Environment-friendly AF film and preparation method thereof

By combining chitosan, tea polyphenols with citric acid and polylactic acid and other materials, environmentally friendly AF films are prepared, which solves the problem of the lack of degradability of existing AF films, and realizes the preparation of environmentally friendly AF films, and has good Anti-fouling, scratch-proof performance and high degradation rate.

CN119019939APending Publication Date: 2024-11-26XINFENG JIELI ELECTRICAL MATERIALS CO LTD

Patent Information

Application Number
CN202411293801.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing AF membrane has excellent anti-fouling and scratch resistance but lacks degradable and environmentally friendly properties, and there is a problem that the material is not environmentally friendly.

Method used

Use chitosan and glycerin to mix, tea polyphenols dissolved with citric acid, combined with polylactic acid and ethylenediamine to react, add isocyanate groups, prepare an environmentally friendly film layer, and apply epoxy resin glue and AF layer on the surface of the substrate , an environmentally friendly AF film is formed by drying.

Benefits of technology

The preparation of environmentally friendly AF film has been realized, with good biodegradability and wear resistance, simple operation, low cost, high production efficiency, and a degradation rate of 94-98%.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of AF films, and discloses an environment-friendly AF film and a preparation method thereof.The preparation method comprises the steps that chitosan and glycerin are mixed to obtain a solution A, tea polyphenol and citric acid are mixed to obtain a solution B, and the solution A and the solution B are mixed to obtain a tea polyphenol-chitosan film; the preparation method comprises the following steps: reacting polylactic acid with ethylenediamine to obtain aminated polylactic acid, and then introducing an isocyanate group to react with a tea polyphenol-chitosan membrane to obtain the environment-friendly membrane. The surface of the base material film is coated with glue, then the environment-friendly film layer is pasted, then the AF layer is plated, drying is conducted, and the environment-friendly AF film is obtained; the degradable environment-friendly plastic has good degradable and environment-friendly performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of AF films, in particular to an environmentally friendly AF film and a preparation method thereof. Background Art

[0002] AF film is a high-transmittance anti-fingerprint and anti-oil film. It is a layer of AF anti-fingerprint coating sprayed on the surface of the substrate through AF spraying technology. After the AF anti-fingerprint coating contacts the substrate, a film layer with a certain thickness is formed to strengthen the molecular structure and ensure the excellent anti-fouling and anti-scratch properties of the substrate surface. Its main features are: anti-fouling, excellent anti-fouling effect, fingerprints and oil stains are not easy to adhere and can be easily wiped off; anti-scratch, smooth surface, prevent surface scratches; thin film layer, uniform ultra-thin coating, does not change the original texture and optical properties of the substrate; wear-resistant, has good wear resistance. Summary of the invention

[0003] 1. Technical issues to be resolved

[0004] In view of the deficiencies of the prior art, the present invention provides an environmentally friendly AF film and a preparation method thereof, which has good degradability and environmental protection performance.

[0005] (II) Technical solution

[0006] To achieve the above object, the present invention provides the following technical solution: a method for preparing an environmentally friendly AF film, the method for preparing the environmentally friendly AF film comprising the following steps:

[0007] (1) dissolving chitosan in an acetic acid solution at 50-70° C., and then adding glycerol thereto to obtain a mixed solution A; dissolving 10-15 g of tea polyphenols and 8-12 g of citric acid in pure water, stirring to obtain a mixed solution B; fully mixing the mixed solution A and the mixed solution B, and ultrasonically degassing for 2-4 hours to obtain a tea polyphenol-chitosan film;

[0008] (2) adding polylactic acid to dichloromethane to dissolve it, introducing nitrogen, activating it at 2-6° C. for 2-4 hours, and then adding ethylenediamine, N-hydroxysuccinimide, and dicyclohexylcarbodiimide to it, reacting it at 30-40° C. for 20-30 hours, distilling it under reduced pressure after the reaction, filtering, washing and drying to obtain amino polylactic acid;

[0009] (3) adding amino polylactic acid to N,N-dimethylformamide solvent to dissolve it, and then adding tea polyphenol-chitosan film, 2,4-toluene diisocyanate, and dibutyltin dilaurate catalyst, reacting at 50-70° C. for 3-6 hours, and distilling under reduced pressure after the reaction, filtering, washing and drying to obtain an environmentally friendly film layer;

[0010] (4) Apply glue to the surface of the substrate film, attach the environmentally friendly film layer, and then plate the AF layer and dry it at 60-90° C. for 2-4 hours to obtain an environmentally friendly AF film.

