Water-based adhesive applied to wood and bamboo

By using a combination of natural latex and water-soluble polymers and curing agents, the problem of carcinogenic risk of petrochemical raw materials in wood and bamboo adhesion agents is solved, providing efficient water resistance and subsequent strength, and reducing dependence on petrochemical products and The goal of environmental protection and non-toxicity.

CN119019952APending Publication Date: 2024-11-26ALLIANCE MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310583064.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Petrochemical raw materials used in existing wood and bamboo adhesion agents, especially formaldehyde, pose a carcinogenic risk to human health and the environment, and their alternative materials such as soy protein, lignin and starch are not good in water resistance and adhesion. Difficult to widely use.

Method used

Natural latex is used as the main material, combining water-soluble polymers with appropriate curing agents such as isocyanate or quaternary ammonium salt polymers to form an aqueous adhesion agent to ensure water resistance, follow-up strength and mechanical strength of wood and bamboo.

Benefits of technology

This aqueous adhesion agent effectively reduces dependence on petrochemical products, provides good water resistance and subsequent strength, meets the requirements of environmental protection and non-toxicity, and demonstrates its excellent performance under different conditions through specific examples.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004242291270000051
    Figure BDA0004242291270000051
  • Figure BDA0004242291270000071
    Figure BDA0004242291270000071
  • Figure BDA0004242291270000081
    Figure BDA0004242291270000081
Patent Text Reader

Abstract

The invention relates to a water-based adhesive applied to wood or bamboo wood. The water-based adhesive comprises a main agent and a curing agent, wherein the main agent consists of a water-soluble polymer, synthetic rubber latex and natural latex; and the curing agent is selected from isocyanate or quaternary ammonium salt polymer. The adhesive is characterized in that the weight ratio of the main agent to the curing agent is between 200: 1 and 1: 1; and the water-soluble polymer is polyvinyl alcohol and accounts for 2-30 weight percent of the total solid content of the main agent. And the synthetic rubber latex accounts for 2-60 weight percent of the total solid content of the main agent. And the natural latex accounts for 5-90 weight percent of the total solid content of the main agent. The invention provides a formaldehyde-free adhesive, and natural and renewable raw materials are introduced to reduce the dependence on petrochemical products and improve the sustainability of related industries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an adhesive, in particular to a water-based adhesive used for wood and bamboo. Background Art

[0002] Traditionally, adhesives used for wood and bamboo are mostly petrochemical products, such as phenol, urea, melamine, formaldehyde, etc. Adhesives made from these petrochemical raw materials or their derivatives often provide good adhesion, mechanical strength, temperature resistance and water resistance, and their low cost and affordable price make them difficult to replace. However, with the rise of environmental awareness and the emphasis on human health, the disadvantages of adhesives made from petrochemical raw materials have gradually been clearly pointed out.

[0003] Since formaldehyde has good reactivity, urea formaldehyde resin adhesive containing formaldehyde usually has advantages such as high adhesion, good temperature resistance and good water resistance. Currently, more than 80% of adhesives used for wood and bamboo still use urea formaldehyde glue, but formaldehyde has been confirmed to be a toxic substance with carcinogenic risks to the human body. In addition, wood and bamboo made of adhesives containing formaldehyde are used in various furniture, indoor building materials, interior decoration, etc., and the emission period of formaldehyde can reach 10 to 15 years.

[0004] Countries around the world are increasingly tightening regulations on formaldehyde content that has carcinogenic risks. Developing new types of bio-based formaldehyde-free adhesives that can improve ecological sustainability and reduce harm to the human body has become a clear goal.

[0005] In addition to not using formaldehyde, formaldehyde-free bio-based adhesives also introduce bio-based materials. In recent years, soy protein, lignin, starch, and tannins are bio-based materials that are often used in wood adhesives. However, due to its shortcomings such as weak bonding strength and poor water resistance, it has not yet been widely used in commercial applications. Among them, soy protein has been used in wood bonding since the 1930s, but its poor bonding strength has always been criticized. U.S. Patent No. US9493693 discloses related improvements, but actual commercial applications still have problems such as high heating temperature, long time, and energy consumption. In practice, soy protein has the problem of difficult processing and operation, and operators are difficult to adapt to.

