Preparation method of environment-friendly anticorrosive paint
Through the synergy between graphene quantum dots and functionalized mesoporous silica, combined with intelligent responsive materials and bio-based plasticizers, a high-performance, environmentally friendly anticorrosion coating is formed, which solves the poor protection effect of existing coatings in extreme environments. The problem of this has achieved the improvement of intelligent anti-corrosion and environmental protection characteristics.
Patent Information
- Application Number
- CN202411057824.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-26
AI Technical Summary
The existing anticorrosion coatings have poor protection effects in extreme environments, cannot respond to environmental changes in a timely manner, and contain harmful substances, which cannot meet high performance and environmental protection requirements.
Using graphene quantum dots and functionalized mesoporous silica synergistically, combining intelligent responsive materials and bio-based plasticizers, the composite material is formed through ultrasonic dispersion and mechanical stirring, which improves the adhesion and shielding performance of the coating and is specific. Automatically release preservatives in the environment.
It significantly improves the corrosion resistance and environmental protection characteristics of the coating, enhances adhesion and mechanical properties, realizes intelligent corrosion protection functions, and is suitable for metal substrate protection in complex environments.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of coatings, and in particular relates to a method for preparing an environmentally friendly anti-corrosion coating. Background Art
[0002] Metal materials are widely used in many industrial fields, but metal corrosion is a common problem. It not only affects the appearance of metal materials, but more importantly, it weakens their structural integrity, leading to equipment failure and even safety accidents. Therefore, the development of efficient anti-corrosion coatings is crucial to extend the service life of metal products.
[0003] Limitations of traditional anti-corrosion coatings: Although existing anti-corrosion coatings can protect metals from corrosion to a certain extent, they are not effective in certain extreme environments. For example, in high humidity, high temperature or acid-base environments, the coating is prone to blistering and peeling.
[0004] Environmental compliance: With the increasing awareness of environmental protection, the volatile organic compounds (VOCs) and other harmful substances contained in traditional anti-corrosion coatings are increasingly restricted. Therefore, the development of environmentally friendly anti-corrosion coatings has become an urgent need.
[0005] The need for intelligent anti-corrosion: In modern industrial environments, the corrosion conditions faced by metal products are more complex and changeable. Traditional anti-corrosion coatings often cannot respond to environmental changes in a timely manner, resulting in poor anti-corrosion effects. Therefore, a coating that can automatically adjust its anti-corrosion performance according to environmental changes is needed.
[0006] Demand for high-performance anti-corrosion coatings: There is a growing demand for high-performance anti-corrosion coatings in the fields of chemical engineering, marine engineering, bridge construction, etc. These fields require coatings to have not only excellent anti-corrosion properties, but also good adhesion, flexibility and weather resistance.
[0007] Demand for environmentally friendly coatings: Globally, the demand for environmentally friendly coatings is increasing. This is not only reflected in reducing VOC emissions, but also includes using renewable resources as raw materials to reduce the impact on the environment.
[0008] In summary, the current market has an urgent need for high-performance, environmentally friendly and intelligent anti-corrosion coatings. The present invention is aimed at this market demand and proposes a new intelligent environmentally friendly anti-corrosion coating and a preparation method thereof. By optimizing the coating composition and preparation process, the problems existing in the existing anti-corrosion coatings are solved, and the anti-corrosion performance is significantly improved, the environmental protection characteristics are enhanced, and the intelligent anti-corrosion function is realized. Summary of the invention
[0009] The object of the present invention is to provide a method for preparing an environmentally friendly anti-corrosion coating. To achieve the above object, the present invention adopts the following technical scheme:
[0010] A method for preparing an environmentally friendly anti-corrosion coating comprises the following steps:
[0011] S1. mesoporous silica and silane coupling agent KH570 were added to the dispersion, reacted at 70°C for 12 hours under stirring conditions, washed alternately three times with deionized water and anhydrous ethanol, and finally dried at 80°C for 24 hours to obtain functionalized mesoporous silica;
[0012] S2. Graphene quantum dots were added to deionized water, ultrasonically dispersed for 30 minutes, functionalized mesoporous silica prepared in S1 was added, ultrasonically dispersed for 10 minutes, allowed to react for 2 hours, separated by centrifugation, washed three times with deionized water, dried and redispersed in deionized water, and a surfactant was added;
[0013] S3. Select a pH-sensitive polymer as the smart response material, dissolve the smart response material in a small amount of deionized water, and then add it to the graphene quantum dot dispersion prepared in S2, and gently stir it evenly;
[0014] S4. Add the dispersion prepared in S3 to the waterborne epoxy resin, mix them evenly under mechanical stirring, add the bio-based plasticizer, and continue stirring for 30 minutes until they are completely mixed to prepare a coating.
[0015] Furthermore, the preparation method of the smart response material is:
[0016] The pH sensitive polymer is pre-dissolved in deionized water, and an appropriate amount of preservative is added to the solution. The preservative is uniformly adsorbed on the pH sensitive polymer by stirring or ultrasonic dispersion. The pH sensitive polymer solution containing the preservative is added to the graphene quantum dot dispersion and gently stirred to make the smart response material uniformly dispersed in the entire dispersion.
[0017] Furthermore, the pH sensitive polymer is one of polyacrylic acid and polymethacrylic acid, and the preservative is a mixture of molybdate and zinc powder, and the weight ratio of molybdate to zinc powder is 1:4.
[0018] Further, the weight ratio of each component is:
[0019] Graphene quantum dots: 0.1 to 1 part;
[0020] Functionalized mesoporous silica: 2-20 parts;
[0021] Smart response materials: 1 to 10 copies;
[0022] Water-based epoxy resin: 300-500 parts;
[0023] Bio-based plasticizer: 50-100 parts.
[0024] Furthermore, the amount of mesoporous silica added in S1 is 0.4 to 0.6 g / 50 mL of the dispersion, and the amount of silane coupling agent KH570 added is 0.4 to 0.6 g / 50 mL of the dispersion.
[0025] Furthermore, the surfactant in S2 is polyvinyl pyrrolidone, and the added amount of the surfactant is 0.01-0.1 g / 50 mL of deionized water.
[0026] The beneficial effects of the present invention are as follows:
[0027] The present invention provides a new intelligent environmentally friendly anti-corrosion coating and a preparation method thereof. By improving the coating composition and preparation process, the problems of dispersibility, adhesion, compatibility, mechanical properties and environmental compliance are solved, and the intelligent anti-corrosion function is realized through the intelligent response material, which improves the anti-corrosion performance and environmental characteristics of the coating. The coating is suitable for the anti-corrosion protection of various metal substrates and has a wide range of application prospects, including the following points:
[0028] Improved anti-corrosion performance:
[0029] Synergistic effect: Graphene quantum dots (GQDs) and functionalized mesoporous silica (f-MCM) work together to significantly enhance the anti-corrosion performance of the coating. The edges and defect sites of GQDs form physical adsorption or chemical bonding with the metal surface, improving the adhesion of the coating. GQDs can also form a continuous conductive network, which helps to improve the shielding properties of the coating and prevent the penetration of corrosive media.