[0011] Preferably, the mass ratio of chitosan to glycerol in (1) is 1.2-1.5:1.

[0012] Preferably, the mass ratio of the mixed solution A to the mixed solution B in (1) is 1.1-1.3:1.

[0013] Preferably, the mass ratio of polylactic acid, ethylenediamine, N-hydroxysuccinimide and dicyclohexylcarbodiimide in (2) is 2.1-2.5:1:0.02-0.04:0.03-0.05.

[0014] Preferably, the mass ratio of the amino polylactic acid, tea polyphenol-chitosan film, 2,4-toluene diisocyanate and dibutyltin dilaurate catalyst in (3) is 1.3-1.6:1:0.02-0.04:0.05-0.08.

[0015] Preferably, the glue in (4) is epoxy resin glue.

[0016] Preferably, the substrate film in (4) is a polyethylene film.

[0017] Preferably, the compound is obtained by the preparation method according to any one of claims 1 to 6.

[0018] (III) Beneficial technical effects

[0019] The invention comprises the following steps: mixing chitosan and glycerol to obtain solution A, mixing tea polyphenol and citric acid to obtain solution B, and mixing solution A and solution B to obtain a tea polyphenol-chitosan film; reacting polylactic acid and ethylenediamine to obtain amino polylactic acid, and then introducing isocyanate groups to react with the tea polyphenol-chitosan film to obtain an environmentally friendly film; coating the surface of the substrate film with glue, attaching an environmentally friendly film layer, and then coating an AF layer and drying the layer to obtain the environmentally friendly AF film.

[0020] The chitosan and polylactic acid of the present invention have good biodegradability and act synergistically with the polylactic acid on the AF film. The present invention has simple operation process, low cost and high production efficiency. DETAILED DESCRIPTION

[0021] Example 1

[0022] (1) Dissolving chitosan in an acetic acid solution at 50° C., and then adding glycerol thereto, wherein the mass ratio of chitosan to glycerol is 1.2:1, to obtain a mixed solution A; dissolving 10 g of tea polyphenols and 8 g of citric acid in pure water, dissolving, and stirring to obtain a mixed solution B; fully mixing the mixed solution A and the mixed solution B, wherein the mass ratio of the mixed solution A to the mixed solution B is 1.1:1, and ultrasonically degassing for 2 h to obtain a tea polyphenol-chitosan film;

[0023] (2) adding polylactic acid to dichloromethane to dissolve it, introducing nitrogen, activating it at 2° C. for 2 hours, and then adding ethylenediamine, N-hydroxysuccinimide, and dicyclohexylcarbodiimide, wherein the mass ratio of polylactic acid, ethylenediamine, N-hydroxysuccinimide, and dicyclohexylcarbodiimide is 2.1:1:0.02:0.03, reacting at 30° C. for 20 hours, distilling under reduced pressure after the reaction, filtering, washing, and drying to obtain amino polylactic acid;

[0024] (3) adding amino polylactic acid to N,N-dimethylformamide solvent for dissolution, and then adding tea polyphenol-chitosan film, 2,4-toluene diisocyanate, and dibutyltin dilaurate catalyst, wherein the mass ratio of amino polylactic acid, tea polyphenol-chitosan film, 2,4-toluene diisocyanate, and dibutyltin dilaurate catalyst is 1.3:1:0.02:0.05, reacting at 50° C. for 3 h, distilling under reduced pressure after the reaction, filtering, washing and drying to obtain an environmentally friendly film layer;

[0025] (4) Epoxy resin glue is applied to the surface of the substrate film, and then an environmentally friendly film layer is attached, and then an AF layer is plated and dried at 60° C. for 2 h to obtain an environmentally friendly AF film.