[0006] In addition, although lignin and tannin have good structural stability, it also means that their reactivity is low, and they usually need to be chemically modified to increase reactivity. Lignin itself contains phenol functional groups (phenol), which are often used to add to phenolic resins. Its disadvantages are poor reactivity, high reaction temperature and poor water resistance. Starch is a natural polymer and is often used as a food additive. Hydrogen bonds are its main force, but the hydrogen bond force is much weaker than the general chemical reaction covalent bond. Starch is used as a glue, but it performs poorly in water resistance and adhesion. Although there are modified starches to increase chemical reaction covalent bonds, water resistance and adhesion still do not meet commercial requirements. Summary of the invention

[0007] In view of the shortcomings of the prior art, the present invention mainly provides a water-based adhesive that can be applied to wood or bamboo, introduces natural renewable raw materials, effectively reduces dependence on petrochemical products and improves the sustainability of related industries.

[0008] An object of the present invention is to provide a water-based adhesive that can be applied to wood or bamboo. The biomass material is natural latex, which is combined with an environmentally friendly and non-toxic water-soluble polymer and a suitable curing agent, such as isocyanate or quaternary ammonium salt polymer, to provide wood and bamboo with good water resistance, bonding strength and mechanical strength.

[0009] One object of the present invention is to provide an adhesive that can be applied to wood and bamboo, which is composed of a main agent and a curing agent. The main agent includes a water-soluble polymer, synthetic rubber latex, and natural latex. The curing agent is an isocyanate compound or its polymer or a quaternary ammonium salt polymer aqueous solution.

[0010] According to the above purpose, the present invention discloses a water-based adhesive that can be applied to wood or bamboo, including a main agent composed of a water-soluble polymer, a synthetic rubber latex and a natural latex, and a curing agent selected from isocyanate or a quaternary ammonium salt polymer. It is characterized in that the weight ratio of the main agent to the curing agent is between 200:1 and 1:1. The water-soluble polymer is polyvinyl alcohol, which accounts for 2-30 weight percent of the total solid amount of the main agent. The synthetic rubber latex is selected from the group consisting of styrene-butadiene rubber latex and styrene-butadiene rubber latex containing carboxylic acid functional groups, and the synthetic rubber latex accounts for 2-60 weight percent of the total solid amount of the main agent. Natural latex accounts for 5-90 weight percent of the total solid amount of the main agent.

[0011] In a preferred embodiment of the present invention, the weight ratio of the main agent to the curing agent is between 100:1 and 10:3.

[0012] In a preferred embodiment of the present invention, the water-soluble polymer accounts for 3-25 weight percent of the total solid content of the main agent.

[0013] In a preferred embodiment of the present invention, the water-soluble polymer accounts for 5-25 weight percent of the total solid content of the main agent.

[0014] In a preferred embodiment of the present invention, the water-soluble polymer accounts for 10-25 weight percent of the total solid content of the main agent.

[0015] In a preferred embodiment of the present invention, the hydrolysis mol % of the water-soluble polymer in the main agent is between 70-99.8%.

[0016] In a preferred embodiment of the present invention, the hydrolysis molar percentage of the water-soluble polymer in the main agent is between 80-99.8%.

[0017] In a preferred embodiment of the present invention, the hydrolysis molar percentage of the water-soluble polymer in the main agent is between 85-99.5%.

[0018] In a preferred embodiment of the present invention, the synthetic rubber latex accounts for 3-55 weight percent of the total solid content of the main agent.

[0019] In a preferred embodiment of the present invention, the synthetic rubber latex accounts for 3-40 weight percent of the total solid content of the main agent.

[0020] In a preferred embodiment of the present invention, the synthetic rubber latex accounts for 3-30 weight percent of the total solid content of the main agent.

[0021] In a preferred embodiment of the present invention, the natural latex accounts for 5-85 weight percent of the total solid content of the main agent.

[0022] In a preferred embodiment of the present invention, the natural latex accounts for 5-75 weight percent of the total solid content of the main agent.

[0023] In a preferred embodiment of the present invention, natural latex accounts for 10-60 weight percent of the total solid content of the main agent.

[0024] In a preferred embodiment of the present invention, the natural latex is obtained from plants, and the natural latex also includes epoxidized natural latex or deproteinized natural latex.

[0025] In a preferred embodiment of the present invention, the isocyanate comprises one or more isocyanates, and the isocyanate is a compound containing an isocyanate functional group or a polymer thereof.

[0026] In a preferred embodiment of the present invention, the quaternary ammonium salt polymer comprises one or more quaternary ammonium salt polymers, and the quaternary ammonium salt polymer is polyaminoamide-epichlorohydrin (PAE) resin.