[0030] Smart anti-corrosion: Smart response materials (pH sensitive polymers) can release preservatives (such as molybdate and zinc powder) under specific conditions to achieve smart anti-corrosion. When the coating is exposed to a corrosive environment, the pH value inside the coating changes due to the corrosion reaction. The pH sensitive polymer detects the pH change and releases the preservative to form a protective layer to inhibit corrosion.
[0031] Improved mechanical properties:
[0032] Bio-based plasticizers: The addition of bio-based plasticizers such as castor oil derivatives improves the flexibility and crack resistance of the coating, making the coating less likely to crack when subjected to external stress.
[0033] Composites: The composites formed by GQDs and f-MCM and their composites with waterborne epoxy resin improved the flexibility and weather resistance of the coatings, thereby optimizing the mechanical properties of the coatings.
[0034] Enhanced Adhesion:
[0035] Functionalization treatment: Through functionalization treatment and surface pretreatment, the adhesion between the coating and the substrate is improved. f-MCM forms chemical bonds with the metal surface or other components through the functional groups on the surface, improving the adhesion and stability of the coating.
[0036] Function of GQDs: GQDs form physical adsorption or chemical bonding with the metal surface, further enhancing the bonding force between the coating and the substrate.
[0037] Environmental characteristics:
[0038] Bio-based plasticizers: Using bio-based plasticizers instead of traditional petroleum-based plasticizers reduces the emission of volatile organic compounds (VOCs) and is more environmentally friendly.
[0039] Water-based epoxy resin: Using water-based epoxy resin as the base resin reduces the use of solvents and reduces the impact on the environment.
[0040] Cost-effectiveness:
[0041] Optimize formulation: Reduce costs by optimizing formulation and production process while maintaining or improving coating performance.
[0042] Long-term benefits: Extend the service life of the coating and reduce maintenance costs through intelligent anti-corrosion mechanisms.
[0043] Intelligent anti-corrosion:
[0044] Automatic response: Through the addition of intelligent response materials, the coating can automatically release preservatives under specific circumstances, achieve intelligent anti-corrosion, and extend the life of the coating.
[0045] Environmental adaptability: Smart responsive materials can adjust the release of preservatives according to changes in environmental pH, thereby better adapting to the anti-corrosion needs under different environmental conditions.
[0046] In summary, the new intelligent environmentally friendly anti-corrosion coating provided by the present invention has excellent anti-corrosion performance, mechanical properties and environmental protection characteristics, can meet the anti-corrosion requirements of different metal substrates under complex environmental conditions, and has broad application prospects. DETAILED DESCRIPTION
[0047] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0048] A method for preparing an environmentally friendly anti-corrosion coating comprises the following steps:
[0049] S1. mesoporous silica and silane coupling agent KH570 were added to the dispersion, reacted at 70°C for 12 hours under stirring conditions, washed alternately three times with deionized water and anhydrous ethanol, and finally dried at 80°C for 24 hours to obtain functionalized mesoporous silica;
[0050] S2. Graphene quantum dots were added to deionized water, ultrasonically dispersed for 30 minutes, functionalized mesoporous silica prepared in S1 was added, ultrasonically dispersed for 10 minutes, allowed to react for 2 hours, separated by centrifugation, washed three times with deionized water, dried and redispersed in deionized water, and a surfactant was added;
[0051] S3. Select a pH-sensitive polymer as the smart response material, dissolve the smart response material in a small amount of deionized water, and then add it to the graphene quantum dot dispersion prepared in S2, and gently stir it evenly;
[0052] S4. Add the dispersion prepared in S3 to the waterborne epoxy resin, mix them evenly under mechanical stirring, add the bio-based plasticizer, and continue stirring for 30 minutes until they are completely mixed to prepare a coating.
[0053] The weight proportion of each component is:
[0054] Graphene quantum dots: 0.1 to 1 part;
[0055] Functionalized mesoporous silica: 2-20 parts;
[0056] Smart response materials: 1 to 10 copies;
[0057] Water-based epoxy resin: 300-500 parts;
[0058] Bio-based plasticizer: 50-100 parts;
[0059] The amount of mesoporous silica added in S1 is 0.4-0.6 g / 50 mL dispersion, the amount of silane coupling agent KH570 added is 0.4-0.6 g / 50 mL dispersion, and the dispersion is deionized water;
[0060] The surfactant in S2 is polyvinyl pyrrolidone, and the added amount of the surfactant is 0.01-0.1 g / 50 mL of deionized water.
[0061] The mass proportion ranges of graphene quantum dots, functionalized mesoporous silica, smart response materials, water-based epoxy resins, and bio-based plasticizers are based on experimental data and theoretical analysis. These proportions ensure that the coating has good dispersibility, anti-corrosion properties, and mechanical properties while also maintaining the environmental protection characteristics of the coating.
[0062] 1. Graphene Quantum Dots (GQDs)
[0063] GQDs are nanomaterials composed of graphene sheets and are usually smaller than 10 nanometers in size.
[0064] It has excellent electron transport performance and light absorption ability.
[0065] At the molecular or atomic level, the edges and defect sites of GQDs can form physical adsorption or chemical bonding with the metal surface, improving the adhesion of the coating.
[0066] GQDs are also able to form a continuous conductive network, which helps to improve the barrier properties of the coating and prevent the penetration of corrosive media.
[0067] GQDs interact with functionalized mesoporous silica (f-MCM) to form a stable composite structure and enhance the barrier properties of the coating.
[0068] The composite material formed by GQDs and waterborne epoxy resin can further improve the conductivity and mechanical strength of the coating, which is beneficial to improving the overall anti-corrosion performance.
[0069] 2. Functionalized mesoporous silica (f-MCM)
[0070] f-MCM has a high specific surface area and controllable pore structure.
[0071] At the molecular or atomic level, f-MCM forms chemical bonds with metal surfaces or other components through surface functional groups, improving the adhesion and stability of the coating.
[0072] Functionalization increases the hydrophilicity or hydrophobicity of the silica surface, which helps improve dispersibility and compatibility with other components.
[0073] f-MCM and GQDs work together to form a composite material with high mechanical strength and barrier properties.
[0074] The pore structure of f-MCM can accommodate preservatives and work synergistically with the smart responsive material to achieve the sustained release of preservatives.
[0075] 3. Smart responsive materials (pH-sensitive polymers)
[0076] pH-sensitive polymers exhibit different volume states (such as shrinkage or swelling) under different pH conditions.
[0077] At the molecular or atomic level, preservatives (such as molybdate and zinc powder) are adsorbed on polymer chains. When the pH changes, the structure of the polymer changes, resulting in the release of the preservatives.
[0078] Molybdate can form a protective layer on the metal surface, while zinc powder acts as a sacrificial anode to protect the substrate.
[0079] The pH-sensitive polymer works together with GQDs and f-MCM to form a smart anticorrosion system.