[0026] Example 2

[0027] (1) Dissolving chitosan in an acetic acid solution at 70° C., and then adding glycerol thereto, wherein the mass ratio of chitosan to glycerol is 1.5:1, to obtain a mixed solution A; dissolving 15 g of tea polyphenols and 12 g of citric acid in pure water, dissolving, and stirring to obtain a mixed solution B; fully mixing the mixed solution A and the mixed solution B, wherein the mass ratio of the mixed solution A to the mixed solution B is 1.3:1, and ultrasonically degassing for 4 hours to obtain a tea polyphenol-chitosan film;

[0028] (2) adding polylactic acid to dichloromethane to dissolve it, introducing nitrogen, activating it at 6° C. for 4 hours, and then adding ethylenediamine, N-hydroxysuccinimide, and dicyclohexylcarbodiimide, wherein the mass ratio of polylactic acid, ethylenediamine, N-hydroxysuccinimide, and dicyclohexylcarbodiimide is 2.5:1:0.04:0.05, reacting at 40° C. for 30 hours, distilling under reduced pressure after the reaction, filtering, washing, and drying to obtain amino polylactic acid;

[0029] (3) adding amino polylactic acid to N,N-dimethylformamide solvent for dissolution, and then adding tea polyphenol-chitosan film, 2,4-toluene diisocyanate, and dibutyltin dilaurate catalyst, wherein the mass ratio of amino polylactic acid, tea polyphenol-chitosan film, 2,4-toluene diisocyanate, and dibutyltin dilaurate catalyst is 1.6:1:0.04:0.08, reacting at 70° C. for 6 hours, distilling under reduced pressure after the reaction, filtering, washing and drying to obtain an environmentally friendly film layer;

[0030] (4) Epoxy resin glue is applied to the surface of the substrate film, and then an environmentally friendly film layer is attached, and then an AF layer is plated and dried at 90° C. for 4 h to obtain an environmentally friendly AF film.

[0031] Example 3

[0032] (1) Dissolving chitosan in an acetic acid solution at 60° C., and then adding glycerol thereto, wherein the mass ratio of chitosan to glycerol is 1.35:1, to obtain a mixed solution A; dissolving 12.5 g of tea polyphenols and 10 g of citric acid in pure water, dissolving, and stirring to obtain a mixed solution B; fully mixing the mixed solution A and the mixed solution B, wherein the mass ratio of the mixed solution A to the mixed solution B is 1.2:1, and ultrasonically degassing for 3 h to obtain a tea polyphenol-chitosan film;

[0033] (2) adding polylactic acid to dichloromethane to dissolve it, introducing nitrogen, activating it at 4° C. for 3 hours, and then adding ethylenediamine, N-hydroxysuccinimide, and dicyclohexylcarbodiimide, wherein the mass ratio of polylactic acid, ethylenediamine, N-hydroxysuccinimide, and dicyclohexylcarbodiimide is 2.3:1:0.03:0.04, reacting at 30-40° C. for 25 hours, and distilling under reduced pressure after the reaction, filtering, washing, and drying to obtain amino polylactic acid;

[0034] (3) adding amino polylactic acid to N,N-dimethylformamide solvent for dissolution, and then adding tea polyphenol-chitosan film, 2,4-toluene diisocyanate, and dibutyltin dilaurate catalyst, wherein the mass ratio of amino polylactic acid, tea polyphenol-chitosan film, 2,4-toluene diisocyanate, and dibutyltin dilaurate catalyst is 1.45:1:0.03:0.00.065, reacting at 60° C. for 4.5 hours, distilling under reduced pressure after the reaction, filtering, washing and drying to obtain an environmentally friendly film layer;

[0035] (4) Epoxy resin glue is applied to the surface of the substrate film, and then an environmentally friendly film layer is attached, and then an AF layer is plated and dried at 75° C. for 3 h to obtain an environmentally friendly AF film.

[0036] Example 4

[0037] (1) Dissolving chitosan in an acetic acid solution at 50° C., and then adding glycerol thereto, wherein the mass ratio of chitosan to glycerol is 1.2:1, to obtain a mixed solution A; dissolving 10 g of tea polyphenols and 8 g of citric acid in pure water, dissolving, and stirring to obtain a mixed solution B; fully mixing the mixed solution A and the mixed solution B, wherein the mass ratio of the mixed solution A to the mixed solution B is 1.1:1, and ultrasonically degassing for 2 h to obtain a tea polyphenol-chitosan film;