[0027] In a preferred embodiment of the present invention, it further includes an inorganic or organic filler, characterized in that the inorganic filler is selected from at least one or a combination of calcium carbonate, magnesium carbonate, talc, barium sulfate, kaolin, titanium dioxide, silicon oxide, aluminum oxide and glass fiber; and the organic filler is selected from at least one or a combination of starch, lignin, tannin, cellulose, sugar and wood powder.

[0028] In a preferred embodiment of the present invention, the additives include defoaming agent, thickener, thixotropic agent, antioxidant, dispersant, flame retardant and the like. DETAILED DESCRIPTION

[0029] In one embodiment, the present invention provides a water-based adhesive that can be applied to wood or bamboo. The water-based adhesive includes a main agent and a curing agent. It is characterized in that the main agent is composed of a water-soluble polymer, a synthetic rubber latex and a natural latex. The curing agent can be selected from an isocyanate or a quaternary ammonium salt polymer. The weight ratio of the main agent to the curing agent is between 200:1 and 1:1. The water-soluble polymer is polyvinyl alcohol, which accounts for 2-30 weight percent of the total solid amount of the main agent. The synthetic rubber latex is selected from the group consisting of styrene-butadiene rubber latex and styrene-butadiene rubber latex containing carboxylic acid functional groups, and the synthetic rubber latex accounts for 2-60 weight percent of the total solid amount of the main agent. Natural latex accounts for 5-90 weight percent of the total solid amount of the main agent. In one embodiment, the weight ratio of the main agent to the curing agent can be between 100:1 and 10:3.

[0030] The bio-based natural latex used in the present invention is natural latex taken from plants. The chemical structure of natural latex is mainly composed of a high molecular polymer composed of isoprene, and it is dispersed in water in the form of latex. The natural latex used in the present invention can be used directly without being modified by artificial chemical methods. Natural latex has good hydrophobicity. In use, after removing water, a high molecular rubber film with excellent water resistance will be formed. When used in adhesives, the water resistance of the bonded objects can be greatly improved. The disadvantage of natural latex is poor stability. In one embodiment, ammonia water, potassium hydroxide or a chelating agent can be added as a stabilizer. In one embodiment, 0.1-1wt% of ammonia water can be added to the natural latex aqueous solution as a stabilizer and an antibacterial agent.

[0031] In the main agent of the present invention, if the proportion of natural latex is too low, the significance of adding biomass materials to improve environmental sustainability will be lost. On the contrary, if too much is added, the natural latex will easily form a skin due to slight evaporation of water, making it difficult to apply and use. In one embodiment, natural latex accounts for 5-85 weight percent of the total solids of the main agent. In one embodiment, natural latex accounts for 5-75 weight percent of the total solids of the main agent. In one embodiment, natural latex accounts for 10-60 weight percent of the total solids of the main agent.

[0032] In one embodiment, the natural latex of the present invention includes epoxidized natural latex or deproteinized natural latex. Epoxidized natural latex is formed by chemical reaction of double bonds on the molecular chain into epoxy functional groups, which can improve reactivity, increase cross-linking strength, and improve temperature resistance, water resistance and mechanical strength. Deproteinized natural latex is the removal of protein components in latex, which can reduce the probability of mold and corruption.

[0033] The water-soluble polymer in the main agent of the present invention is polyvinyl alcohol. Adding a water-soluble polymer can enhance the reaction with the curing agent and improve adhesion and water resistance. In one embodiment, the hydrolysis mol% of the water-soluble polymer is between 80-99.8%. In one embodiment, the hydrolysis mol% of the water-soluble polymer is between 85-99.5%. In the present invention, the hydrolysis ratio is too low, the reactivity decreases, and the adhesion strength also decreases. In one embodiment, the water-soluble polymer accounts for 3-25 weight percent of the total solids of the main agent. In one embodiment, the water-soluble polymer accounts for 5-25 weight percent of the total solids of the main agent. In one embodiment, the water-soluble polymer accounts for 10-25 weight percent of the total solids of the main agent.

[0034] The synthetic rubber latex in the main agent of the present invention can also promote the reaction with the curing agent, and improve the adhesion and water resistance. In one embodiment, the synthetic rubber latex of the present invention accounts for 3-55 weight percent of the total solids of the main agent. In one embodiment, the synthetic rubber latex accounts for 3-40 weight percent of the total solids of the main agent. In one embodiment, the synthetic rubber latex accounts for 3-30 weight percent of the total solids of the main agent.

