filter cloth or filter to remove insoluble impurities from the mixing process.

8. The method for preparing a composite coating for enhancing ink adhesion according to claim 7, characterized in that: Before adding the viscosity enhancer and continuing stirring until all components are uniformly mixed to form a uniform coating solution, the method further comprises: The weight percentages are 1-2% of silane coupling agent and 0.1-0.5% of surfactant.

9. The method for preparing a composite coating for enhancing ink adhesion according to claim 8, characterized in that: Before adding 1-2% by weight of a silane coupling agent and 0.1-0.5% by weight of a surfactant, the method further comprises: The silane coupling agent is microencapsulated, specifically comprising: Dissolving the silane coupling agent in the oil phase to obtain a capsule-core mixed solution; Dissolving any one or more of polylactic acid, polyvinyl alcohol, gelatin, and sodium alginate in an aqueous phase to obtain a capsule wall mixture, and adding an emulsifier to the capsule wall mixture; Adding the capsule core mixed liquid into the capsule wall mixed liquid and stirring to form a uniform emulsion; A crosslinking agent is added to the emulsion, and after reacting for a first preset time, a curing agent is added and the reaction is continued for a second preset time to obtain silane coupling agent microcapsules.

10. An image printing method, characterized in that: The method comprises: Spraying the composite coating according to any one of claims 1 to 6 or the composite coating prepared according to claim 7 or 8 onto the surface of a printing medium to form a coating; The printing nozzle is controlled to spray ink onto the coating surface to form an image.

Citation Information

Patent Citations

  • Two-component polymer cement waterproof coating

    CN105837112A

  • Coloring layer coating capable of being used for printing laser stamping foil after cold stamping and hot stamping high-speed stamping and preparation method of coloring layer coating

    CN108276891A

  • Quick-drying coating liquid for pigment receiving layer of ink-jet printing material

    CN108641507A

  • Prime coating liquid suitable for aqueous pigment ink printed non-absorptive printing medium, and preparation method and applications thereof