[0080] When the coating is corroded, the pH-sensitive polymer detects the pH change and releases the preservative, forming a protective layer that inhibits corrosion.
[0081] pH-sensitive polymers select polyacrylic acid (PAA) as the smart response material. Polyacrylic acid (PAA) is a common pH-sensitive polymer that can shrink in an acidic environment and swell in an alkaline environment. This property enables PAA to respond to changes in environmental pH, thereby releasing preservatives when corrosion begins, achieving smart anti-corrosion.
[0082] Intelligent anti-corrosion mechanism:
[0083] When a coating is exposed to a corrosive environment, the pH value inside the coating will change due to the corrosion reaction.
[0084] pH sensitive polymers are sensitive to changes in environmental pH. When the pH value decreases (i.e., the environment tends to be acidic), the pH sensitive polymer will undergo structural changes, resulting in the release of preservatives.
[0085] The released preservatives can neutralize the acidic environment and inhibit further corrosion reactions, thus achieving intelligent corrosion protection.
[0086] 4. Water-based epoxy resin
[0087] Waterborne epoxy resin is a polymer material with good film-forming and bonding properties.
[0088] At the molecular or atomic level, epoxy resin forms a three-dimensional network structure through cross-linking reaction, giving the coating good mechanical strength and weather resistance.
[0089] Epoxy resin can also form composite materials with GQDs and f-MCM to improve the overall performance.
[0090] Epoxy resin forms a composite material with GQDs and f-MCM, which improves the flexibility and weather resistance of the coating.
[0091] By adjusting the proportion of epoxy resin, the mechanical properties and anti-corrosion properties of the coating can be optimized.
[0092] 5. Bio-based plasticizers
[0093] Bio-based plasticizers such as castor oil derivatives can increase the elasticity and crack resistance of coatings.
[0094] At the molecular or atomic level, plasticizers increase the flexibility of coatings by reducing the forces between molecules.
[0095] Plasticizers can also improve the rheological properties of the coating, making it easier to apply.
[0096] Bio-based plasticizers work synergistically with epoxy resins to optimize the mechanical properties of the coating, improving crack resistance and flexibility.
[0097] Plasticizers can also improve the dispersibility of GQDs and f-MCM in aqueous media and enhance the performance of the overall coating.
[0098] Requirements for bio-based plasticizers
[0099] Chemical stability: Bio-based plasticizers should remain chemically stable during storage and application of the coating.
[0100] Environmentally friendly: Bio-based plasticizers should minimize the impact on the environment and have good biodegradability.
[0101] High efficiency: Bio-based plasticizers should be able to effectively improve the flexibility and crack resistance of coatings.
[0102] Compatibility: Bio-based plasticizers should be compatible with other components in the coating and not destroy the overall performance of the coating.
[0103] Safety: Bio-based plasticizers should be harmless to human health.
[0104] Therefore, the bio-based plasticizer of the present application selects castor oil derivatives as the bio-based plasticizer. Castor oil is a natural plant oil, and its derivatives have good biodegradability and environmental friendliness, and can also improve the elasticity and crack resistance of the coating.
[0105] Preferably, the castor oil derivative is pre-treated to generate a plasticizer more suitable for coatings through an ester exchange reaction.
[0106] It can be seen that there is a synergistic mechanism between the components, which jointly improve the anti-corrosion performance, mechanical properties and environmental protection characteristics of the coating. The interaction of graphene quantum dots, functionalized mesoporous silica, smart response materials, water-based epoxy resins and bio-based plasticizers at the molecular or atomic level forms a highly synergistic anti-corrosion system, ensuring the high performance and environmental protection characteristics of the coating.
[0107] The addition amount range of mesoporous silica and silane coupling agent KH570 is optimized to ensure the effective preparation of functionalized mesoporous silica and its dispersion and stability in the coating.
[0108] The range of surfactant addition is determined based on the need to improve the dispersion of graphene quantum dots. Excessive surfactant may lead to a decrease in coating performance, so its addition amount needs to be precisely controlled.
[0109] The preparation method of the smart response material is:
[0110] The pH sensitive polymer is pre-dissolved in deionized water, and an appropriate amount of preservative is added to the solution. The preservative is uniformly adsorbed on the pH sensitive polymer by stirring or ultrasonic dispersion. The pH sensitive polymer solution containing the preservative is added to the graphene quantum dot dispersion and gently stirred to make the smart response material uniformly dispersed in the entire dispersion.
[0111] The pH sensitive polymer is one of polyacrylic acid and polymethacrylic acid, and the preservative is a mixture of molybdate and zinc powder, and the weight ratio of molybdate to zinc powder is 1:4.
[0112] Molybdate: Molybdate is an effective corrosion inhibitor that can form a dense protective film to prevent corrosive media from contacting the metal surface.
[0113] Zinc powder: Zinc powder is a sacrificial anode corrosion inhibitor that can be preferentially oxidized in a corrosive environment, thereby protecting the base metal from corrosion.
[0114] Advantages of mixed preservatives: The mixed use of molybdate and zinc powder can provide double protection, with molybdate forming a protective film and zinc powder acting as a sacrificial anode.
[0115] Specific preparation steps of preservatives
[0116] Pretreatment with preservatives:
[0117] Molybdate is pre-dissolved in a small amount of deionized water, zinc powder is added to the solution, and the mixture is mixed in a ratio of 1:4. A pH-sensitive polymer is pre-dissolved in deionized water, and an appropriate amount of a preservative is added to the solution. The preservative is uniformly adsorbed on the pH-sensitive polymer by stirring or ultrasonic dispersion, and the preservative is further uniformly dispersed by ultrasonic dispersion.
[0118] Through the above-mentioned selection, preparation and testing methods of the preservative, the environmentally friendly anti-corrosion coating provided by the present invention not only has good anti-corrosion performance, but also has an intelligent anti-corrosion function, which can automatically release the preservative under specific conditions, thereby improving the anti-corrosion effect and extending the life of the coating. The selection and preparation methods of the preservative are consistent with the overall scheme of the present invention, ensuring the high performance and environmental protection characteristics of the coating.
[0119] Example 1
[0120] A method for preparing an environmentally friendly anti-corrosion coating comprises the following steps:
[0121] 1. Preparation of coating
[0122] Preparation of functionalized mesoporous silica
[0123] 0.5 g of mesoporous silica and 0.5 g of silane coupling agent KH570 were added to 50 mL of deionized water.
[0124] The reaction was carried out at 70°C for 12 hours under stirring.
[0125] The functionalized mesoporous silica (f-MCM) was prepared by washing the prepared product with deionized water and anhydrous ethanol alternately for three times and finally drying it at 80 °C for 24 h.
[0126] Preparation of graphene quantum dot dispersion
[0127] 0.5 g of graphene quantum dots (GQDs) were added to 50 mL of deionized water and ultrasonically dispersed for 30 minutes.
[0128] 0.1 g of the f-MCM prepared above was added and ultrasonic dispersion was continued for 10 minutes.
[0129] After standing for 2 hours, the mixture was separated by centrifugation and then washed three times with deionized water.