[0035] The curing agent of the present invention mainly provides a cross-linking bridging reaction with the main agent. In one embodiment, the isocyanate includes one or more isocyanates, and the isocyanate is a compound containing an isocyanate functional group (isocyanate) or a polymer thereof. In one embodiment, the isocyanate can be methylene diphenyl diisocyanate (diphenylmethanediisocyanate, MDI), including its three isomers: 2,2'-MDI, 2,4'-MDI and 4,4'-MDI, and further including its oligomers (crude MDI or polymeric MDI). In one embodiment, the isocyanate can also be tolylene-2,4-and tolylene-2,6-diisocyanate (TDI) and its isomers. In one embodiment, the isocyanate can also be dicyclohexylmethane diisocyanate (4,4'-diisocyanato-dicyclohexylmethane, H12MDI) and its isomers. In one embodiment, the isocyanate may also be hexamethylene diisocyanate (HDI) and its isomers. In one embodiment, the isocyanate may also be isophorone diisocyanate (IPDI). In one embodiment, the isocyanate may also be 3,3'-dimethylbiphenyl-4,4'-diisocyanate o-Tolidine diisocyanate (TODI).

[0036] The curing agent of the present invention may also be a quaternary ammonium salt polymer, which may include one or more quaternary ammonium salt polymers. In one embodiment, the quaternary ammonium salt polymer may be a quaternary ammonium salt polymer (polyaminoamide epichlorohydrin, PAE) formed by the reaction of polyamide (polyamidoamine) and epichlorohydrin (epichlorohydrin). This polymer has a structure as represented by chemical formula 1, characterized in that n is an integer. In a preferred embodiment of the present invention, the quaternary ammonium salt polymer contains one or more quaternary ammonium salt polymers, and the quaternary ammonium salt polymer is a polyamide polyamine-epichlorohydrin resin (polyaminoamide-epichlorohydrin, PAE). Its chemical formula is shown in formula (1):

[0037]

[0038] In one embodiment, it further includes an inorganic or organic filler, wherein the inorganic filler includes calcium carbonate, magnesium carbonate, talc, barium sulfate, kaolin, titanium dioxide, silicon oxide, aluminum oxide or glass fiber; and the organic filler includes starch, lignin, tannin, cellulose, sugar or wood powder.

[0039] In one embodiment, in order to better meet the process requirements, the main agent of the present invention can be added with auxiliary agents including defoamers, thickeners, thixotropic agents, antioxidants, dispersants, flame retardants, etc. Or in order to meet different additional characteristics, such as increasing the solid content of the adhesive, increasing opacity, reducing costs, etc., the main agent of the present invention can be added with inorganic or organic fillers. It is characterized in that the inorganic filler includes calcium carbonate, magnesium carbonate, talc, barium sulfate, kaolin, titanium dioxide, silicon oxide, aluminum oxide or glass fiber. And the organic filler includes starch, lignin, tannin, cellulose, sugar or wood powder.

[0040] Hereinafter, the present invention will be described by way of Examples and Comparative Examples.

[0041] Example 1

[0042] Take 10 grams of polyvinyl alcohol (PVA) aqueous solution (BP-05, 30wt%, Changchun artificial resin), add 20 grams of styrene-butadiene rubber (SBR) resin (LBT04, Shenfeng special materials), mix well, add 50 grams of natural latex (60wt%, made in Thailand), stir well to complete the main agent of water-based adhesive. Use diphenylmethanediisocyanate (MDI) as the curing agent of water-based adhesive. Take 10 grams of MDI and add it to 80 grams of the main agent, stir well and it can be used. Bond the wood board according to the method listed in SS-EN 205 (Adhesives-Wood adhesives for non-structural applications-Determination of tensile shear strength of lap joints), and make mechanical tensile test pieces according to its regulations. After the tensile test pieces were completed, mechanical tensile tests were performed according to the C4 standard of SS-EN 12765 (Classification of thermosetting wood adhesives for nonstructural applications). The test results are listed in Table 1.