[0038] (2) adding polylactic acid to dichloromethane to dissolve it, introducing nitrogen, activating it at 2° C. for 2 hours, and then adding ethylenediamine, N-hydroxysuccinimide, and dicyclohexylcarbodiimide, wherein the mass ratio of polylactic acid, ethylenediamine, N-hydroxysuccinimide, and dicyclohexylcarbodiimide is 2.1:1:0.02:0.03, reacting at 30° C. for 20 hours, distilling under reduced pressure after the reaction, filtering, washing, and drying to obtain amino polylactic acid;

[0039] (3) adding amino polylactic acid to N,N-dimethylformamide solvent for dissolution, and then adding tea polyphenol-chitosan film, 2,4-toluene diisocyanate, and dibutyltin dilaurate catalyst, wherein the mass ratio of amino polylactic acid, tea polyphenol-chitosan film, 2,4-toluene diisocyanate, and dibutyltin dilaurate catalyst is 1.6:1:0.04:0.08, reacting at 70° C. for 6 hours, distilling under reduced pressure after the reaction, filtering, washing and drying to obtain an environmentally friendly film layer;

[0040] (4) Epoxy resin glue is applied to the surface of the substrate film, and then an environmentally friendly film layer is attached, and then an AF layer is plated and dried at 90° C. for 2 h to obtain an environmentally friendly AF film.

[0041] Example 5

[0042] (1) Dissolving chitosan in an acetic acid solution at 70° C., and then adding glycerol thereto, wherein the mass ratio of chitosan to glycerol is 1.5:1, to obtain a mixed solution A; dissolving 15 g of tea polyphenols and 12 g of citric acid in pure water, dissolving, and stirring to obtain a mixed solution B; fully mixing the mixed solution A and the mixed solution B, wherein the mass ratio of the mixed solution A to the mixed solution B is 1.3:1, and ultrasonically degassing for 4 hours to obtain a tea polyphenol-chitosan film;

[0043] (2) adding polylactic acid to dichloromethane to dissolve it, introducing nitrogen, activating it at 6° C. for 4 hours, and then adding ethylenediamine, N-hydroxysuccinimide, and dicyclohexylcarbodiimide, wherein the mass ratio of polylactic acid, ethylenediamine, N-hydroxysuccinimide, and dicyclohexylcarbodiimide is 2.5:1:0.04:0.05, reacting at 40° C. for 30 hours, distilling under reduced pressure after the reaction, filtering, washing, and drying to obtain amino polylactic acid;

[0044] (3) adding amino polylactic acid to N,N-dimethylformamide solvent for dissolution, and then adding tea polyphenol-chitosan film, 2,4-toluene diisocyanate, and dibutyltin dilaurate catalyst, wherein the mass ratio of amino polylactic acid, tea polyphenol-chitosan film, 2,4-toluene diisocyanate, and dibutyltin dilaurate catalyst is 1.45:1:0.03:0.00.065, reacting at 60° C. for 4.5 hours, distilling under reduced pressure after the reaction, filtering, washing and drying to obtain an environmentally friendly film layer;

[0045] (4) Epoxy resin glue is applied to the surface of the substrate film, and then an environmentally friendly film layer is attached, and then an AF layer is plated and dried at 80° C. for 4 h to obtain an environmentally friendly AF film.

[0046] Example 6

[0047] (1) Dissolving chitosan in an acetic acid solution at 60° C., and then adding glycerol thereto, wherein the mass ratio of chitosan to glycerol is 1.35:1, to obtain a mixed solution A; dissolving 12.5 g of tea polyphenols and 10 g of citric acid in pure water, dissolving, and stirring to obtain a mixed solution B; fully mixing the mixed solution A and the mixed solution B, wherein the mass ratio of the mixed solution A to the mixed solution B is 1.2:1, and ultrasonically degassing for 3 h to obtain a tea polyphenol-chitosan film;

[0048] (2) adding polylactic acid to dichloromethane to dissolve it, introducing nitrogen, activating it at 4° C. for 3 hours, and then adding ethylenediamine, N-hydroxysuccinimide, and dicyclohexylcarbodiimide, wherein the mass ratio of polylactic acid, ethylenediamine, N-hydroxysuccinimide, and dicyclohexylcarbodiimide is 2.3:1:0.03:0.04, reacting at 30-40° C. for 25 hours, and distilling under reduced pressure after the reaction, filtering, washing, and drying to obtain amino polylactic acid;

[0049] (3) adding amino polylactic acid to N,N-dimethylformamide solvent for dissolution, and then adding tea polyphenol-chitosan film, 2,4-toluene diisocyanate, and dibutyltin dilaurate catalyst, wherein the mass ratio of amino polylactic acid, tea polyphenol-chitosan film, 2,4-toluene diisocyanate, and dibutyltin dilaurate catalyst is 1.3:1:0.02:0.05, reacting at 50° C. for 3 h, distilling under reduced pressure after the reaction, filtering, washing and drying to obtain an environmentally friendly film layer;

[0050] (4) Epoxy resin glue is applied to the surface of the substrate film, and then an environmentally friendly film layer is attached, and then an AF layer is plated and dried at 60° C. for 4 h to obtain an environmentally friendly AF film.