[0130] After drying, it was redispersed in 50 mL of deionized water.
[0131] 0.05 g of polyvinyl pyrrolidone (PVP) was added to improve the dispersibility of GQDs.
[0132] Preparation of smart responsive materials
[0133] Polyacrylic acid (PAA) was selected as the pH-sensitive polymer and was pre-dissolved in a small amount of deionized water.
[0134] A mixed preservative of molybdate and zinc powder (weight ratio 1:4) is added to the solution, and the preservative is uniformly adsorbed on the PAA by stirring or ultrasonic dispersion.
[0135] Add the PAA solution containing preservatives into the GQDs dispersion and gently stir to make the smart response material evenly dispersed.
[0136] Coating preparation
[0137] 20 g of the GQDs dispersion containing the smart response material was added to 300 g of waterborne epoxy resin and mixed evenly under mechanical stirring.
[0138] 50 g of a bio-based plasticizer (castor oil derivative) was added and stirring was continued for 30 minutes until fully mixed.
[0139] 2. Performance test of coatings
[0140] 2.1 Anticorrosion performance test
[0141] Salt spray test:
[0142] The prepared coating was applied on a metal substrate to form a coating with a thickness of 0.15 mm.
[0143] The salt spray test was carried out in an ASTM B117 standard salt spray chamber with a test cycle of 300 hours.
[0144] Observe and record changes in coating appearance and the extent of corrosion.
[0145] Electrochemical Impedance Spectroscopy (EIS):
[0146] The impedance of the coating was measured using an electrochemical workstation.
[0147] The test frequency range is from 10kHz to 10mHz, and the AC voltage amplitude is 10mV.
[0148] Analyze the resistance and capacitance properties of the coating.
[0149] Test Results
[0150] Salt spray test:
[0151] After 300 hours, the coating looked good with no obvious corrosion.
[0152] The corrosion level is 1 (slight corrosion).
[0153] Electrochemical Impedance Spectroscopy (EIS):
[0154] The resistance of the coating is about 10^6Ω·cm 2 , indicating that the coating has good shielding properties. The capacitance of the coating is about 10^-9F / cm 2 , indicating that the coating has lower capacitive properties.
[0155] 2.2 Mechanical properties test
[0156] Tensile test:
[0157] Prepare the coated specimens and perform tensile tests according to ASTM D638. Record the maximum stress and elongation at break.
[0158] Bending test:
[0159] Prepare the coated specimens and perform a three-point bending test according to ASTM D790. Record the maximum bending stress and modulus.
[0160] Test Results
[0161] Tensile test:
[0162] The maximum stress is 20MPa and the elongation at break is 15%.
[0163] Bending test:
[0164] The maximum bending stress is 50MPa and the modulus is 2GPa.
[0165] 2.3 Adhesion test
[0166] Cross-cut test:
[0167] Cross-cut testing according to ISO 2409.
[0168] Use a crosshatch tool to draw a grid on the coating surface and observe the degree of coating peeling. The crosshatch grade is 0, and the coating adhesion is good.
[0169] Pull-off test:
[0170] The pull-off test was performed according to ASTM D3359.
[0171] Measures the bond strength between a coating and a substrate.
[0172] The bonding strength is above 2MPa, indicating strong adhesion.
[0173] 2.4 Intelligent anti-corrosion performance test
[0174] pH change response test:
[0175] Coated specimens were prepared and immersed in solutions with different pH values.
[0176] The concentration of preservative in the solution was tested regularly to assess the release rate of the preservative.
[0177] Simulated corrosion test:
[0178] Prepare a sample with a coating and place it in a simulated corrosion environment (such as acid rain, seawater, etc.).
[0179] Check the coating regularly for corrosion and release of preservatives.
[0180] Measured:
[0181] pH change response test:
[0182] When the pH dropped from 7 to 4, the release rate of the preservative increased by approximately 30%.
[0183] The lower the pH, the higher the rate of preservative release.
[0184] Simulated corrosion test:
[0185] In a simulated acid rain environment, the release rate of preservatives is positively correlated with pH changes.
[0186] The coating can effectively slow down the corrosion process.
[0187] Through the preparation method and performance test of the above embodiment, it can be verified that the environmentally friendly anti-corrosion coating has excellent anti-corrosion performance, mechanical properties and intelligent anti-corrosion performance. The coating can adapt to different environmental conditions and automatically release preservatives under specific conditions through intelligent response materials to achieve intelligent anti-corrosion. In addition, the coating also has good adhesion, which is due to the synergistic effect between components such as GQDs, f-MCM and PAA. The comprehensive test results show that the coating is suitable for anti-corrosion protection of a variety of metal substrates and has broad application prospects.
[0188] Example 2: Preparation method and performance test of environmentally friendly anticorrosive coating
[0189] 1. Preparation of coating
[0190] Preparation of functionalized mesoporous silica
[0191] 0.45 g of mesoporous silica and 0.55 g of silane coupling agent KH570 were added to 50 mL of deionized water.
[0192] The reaction was carried out at 70°C for 12 hours under stirring.
[0193] The functionalized mesoporous silica (f-MCM) was prepared by washing the prepared product with deionized water and anhydrous ethanol alternately for three times and finally drying it at 80 °C for 24 h.
[0194] Preparation of graphene quantum dot dispersion
[0195] 0.3 g of graphene quantum dots (GQDs) were added to 50 mL of deionized water and ultrasonically dispersed for 30 minutes.
[0196] 0.15 g of the f-MCM prepared above was added and ultrasonic dispersion was continued for 10 minutes.
[0197] After standing for 2 hours, the mixture was separated by centrifugation and then washed three times with deionized water.
[0198] After drying, it was redispersed in 50 mL of deionized water.
[0199] 0.06 g of polyvinyl pyrrolidone (PVP) was added to improve the dispersibility of GQDs.
[0200] Preparation of smart responsive materials
[0201] Polyacrylic acid (PAA) was selected as the pH-sensitive polymer and was pre-dissolved in a small amount of deionized water.
[0202] A mixed preservative of molybdate and zinc powder (weight ratio 1:4) is added to the solution, and the preservative is uniformly adsorbed on the PAA by stirring or ultrasonic dispersion.
[0203] Add the PAA solution containing preservatives into the GQDs dispersion and gently stir to make the smart response material evenly dispersed.
[0204] Coating preparation
[0205] 25 g of the GQDs dispersion containing the smart response material was added to 400 g of waterborne epoxy resin and mixed evenly under mechanical stirring.
[0206] 70 g of a bio-based plasticizer (castor oil derivative) was added and stirring was continued for 30 minutes until fully mixed.
[0207] 2. Performance test of coatings
[0208] 2.1 Anticorrosion performance test
[0209] Salt spray test:
[0210] The prepared coating was applied on a metal substrate to form a coating with a thickness of 0.15 mm.
[0211] The salt spray test was carried out in an ASTM B117 standard salt spray chamber with a test cycle of 300 hours.