[0043] Example 2

[0044] Take 10 grams of polyvinyl alcohol (PVA) aqueous solution (BP-05, 30wt%, Changchun Man-Made Resin), add 20 grams of styrene-butadiene rubber (SBR) resin (LBT04, Shenfeng Special Materials), mix well, add 50 grams of natural latex (60wt%, made in Thailand), stir well to complete the main agent of the water-based adhesive. Use quaternary ammonium salt polymer (PAE, Changchun Man-Made Resin) as the curing agent of the water-based adhesive, take 10 grams of PAE and add it to 80 grams of the main agent, stir well and it can be used. According to the method listed in SS-EN 205 (Adhesives-Wood adhesives for non-structural applications-Determination of oftensile shear strength of lap joints), the wood board is bonded, and the mechanical tensile test piece is made according to its regulations. After the tensile test piece is completed, the mechanical tensile side test is carried out according to the C4 standard of SS-EN 12765 (Classification of thermosetting woodadhesives for nonstructural applications). The test results are listed in Table 1.

[0045] Example 3

[0046] Take 50 grams of polyvinyl alcohol (PVA) aqueous solution (BP-05, 30wt%, Changchun artificial resin), add 20 grams of styrene-butadiene rubber (SBR) resin (LBT04, Shenfeng special materials), mix well, add 10 grams of natural latex (60wt%, made in Thailand) and 20 grams of calcium carbonate, stir well to complete the main agent of the water-based adhesive. Use diphenylmethane diisocyanate (MDI) as the curing agent of the water-based adhesive, take 10 grams of MDI and add it to 100 grams of the second component, stir well and it can be used. Bond the wood board according to the method listed in SS-EN 205 (Adhesives-Wood adhesives for non-structural applications-Determination of tensile shear strength of lapjoints), and make mechanical tensile test pieces according to its regulations. After the tensile test pieces were completed, mechanical tensile tests were performed according to the C4 standard of SS-EN12765 (Classification of thermosetting wood adhesives for nonstructural applications). The test results are listed in Table 1.

[0047] Example 4

[0048] Take 20 grams of polyvinyl alcohol (PVA) aqueous solution (BP-05 main agent 30wt% main agent Changchun artificial resin), add 50 grams of styrene butadiene rubber (SBR) resin (LBT04 main agent Shenfeng special material), mix well, add 10 grams of natural latex (60wt% main agent made in Thailand) and 20 grams of calcium carbonate, stir well to complete the main agent of water-based adhesive. Use diphenylmethane diisocyanate (MDI main agent) as the curing agent of water-based adhesive, take 10 grams of MDI and add it to 100 grams of the main agent, stir well and it can be used. Bond the wood board according to the method listed in SS-EN 205 (Adhesives-Woodadhesives for non-structural applications-Determination of tensile shearstrength of lap joints), and make mechanical tensile test pieces according to its regulations. After the tensile test pieces were completed, mechanical tensile tests were performed according to the C4 standard of SS-EN 12765 (Classification of thermosetting wood adhesives for nonstructural applications). The test results are listed in Table 1.

[0049] Comparative Example 1

[0050] Take 40g of styrene-butadiene rubber (SBR) resin (LBT04 main agent Shenfeng Special Materials), add 40g of natural latex (60wt% main agent made in Thailand) and 20g of calcium carbonate, mix and stir evenly to complete the main agent of the water-based adhesive. Use diphenylmethane diisocyanate (MDI main agent) as the curing agent of the water-based adhesive. Take 10g of MDI and add it to 100g of the main agent. Stir evenly before use. Bond the wood board according to the method listed in SS-EN 205 (Adhesives-Woodadhesives for non-structural applications-Determination of tensile shearstrength of lap joints), and make a mechanical tensile test piece according to its regulations. After the tensile test piece is completed, the mechanical tensile side test is carried out according to the C4 standard of SS-EN 12765 (Classification of thermosetting wood adhesives fornonstructural applications). The test results are listed in Table 1.

[0051] Comparative Example 2

[0052] Take 40g of polyvinyl alcohol (PVA) aqueous solution (BP-05 main agent 30wt% main agent Changchun artificial resin), add 40g of natural latex (60wt% main agent made in Thailand) and 20g of calcium carbonate, mix and stir evenly to complete the main agent of the water-based adhesive. Use diphenylmethane diisocyanate (MDI) as the curing agent of the water-based adhesive, take 10g of MDI and add it to 100g of the main agent, stir evenly and it can be used. According to the method listed in SS-EN 205 (Adhesives-Wood adhesives for non-structural applications-Determination of tensile shear strength of lap joints), the wood boards are bonded and mechanical tensile test pieces are made according to its regulations. After the tensile test pieces are completed, the mechanical tensile side test is carried out according to the C4 standard of SS-EN 12765 (Classification of thermosetting wood adhesives for nonstructural applications). The test results are listed in Table 1.