[0051] Comparative Example 1

[0052] (1) The AF layer is plated on the surface of the substrate film and then dried at 90°C for 4 hours to obtain an environmentally friendly AF film

[0053] The degradation rate test was performed on Examples 1-6 of the present invention and Comparative Example 1. The test results are shown in Table 1.

[0054] project Degradation rate (%) Example 1 98 Example 2 94 Example 3 97 Example 4 99 Example 5 96 Example 6 98 Comparative Example 1 60

[0055] As can be seen from Table 1, the degradation rates of Examples 1-6 of the present invention reach 94-98%.

[0056] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing an environmentally friendly AF film, characterized in that: The method for preparing the environmentally friendly AF film comprises the following steps: (1) dissolving chitosan in an acetic acid solution at 50-70° C., and then adding glycerol thereto to obtain a mixed solution A; dissolving 10-15 g of tea polyphenols and 8-12 g of citric acid in pure water, stirring to obtain a mixed solution B; fully mixing the mixed solution A and the mixed solution B, and ultrasonically degassing for 2-4 hours to obtain a tea polyphenol-chitosan film; (2) adding polylactic acid to dichloromethane to dissolve it, introducing nitrogen, activating it at 2-6° C. for 2-4 hours, and then adding ethylenediamine, N-hydroxysuccinimide, and dicyclohexylcarbodiimide to it, reacting it at 30-40° C. for 20-30 hours, distilling it under reduced pressure after the reaction, filtering, washing and drying to obtain amino polylactic acid; (3) adding amino polylactic acid to N,N-dimethylformamide solvent to dissolve it, and then adding tea polyphenol-chitosan film, 2,4-toluene diisocyanate, and dibutyltin dilaurate catalyst, reacting at 50-70° C. for 3-6 hours, and distilling under reduced pressure after the reaction, filtering, washing and drying to obtain an environmentally friendly film layer; (4) Apply glue to the surface of the substrate film, attach the environmentally friendly film layer, and then plate the AF layer and dry it at 60-90° C. for 2-4 hours to obtain an environmentally friendly AF film.

2. The method for preparing the environmentally friendly AF film according to claim 1, characterized in that: The mass ratio of chitosan to glycerol in (1) is 1.2-1.5:

1.

3. The method for preparing the environmentally friendly AF film according to claim 1, characterized in that: The mass ratio of the mixed solution A to the mixed solution B in (1) is 1.1-1.3:

1.

4. The method for preparing the environmentally friendly AF film according to claim 1, characterized in that: The mass ratio of polylactic acid, ethylenediamine, N-hydroxysuccinimide and dicyclohexylcarbodiimide in (2) is 2.1-2.5:1:0.02-0.04:0.03-0.

05.

5. The method for preparing the environmentally friendly AF film according to claim 1, characterized in that: The mass ratio of the amino polylactic acid, tea polyphenol-chitosan film, 2,4-toluene diisocyanate and dibutyltin dilaurate catalyst in (3) is 1.3-1.6:1:0.02-0.04:0.05-0.

08.

6. The method for preparing the environmentally friendly AF film according to claim 1, characterized in that: The glue in (4) is epoxy resin glue.

7. The method for preparing the environmentally friendly AF film according to claim 1, characterized in that: The substrate film in (4) is a polyethylene film.

8. An environmentally friendly AF film, characterized in that: The preparation method according to any one of claims 1 to 7 is used to obtain the product.

Citation Information

Patent Citations

  • Method for preparing chitosan-based anti-oxidant composite membrane based on tea polyphenol

    CN106188588A

  • Preparation method of degradable food packaging film

    CN108864670A

Cited By

  • Hydrophobic EC outside rear-view mirror

    CN223618651U