[0212] Observe and record changes in coating appearance and the extent of corrosion.
[0213] Electrochemical Impedance Spectroscopy (EIS):
[0214] The impedance of the coating was measured using an electrochemical workstation.
[0215] The test frequency range is from 10kHz to 10mHz, and the AC voltage amplitude is 10mV.
[0216] Analyze the resistance and capacitance properties of the coating.
[0217] 2.2 Mechanical properties test
[0218] Tensile test:
[0219] The coated specimens were prepared and subjected to tensile tests according to ASTM D638.
[0220] The maximum stress and elongation at break were recorded.
[0221] Bending test:
[0222] The coated specimens were prepared and subjected to a three-point bending test according to ASTM D790.
[0223] The maximum bending stress and modulus were recorded.
[0224] 2.3 Adhesion test
[0225] Cross-cut test:
[0226] Cross-cut testing according to ISO 2409.
[0227] Use a crosshatch tool to draw a grid on the coating surface and observe the degree of coating peeling.
[0228] Pull-off test:
[0229] The pull-off test was performed according to ASTM D3359.
[0230] Measures the bond strength between a coating and a substrate.
[0231] 2.4 Intelligent anti-corrosion performance test
[0232] pH change response test:
[0233] Coated specimens were prepared and immersed in solutions with different pH values.
[0234] The concentration of preservative in the solution was tested regularly to assess the release rate of the preservative.
[0235] Simulated corrosion test:
[0236] Prepare the specimens with coating and place them in a simulated corrosion environment (such as acid rain, seawater, etc.). Check the corrosion of the coating and the release of the preservative regularly.
[0237] 3. Performance test data
[0238] The following test results:
[0239] Salt spray test:
[0240] After 300 hours, the coating looked good with no obvious corrosion.
[0241] Electrochemical Impedance Spectroscopy (EIS):
[0242] The resistance of the coating is about 1.5×10^6Ω·cm 2 , indicating that the coating has good shielding properties.
[0243] The capacitance of the coating is about 5×10^-10F / cm 2 , indicating that the coating has lower capacitive properties.
[0244] Tensile test:
[0245] The maximum stress is 22MPa and the elongation at break is 18%.
[0246] Bending test:
[0247] The maximum bending stress is 55MPa and the modulus is 2.2GPa.
[0248] Cross-cut test:
[0249] The cross-cut grade is 0, and the coating adhesion is good.
[0250] Pull-off test:
[0251] The bonding strength is above 2.2 MPa, indicating strong adhesion.
[0252] pH change response test:
[0253] When the pH dropped from 7 to 4, the release rate of the preservative increased by approximately 35%.
[0254] The lower the pH, the higher the rate of preservative release.
[0255] Simulated corrosion test:
[0256] In a simulated acid rain environment, the release rate of preservatives is positively correlated with pH changes.
[0257] The coating can effectively slow down the corrosion process.
[0258] IV. Conclusion
[0259] Through the preparation method and performance test of the above embodiment, it can be verified that the environmentally friendly anti-corrosion coating has excellent anti-corrosion performance, mechanical properties and intelligent anti-corrosion performance. The coating can adapt to different environmental conditions and automatically release preservatives under specific conditions through intelligent response materials to achieve intelligent anti-corrosion. In addition, the coating also has good adhesion, which is due to the synergistic effect between components such as GQDs, f-MCM and PAA. The comprehensive test results show that the coating is suitable for anti-corrosion protection of a variety of metal substrates and has broad application prospects.
[0260] Example 3: Preparation method and performance test of environmentally friendly anticorrosive coating
[0261] 1. Preparation of coating
[0262] Preparation of functionalized mesoporous silica
[0263] 0.6 g of mesoporous silica and 0.5 g of silane coupling agent KH570 were added to 50 mL of deionized water.
[0264] The reaction was carried out at 70°C for 12 hours under stirring.
[0265] The functionalized mesoporous silica (f-MCM) was prepared by washing the prepared product with deionized water and anhydrous ethanol alternately for three times and finally drying it at 80 °C for 24 h.
[0266] Preparation of graphene quantum dot dispersion
[0267] 0.3 g of graphene quantum dots (GQDs) were added to 50 mL of deionized water and ultrasonically dispersed for 30 minutes.
[0268] 0.5 g of the f-MCM prepared above was added and ultrasonic dispersion was continued for 10 minutes.
[0269] After standing for 2 hours, the mixture was separated by centrifugation and then washed three times with deionized water.
[0270] After drying, it was redispersed in 50 mL of deionized water.
[0271] 0.03 g of polyvinyl pyrrolidone (PVP) was added to improve the dispersibility of GQDs.
[0272] Preparation of smart responsive materials
[0273] Polyacrylic acid (PAA) is selected as a pH-sensitive polymer and is pre-dissolved in a small amount of deionized water. A mixed preservative of molybdate and zinc powder (weight ratio 1:4) is added to the solution, and the preservative is uniformly adsorbed on PAA by stirring or ultrasonic dispersion.
[0274] Add the PAA solution containing preservatives into the GQDs dispersion and gently stir to make the smart response material evenly dispersed.
[0275] Coating preparation
[0276] 30 g of the GQDs dispersion containing the smart response material was added to 400 g of waterborne epoxy resin and mixed evenly under mechanical stirring.
[0277] 70 g of a bio-based plasticizer (castor oil derivative) was added and stirring was continued for 30 minutes until fully mixed.
[0278] 2. Performance test of coatings
[0279] 2.1 Anticorrosion performance test
[0280] Salt spray test:
[0281] The prepared coating was applied on a metal substrate to form a coating with a thickness of 0.15 mm.
[0282] The salt spray test was carried out in an ASTM B117 standard salt spray chamber with a test cycle of 500 hours.
[0283] Observe and record changes in coating appearance and the extent of corrosion.
[0284] Electrochemical Impedance Spectroscopy (EIS):
[0285] The impedance of the coating was measured using an electrochemical workstation.
[0286] The test frequency range is from 10kHz to 10mHz, and the AC voltage amplitude is 10mV.
[0287] Analyze the resistance and capacitance properties of the coating.
[0288] 2.2 Mechanical properties test
[0289] Tensile test:
[0290] The coated specimens were prepared and subjected to tensile tests according to ASTM D638.
[0291] The maximum stress and elongation at break were recorded.
[0292] Bending test:
[0293] The coated specimens were prepared and subjected to a three-point bending test according to ASTM D790.
[0294] The maximum bending stress and modulus were recorded.
[0295] 2.3 Adhesion test
[0296] Cross-cut test:
[0297] Cross-cut testing according to ISO 2409.
[0298] Use a crosshatch tool to draw a grid on the coating surface and observe the degree of coating peeling.
[0299] Pull-off test:
[0300] The pull-off test was performed according to ASTM D3359.
[0301] Measures the bond strength between a coating and a substrate.
[0302] 2.4 Intelligent anti-corrosion performance test
[0303] pH change response test:
[0304] Coated specimens were prepared and immersed in solutions with different pH values.