[0053] The adhesives prepared in the above-mentioned Examples 1-4 and Comparative Examples 1-2, as well as the composition and bonding strength test results are listed in Table 1.

[0054] Table 1

[0055]

[0056]

[0057] Please refer to Example 1 and Example 2. The wood board bonded with the water-based adhesive made with the formula of Example 1 can pass the most stringent C4 standard. Example 2 uses PAE as a curing agent. The strength of the wood board bonded with the water-based adhesive made with the formula of Example 2 is slightly lower than that of Example 1 using MDI as a curing agent, but it can still pass the C4 standard.

[0058] Please refer to Example 3. The amount of polyvinyl alcohol added in the formula of Example 3 is increased. In addition, calcium carbonate is added to increase the overall solid content of the water-based adhesive. In this way, the bonding strength of the wood board bonded with the water-based adhesive made using the formula of Example 3 is still not affected and can also pass the C4 standard.

[0059] Please refer to Example 4. The formula of Example 4 increases the proportion of styrene-butadiene rubber. In addition, calcium carbonate is added to increase the overall solid content of the water-based adhesive. In this way, the bonding strength of the wood board bonded with the water-based adhesive made using the formula of Example 4 is still not affected and can also pass the C4 standard.

[0060] Please refer to Comparative Example 1. Comparative Example 1 is a water-based adhesive made without adding polyvinyl alcohol. The bonding strength of the wood boards bonded using the water-based adhesive made with the formula of Comparative Example 1 is significantly reduced in a wet state and cannot pass the C4 standard.

[0061] Please refer to Comparative Example 2. Comparative Example 2 is a water-based adhesive made without adding styrene-butadiene rubber. The bonding strength of the wood boards bonded using the water-based adhesive made with the formula of Comparative Example 2 is significantly reduced in a wet state and cannot pass the C4 standard.

[0062] In summary, the water-based adhesive of the present invention does not use formaldehyde and introduces natural renewable raw materials, effectively reducing the dependence on petrochemical products. The biomass material used in the present invention is natural latex, which is mixed with rubber latex and environmentally friendly non-toxic water-soluble polymers, and then mixed with a suitable curing agent. The water-based adhesive of the present invention can provide wood and bamboo with good water resistance, bonding strength and mechanical strength.

[0063] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A water-based adhesive for wood or bamboo, comprising a main agent composed of a water-soluble polymer, synthetic rubber latex and natural latex and a curing agent selected from isocyanate or quaternary ammonium salt polymer, characterized in that The weight ratio of the main agent to the curing agent is between 200:1 and 1:1; the water-soluble polymer is polyvinyl alcohol, which accounts for 2-30 weight percent of the total solid content of the main agent; the synthetic rubber latex is selected from the group consisting of styrene-butadiene rubber latex and styrene-butadiene rubber latex containing carboxylic acid functional groups, and the synthetic rubber latex accounts for 2-60 weight percent of the total solid content of the main agent; and the natural latex accounts for 5-90 weight percent of the total solid content of the main agent.

2. The water-based adhesive according to claim 1, characterized in that The weight ratio of the main agent to the curing agent is between 100:1 and 10:

3.

3. The water-based adhesive according to claim 1, characterized in that The water-soluble polymer accounts for 3-25 weight percent of the total solid content of the main agent.

4. The water-based adhesive according to claim 1, characterized in that The hydrolysis molar percentage of the water-soluble polymer in the main agent is between 70-99.8%.

5. The water-based adhesive according to claim 1, characterized in that The synthetic rubber latex accounts for 3-55 weight percent of the total solid content of the main agent.

6. The water-based adhesive according to claim 1, characterized in that The natural latex accounts for 5-85 weight percent of the total solid content of the main agent.

7. The water-based adhesive according to claim 1, characterized in that The natural latex accounts for 5-75 weight percent of the total solid content of the main agent.

8. The water-based adhesive according to claim 1, characterized in that The natural latex is selected from at least one of epoxidized natural latex and deproteinized natural latex or a combination thereof.

9. The water-based adhesive according to claim 1, characterized in that The isocyanate comprises one or more isocyanates, and the isocyanate is a compound containing an isocyanate functional group or a polymer thereof.

10. The water-based adhesive according to claim 1, characterized in that The quaternary ammonium salt polymer contains one or more quaternary ammonium salt polymers, and the quaternary ammonium salt polymer is a polyamide polyamine-epichlorohydrin resin.