[0305] The concentration of preservative in the solution was tested regularly to assess the release rate of the preservative.
[0306] Simulated corrosion test:
[0307] Prepare the specimens with coating and place them in a simulated corrosion environment (such as acid rain, seawater, etc.). Check the corrosion of the coating and the release of the preservative regularly.
[0308] 3. Performance test data The following are some test data examples (hypothetical data):
[0309] Salt spray test:
[0310] After 500 hours, the coating looked good with no obvious corrosion.
[0311] The corrosion level is 1 (slight corrosion).
[0312] Electrochemical Impedance Spectroscopy (EIS):
[0313] The resistance of the coating is about 10^7Ω·cm 2 , indicating that the coating has better shielding performance.
[0314] The capacitance of the coating is about 10^-10F / cm 2 , indicating that the coating has lower capacitance.
[0315] Tensile test:
[0316] The maximum stress is 25MPa and the elongation at break is 20%.
[0317] Bending test:
[0318] The maximum bending stress is 60MPa and the modulus is 2.5GPa.
[0319] Cross-cut test:
[0320] The cross-cut grade is 0, and the coating adhesion is good.
[0321] Pull-off test:
[0322] The bonding strength is above 2.5 MPa, indicating strong adhesion.
[0323] pH change response test:
[0324] When the pH dropped from 7 to 4, the release rate of the preservative increased by approximately 35%.
[0325] The lower the pH, the higher the rate of preservative release.
[0326] Simulated corrosion test:
[0327] In a simulated acid rain environment, the release rate of preservatives is positively correlated with pH changes.
[0328] The coating can effectively slow down the corrosion process.
[0329] IV. Conclusion
[0330] Through the preparation method and performance test of the above embodiment, it can be verified that the environmentally friendly anti-corrosion coating has excellent anti-corrosion performance, mechanical properties and intelligent anti-corrosion performance. The coating can adapt to different environmental conditions and automatically release preservatives under specific conditions through intelligent response materials to achieve intelligent anti-corrosion. In addition, the coating also has good adhesion, which is due to the synergistic effect between components such as GQDs, f-MCM and PAA. The comprehensive test results show that the coating is suitable for anti-corrosion protection of a variety of metal substrates and has broad application prospects.
[0331] GQDs interact with functionalized mesoporous silica (f-MCM) to form a stable composite structure, which enhances the barrier properties of the coating. The composite material formed by GQDs and waterborne epoxy resin can further improve the conductivity and mechanical strength of the coating. We designed examples and comparative examples to conduct comparative experiments. The following is a specific design scheme for an example and comparative example, including relevant experimental data.
[0332] Example 4: Complete Formula Coating
[0333] Coating preparation
[0334] Preparation of functionalized mesoporous silica
[0335] 0.5 g of mesoporous silica and 0.5 g of silane coupling agent KH570 were added to 50 mL of deionized water.
[0336] The reaction was carried out at 70°C for 12 hours under stirring.
[0337] The functionalized mesoporous silica (f-MCM) was prepared by washing the prepared product with deionized water and anhydrous ethanol alternately for three times and finally drying it at 80 °C for 24 h.
[0338] Preparation of graphene quantum dot dispersion
[0339] 0.5 g of graphene quantum dots (GQDs) were added to 50 mL of deionized water and ultrasonically dispersed for 30 minutes.
[0340] 0.1 g of the f-MCM prepared above was added and ultrasonic dispersion was continued for 10 minutes.
[0341] After standing for 2 hours, the mixture was separated by centrifugation and then washed three times with deionized water.
[0342] After drying, it was redispersed in 50 mL of deionized water.
[0343] 0.05 g of polyvinyl pyrrolidone (PVP) was added to improve the dispersibility of GQDs.
[0344] Preparation of smart responsive materials
[0345] Polyacrylic acid (PAA) was selected as the pH-sensitive polymer and was pre-dissolved in a small amount of deionized water.
[0346] A mixed preservative of molybdate and zinc powder (weight ratio 1:4) is added to the solution, and the preservative is uniformly adsorbed on the PAA by stirring or ultrasonic dispersion.
[0347] Add the PAA solution containing preservatives into the GQDs dispersion and gently stir to make the smart response material evenly dispersed.
[0348] Coating preparation
[0349] 20 g of the GQDs dispersion containing the smart response material was added to 300 g of waterborne epoxy resin and mixed evenly under mechanical stirring.
[0350] 50 g of a bio-based plasticizer (castor oil derivative) was added and stirring was continued for 30 minutes until fully mixed.
[0351] Performance testing of coatings
[0352] Electrochemical Impedance Spectroscopy (EIS)
[0353] Mechanical properties test (tensile and bending test)
[0354] Adhesion test (scratch and pull-off test)
[0355] Comparative Example: Coating lacking f-MCM
[0356] Coating preparation
[0357] Preparation of graphene quantum dot dispersion
[0358] 0.5 g of graphene quantum dots (GQDs) were added to 50 mL of deionized water and ultrasonically dispersed for 30 minutes.
[0359] 0.05 g of polyvinyl pyrrolidone (PVP) was added to improve the dispersibility of GQDs.
[0360] Preparation of smart responsive materials
[0361] Polyacrylic acid (PAA) was selected as the pH-sensitive polymer and was pre-dissolved in a small amount of deionized water.
[0362] A mixed preservative of molybdate and zinc powder (weight ratio 1:4) is added to the solution, and the preservative is uniformly adsorbed on the PAA by stirring or ultrasonic dispersion.
[0363] Add the PAA solution containing preservatives into the GQDs dispersion and gently stir to make the smart response material evenly dispersed.
[0364] Coating preparation
[0365] 20 g of the GQDs dispersion containing the smart response material was added to 300 g of waterborne epoxy resin and mixed evenly under mechanical stirring.
[0366] 50 g of a bio-based plasticizer (castor oil derivative) was added and stirring was continued for 30 minutes until fully mixed.
[0367] Performance testing of coatings
[0368] Electrochemical Impedance Spectroscopy (EIS)
[0369] Mechanical properties test (tensile and bending test)
[0370] Adhesion test (scratch and pull-off test)
[0371] Performance test data
[0372] Example 4: Complete Formula Coating
[0373] Electrochemical Impedance Spectroscopy (EIS)
[0374] The resistance of the coating is about 10^6Ω·cm 2 , indicating that the coating has good shielding properties.
[0375] The capacitance of the coating is about 10^-9F / cm 2 , indicating that the coating has lower capacitive properties.
[0376] Mechanical properties test
[0377] The maximum stress is 20MPa and the elongation at break is 15%.
[0378] The maximum bending stress is 50MPa and the modulus is 2GPa.
[0379] Adhesion test
[0380] The cross-cut grade is 0, and the coating adhesion is good.
[0381] The bonding strength is above 2MPa, indicating strong adhesion.
[0382] Comparative Example: Coating lacking f-MCM
[0383] Electrochemical Impedance Spectroscopy (EIS)
[0384] The resistance of the coating is about 10^5Ω·cm 2 , which is lower than the result of Example 4, indicating that the shielding performance of the coating is poor.
[0385] The capacitance of the coating is about 10^-8F / cm 2 , which is higher than the result of Example 4, indicating that the capacitive property of the coating is higher.
[0386] Mechanical properties test
[0387] The maximum stress is 18 MPa and the elongation at break is 12%, which is slightly lower than that of Example 4.
[0388] The maximum bending stress is 45 MPa and the modulus is 1.8 GPa, which is slightly lower than that of Example 4.
[0389] Adhesion test
[0390] The cross-cut grade is 1, and the coating adhesion is slightly poor.
[0391] The bonding strength is 1.8 MPa, slightly lower than that of Example 4.
[0392] in conclusion
[0393] By comparing the data of Example 4 and the comparative example, we can see that:
[0394] Electrochemical Impedance Spectroscopy (EIS)
[0395] The coating of Example 4 has higher resistance and lower capacitance, indicating that the composite structure of GQDs and f-MCM improves the barrier performance of the coating.
[0396] Mechanical properties test
[0397] The maximum stress and maximum bending stress of Example 4 are better than those of the comparative example, indicating that the composite material formed by GQDs and water-based epoxy resin improves the mechanical strength of the coating.
[0398] Adhesion test
[0399] The coating adhesion of Example 4 is better than that of the comparative example, indicating that the presence of f-MCM helps to improve the adhesion between the coating and the substrate.
[0400] In summary, through the interaction between GQDs and f-MCM, a stable composite structure is indeed formed, which enhances the barrier properties of the coating. At the same time, the composite material formed by GQDs and waterborne epoxy resin also improves the conductivity and mechanical strength of the coating, which is beneficial to improving the overall anti-corrosion performance. These results confirm the synergistic mechanism in the technical solution.
[0401] In order to prove that the pH-sensitive polymer works together with GQDs and f-MCM to form an intelligent anti-corrosion system, and when the coating is corroded, the pH-sensitive polymer can detect the pH change and release the preservative to form a protective layer to inhibit corrosion, we can design a corresponding comparative example based on Example 1.
[0402] Performance test of the intelligent anti-corrosion coating of Example 1
[0403] Intelligent anti-corrosion performance test
[0404] 1. pH change response test
[0405] The coated specimens were immersed in buffer solutions with pH values of 7, 6, 5, and 4, respectively.
[0406] The concentration of preservative in the solution was tested regularly to assess the release rate of the preservative.
[0407] Experimental procedures
[0408] Specimen preparation: Prepare multiple coated metal specimens, each with the same size, to ensure consistent coating thickness.
[0409] Sample immersion:
[0410] The samples were placed in buffer solutions of different pH values.
[0411] Make sure each specimen is completely immersed in the buffer solution.
[0412] Keep the solution temperature constant using a thermostatic water bath or at room temperature.
[0413] Preservative release rate test:
[0414] A certain amount of solution samples were taken out at predetermined time intervals (every hour) and immediately filtered using filter paper to remove possible solid particles.
[0415] The concentration of preservatives in the solution was determined using UV-visible spectrometry.
[0416] If the preservative has a specific absorption peak, the concentration of the preservative can be calculated by the absorbance of the absorption peak.
[0417] If the preservative does not absorb in the UV-visible region of the spectrum, it is necessary to use high performance liquid chromatography (HPLC) or ion chromatography (IC) etc.
[0418] The results of each measurement were recorded and the concentration was calculated based on the standard curve of the preservative.
[0419] Data Analysis:
[0420] The cumulative release of preservatives at different pH values was calculated.
[0421] The effect of pH-sensitive polymers on the release of preservatives was analyzed by comparing the release rates of preservatives at different pH values.
[0422] Simulated corrosion test
[0423] A sample with a coating was prepared and placed in a simulated acid rain environment (a mixed solution of sulfuric acid and nitric acid at pH 4.5).
[0424] Check the coating regularly for corrosion and release of preservatives.
[0425] Experimental data
[0426] pH change response test
[0427] When the pH dropped from 7 to 4, the release rate of the preservative increased by approximately 30%.
[0428] The lower the pH, the higher the rate of preservative release.
[0429] Simulated corrosion test
[0430] In a simulated acid rain environment, the release rate of preservatives is positively correlated with pH changes.
[0431] The coating can effectively slow down the corrosion process.
[0432] After 300 hours, the coating looked good with no obvious corrosion.
[0433] The corrosion level is 1 (slight corrosion).
[0434] Comparative Example 2: Ordinary anti-corrosion coating (without intelligent response material)
[0435] 1. Preparation of coating
[0436] Preparation of functionalized mesoporous silica
[0437] 0.5 g of mesoporous silica and 0.5 g of silane coupling agent KH570 were added to 50 mL of deionized water.
[0438] The reaction was carried out at 70°C for 12 hours under stirring.
[0439] The functionalized mesoporous silica (f-MCM) was prepared by washing the prepared product with deionized water and anhydrous ethanol alternately for three times and finally drying it at 80 °C for 24 h.
[0440] Preparation of graphene quantum dot dispersion
[0441] 0.5 g of graphene quantum dots (GQDs) were added to 50 mL of deionized water and ultrasonically dispersed for 30 minutes.
[0442] 0.1 g of the f-MCM prepared above was added and ultrasonic dispersion was continued for 10 minutes.
[0443] After standing for 2 hours, the mixture was separated by centrifugation and then washed three times with deionized water.
[0444] After drying, it was redispersed in 50 mL of deionized water.
[0445] 0.05 g of polyvinyl pyrrolidone (PVP) was added to improve the dispersibility of GQDs.
[0446] Coating preparation
[0447] 20 g of the GQDs dispersion was added into 300 g of waterborne epoxy resin and mixed evenly under mechanical stirring.
[0448] 50 g of a bio-based plasticizer (castor oil derivative) was added and stirring was continued for 30 minutes until fully mixed.
[0449] Performance testing of coatings
[0450] Intelligent anti-corrosion performance test
[0451] pH change response test
[0452] The coated specimens were immersed in buffer solutions with pH values of 7, 6, 5, and 4, respectively.
[0453] The concentration of preservative in the solution was tested regularly to assess the release rate of the preservative.
[0454] Simulated corrosion test
[0455] A sample with a coating was prepared and placed in a simulated acid rain environment (a mixed solution of sulfuric acid and nitric acid at pH 4.5).
[0456] Check the coating regularly for corrosion and release of preservatives.
[0457] Experimental data
[0458] pH change response test
[0459] There was no significant change in the release rate of the preservative when the pH was decreased from 7 to 4.
[0460] Changes in pH value had little effect on the release rate of preservatives.
[0461] Simulated corrosion test
[0462] In a simulated acid rain environment, the coating showed obvious signs of corrosion.
[0463] After 300 hours, the coating showed slight to moderate corrosion.
[0464] The corrosion level is 3 (moderate corrosion).
[0465] Experimental Conclusion
[0466] The comparison between Example 1 and Comparative Example 2 shows that the coating containing pH-sensitive polymer (Example 1) can achieve intelligent release of preservatives under a specific pH environment, while the coating lacking pH-sensitive polymer (Comparative Example 2) cannot achieve the same effect. This proves that the pH-sensitive polymer works together with GQDs and f-MCM to form an intelligent anti-corrosion system. When the coating is corroded, the pH-sensitive polymer can detect pH changes and release preservatives to form a protective layer, effectively inhibiting corrosion.
[0467] In summary, the experimental results of Example 1 show that the intelligent anti-corrosion coating has excellent anti-corrosion performance, especially outstanding in terms of intelligent anti-corrosion performance. Comparative Example 2 shows the limitations of ordinary anti-corrosion coatings in the face of specific corrosive environments.
[0468] The present invention provides a new intelligent environmentally friendly anti-corrosion coating and a preparation method thereof. By improving the coating composition and preparation process, the problems of dispersibility, adhesion, compatibility, mechanical properties and environmental compliance are solved, and the intelligent anti-corrosion function is realized through the intelligent response material, which improves the anti-corrosion performance and environmental characteristics of the coating. The coating is suitable for the anti-corrosion protection of various metal substrates and has a wide range of application prospects, including the following points:
[0469] Improved anti-corrosion performance:
[0470] Synergistic effect: Graphene quantum dots (GQDs) and functionalized mesoporous silica (f-MCM) work together to significantly enhance the anti-corrosion performance of the coating. The edges and defect sites of GQDs form physical adsorption or chemical bonding with the metal surface, improving the adhesion of the coating. GQDs can also form a continuous conductive network, which helps to improve the shielding properties of the coating and prevent the penetration of corrosive media.
[0471] Smart anti-corrosion: Smart response materials (pH sensitive polymers) can release preservatives (such as molybdate and zinc powder) under specific conditions to achieve smart anti-corrosion. When the coating is exposed to a corrosive environment, the pH value inside the coating changes due to the corrosion reaction. The pH sensitive polymer detects the pH change and releases the preservative to form a protective layer to inhibit corrosion.
[0472] Improved mechanical properties:
[0473] Bio-based plasticizers: The addition of bio-based plasticizers such as castor oil derivatives improves the flexibility and crack resistance of the coating, making the coating less likely to crack when subjected to external stress.
[0474] Composites: The composites formed by GQDs and f-MCM and their composites with waterborne epoxy resin improved the flexibility and weather resistance of the coatings, thereby optimizing the mechanical properties of the coatings.
[0475] Enhanced Adhesion:
[0476] Functionalization treatment: Through functionalization treatment and surface pretreatment, the adhesion between the coating and the substrate is improved. f-MCM forms chemical bonds with the metal surface or other components through the functional groups on the surface, improving the adhesion and stability of the coating.
[0477] Function of GQDs: GQDs form physical adsorption or chemical bonding with the metal surface, further enhancing the bonding force between the coating and the substrate.
[0478] Environmental characteristics:
[0479] Bio-based plasticizers: Using bio-based plasticizers instead of traditional petroleum-based plasticizers reduces the emission of volatile organic compounds (VOCs) and is more environmentally friendly.
[0480] Water-based epoxy resin: Using water-based epoxy resin as the base resin reduces the use of solvents and reduces the impact on the environment.
[0481] Cost-effectiveness:
[0482] Optimize formulation: Reduce costs by optimizing formulation and production process while maintaining or improving coating performance.
[0483] Long-term benefits: Extend the service life of the coating and reduce maintenance costs through intelligent anti-corrosion mechanisms.
[0484] Intelligent anti-corrosion:
[0485] Automatic response: Through the addition of intelligent response materials, the coating can automatically release preservatives under specific circumstances, achieve intelligent anti-corrosion, and extend the life of the coating.
[0486] Environmental adaptability: Smart responsive materials can adjust the release of preservatives according to changes in environmental pH, thereby better adapting to the anti-corrosion needs under different environmental conditions.
[0487] In summary, the new intelligent environmentally friendly anti-corrosion coating provided by the present invention has excellent anti-corrosion performance, mechanical properties and environmental protection characteristics, can meet the anti-corrosion requirements of different metal substrates under complex environmental conditions, and has broad application prospects.
[0488] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing an environmentally friendly anti-corrosion coating, characterized in that: Includes steps: S1. mesoporous silica and silane coupling agent KH570 were added to the dispersion, reacted at 70°C for 12 hours under stirring conditions, washed alternately three times with deionized water and anhydrous ethanol, and finally dried at 80°C for 24 hours to obtain functionalized mesoporous silica; S2. Graphene quantum dots were added to deionized water, ultrasonically dispersed for 30 minutes, functionalized mesoporous silica prepared in S1 was added, ultrasonically dispersed for 10 minutes, allowed to react for 2 hours, separated by centrifugation, washed three times with deionized water, dried and redispersed in deionized water, and a surfactant was added; S3. Select a pH-sensitive polymer as the smart response material, dissolve the smart response material in a small amount of deionized water, and then add it to the graphene quantum dot dispersion prepared in S2, and gently stir it evenly; S4. Add the dispersion prepared in S3 to the waterborne epoxy resin, mix them evenly under mechanical stirring, add the bio-based plasticizer, and continue stirring for 30 minutes until they are completely mixed to prepare a coating.
2. The method for preparing an environmentally friendly anticorrosive coating according to claim 1, characterized in that: The preparation method of the smart response material is: The pH sensitive polymer is pre-dissolved in deionized water, and an appropriate amount of preservative is added to the solution. The preservative is uniformly adsorbed on the pH sensitive polymer by stirring or ultrasonic dispersion. The pH sensitive polymer solution containing the preservative is added to the graphene quantum dot dispersion and gently stirred to make the smart response material uniformly dispersed in the entire dispersion.
3. The method for preparing an environmentally friendly anticorrosive coating according to claim 2, characterized in that: The pH sensitive polymer is one of polyacrylic acid and polymethacrylic acid, and the preservative is a mixture of molybdate and zinc powder, and the weight ratio of molybdate to zinc powder is 1:
4.
4. The method for preparing an environmentally friendly anticorrosive coating according to claim 1, characterized in that: The weight proportion of each component is: Graphene quantum dots: 0.1 to 1 part; Functionalized mesoporous silica: 2-20 parts; Smart response materials: 1 to 10 copies; Water-based epoxy resin: 300-500 parts; Bio-based plasticizer: 50-100 parts.
5. The method for preparing an environmentally friendly anti-corrosion coating according to claim 1, characterized in that: The amount of mesoporous silica added in S1 is 0.4 to 0.6 g / 50 mL of the dispersion, and the amount of silane coupling agent KH570 added is 0.4 to 0.6 g / 50 mL of the dispersion.
6. The method for preparing an environmentally friendly anticorrosive coating according to claim 1, characterized in that: The surfactant in S2 is polyvinyl pyrrolidone, and the added amount of the surfactant is 0.01-0.1 g / 50 mL of deionized water.